Method for depolymerizing polymers to reusable starting material
By using catalysts and alkali cocatalysts in the depolymerization process of terephthalate polymers, the conversion rate and catalyst recovery rate are improved, the problems of low conversion rate and recovery efficiency in the existing technology are solved, and the requirements for high-purity raw materials are met. needs.
Patent Information
- Application Number
- CN202380017606.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-17
- Filing Date
- 2023-01-12
- Publication Date
- 2024-10-15
AI Technical Summary
When the existing technology depolymerizes terephthalate polymers into reusable raw materials, the conversion rate and catalyst recovery efficiency are low, and it is difficult to meet the high purity requirements of food and medical applications.
A catalyst is used to degrade the polymer into oligomers and monomers, and a base is added as a cocatalyst in the reaction step to improve the conversion rate and the separation and recovery efficiency of the catalyst. Specific methods include using an appropriate solvent such as ethylene glycol in the reactor, selecting an appropriate catalyst such as nanoparticles, separating the catalyst by magnetism or other methods, and conducting the reaction at appropriate temperature and pressure.
It improves the polymer conversion rate and catalyst recovery rate, ensures the production of high-purity raw materials, is suitable for strict applications such as food and medical, and reduces the formation of pollutants and the residual metal ions.
Smart Images

Figure CN118786171A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for depolymerizing a polymer into reusable raw materials, such as, for example, terephthalate monomers and oligomers, using a catalyst. The present invention further relates to recovering the catalyst from the reaction mixture. The present invention also relates to using a base as a co-catalyst in a depolymerization reaction using a catalyst. Background Art
[0002] Depolymerization of polymers into reusable raw materials is currently an area of great concern to the industry. One of the examples of a group of polymers of interest for recycling is terephthalate polymers, which are a group of polyesters containing terephthalate in the main chain. The most common example of terephthalate polymers is polyethylene terephthalate, also known as PET. Alternative examples include polybutylene terephthalate, polytrimethylene terephthalate, polyethylene isophthalate, polypentaerythritol terephthalate and copolymers thereof, such as copolymers of ethylene terephthalate and polyglycols, for example polyoxyethylene glycol (polyoxyethylene glycol) and poly (butylene glycol) copolymers. PET is one of the most common polymers, and it is very desirable to recycle PET by depolymerizing it into reusable raw materials.
[0003] A preferred depolymerization mode is glycolysis, which is preferably catalyzed. Typically, due to the use of an alcohol (such as ethylene glycol), a reaction mixture comprising at least one monomer can be formed, the at least one monomer comprising bis(2-hydroxyethyl) terephthalate (BHET). An example of a suitable depolymerization by glycolysis is known from WO2016 / 105200 under the name of the applicant. According to the method, terephthalate polymers are depolymerized by glycolysis in the presence of a catalyst. At the end of the depolymerization process, water is added and phase separation occurs. This enables the first phase comprising the BHET monomer to be separated from the second phase comprising a catalyst, oligomers and additives. The first phase may contain impurities in dissolved form and as dispersed particles. The BHET monomer can be obtained in pure form by means of crystallization.
[0004] Reuse of the depolymerized raw material requires high purity. It is well known that any contaminants may have an impact on the subsequent polymerization reaction from the raw material. In addition, since terephthalate polymers are used in food and medical applications, strict regulations apply to prevent health problems.
[0005] Although the applicant's method according to WO2016 / 105200 leads to a very high conversion of terephthalate polymers and also facilitates the separation of various additives from the BHET monomer, the depolymerization reaction can be further optimized. In addition, the recovery of the catalyst from the reaction mixture can be further improved. Summary of the invention
[0006] Therefore, it is desirable to provide a method for depolymerizing polymers into reusable raw materials with high purity, so that the method is suitable for preparing fresh polymers. One example is terephthalate polymers. Although such methods may not always produce very high polymer conversions, acceptable conversions (rates) can be achieved. In order to increase the conversion, catalysts are used. These catalysts are separated from the monomers and reused after separation. The object of the present invention is to further improve the catalytic depolymerization process and to further improve the separation and recovery of the catalyst.
[0007] According to a first aspect of the present invention, there is provided a method for obtaining a monomer by degrading a polymer, the polymer being a homopolymer or a copolymer of the monomer, the method comprising the following steps:
[0008] a. providing a polymer and a solvent as a reaction mixture in a reactor, wherein the solvent is a reactant capable of reacting with the polymer to degrade the polymer into oligomers and at least one monomer;
[0009] b. providing a reusable catalyst capable of degrading a polymer into oligomers and at least one monomer; and
[0010] c. using a catalyst to degrade the polymer in the reaction mixture under reaction conditions to form at least one monomer; and
[0011] d. recovering the catalyst from the reaction mixture;
[0012] Wherein the process further comprises adding at least one base to the reaction mixture in at least one reaction step of reaction steps a to d.
[0013] According to a second aspect of the invention, the invention relates to the use of a base as a cocatalyst for a catalyst for degrading a polymer in a reaction mixture under reaction conditions.
[0014] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. The terms used in the description of the present invention are for the purpose of describing particular embodiments only and are not intended to limit the present invention.
[0015] The present invention is a method for obtaining a monomer by degrading a polymer, which is a homopolymer or copolymer of a monomer. A reusable catalyst capable of degrading the polymer into an oligomer and at least one monomer is used. In order to recover the catalyst more easily and to a higher degree, at least one base is added to the reaction mixture in at least one reaction step in reaction steps a to d. It has been further confirmed that when a base is added to the reaction mixture in or before step c, the base improves the catalytic degradation of the polymer into smaller molecules. Reaction time and selectivity are improved.
[0016] Polymer and solvent are provided as reaction mixture in the reactor, wherein the solvent is a reactant capable of reacting with the polymer to degrade the polymer into oligomers and at least one monomer. The depolymerization of polyester preferably occurs by means of solvent decomposition, wherein the solvent serves as a reactant. Typical solvents are alkanols and alkanediols, such as ethylene glycol, methanol, diethylene glycol, propylene glycol, dipropylene glycol. Considering the physical properties of ethylene glycol (such as boiling point at about 200° C.), it has been found that ethylene glycol is suitable. For the depolymerization of PET, the use of ethylene glycol will result in bis(2-hydroxyethyl) terephthalate (BHET) as the main depolymerization product. Dimers, trimers and other oligomers can also be obtained. BHET and its dimer can be purified and obtained with sufficient purity by crystallization. One method is to process the aqueous phase obtained after adding water and / or aqueous solution in a downstream container, and separate it from the second phase in a centrifuge, as mentioned above. Examples are specified in WO2017 / 111602 mentioned above, which is included by reference.
[0017] Advantageously, the weight ratio of solvent (preferably ethylene glycol) to polymer is in the range of 10:10 to 100:10, more preferably in the range of 20:10 to 90:10, and most preferably in the range of 40:10 to 60:10.
[0018] In a preferred embodiment of the present invention, the polymer concentration in the dispersion is from 1 to 30% by weight, based on the total weight of the reaction mixture.
[0019] A reusable catalyst capable of degrading the polymer into oligomers and at least one monomer is provided to the reaction mixture.The present invention may be carried out using any catalyst suitable for the purpose.
[0020] In the depolymerization process according to an embodiment, the catalyst forms a dispersion in the reaction mixture during step c.
[0021] Recently, nanoparticles have received considerable attention as depolymerization catalysts. Reactions in the liquid phase require small particles because the diffusion rate in liquids is several orders of magnitude smaller than that in gases. Such nanoparticles have small diameters and are between 0.5 and 200 μm in diameter. 2 / g of surface area. Nanoparticles are highly active, which is believed to lead to faster depolymerization, and is therefore an economically viable method. In order to separate such nanoparticles, a variety of options are available. Several possible depolymerization catalysts are based on ferromagnetic materials and / or ferrimagnetic materials. Antiferromagnetic materials, synthetic magnetic materials, paramagnetic materials, superparamagnetic materials, such as materials containing at least one of Fe, Co, Ni, Gd, Dy, Mn, Nd, Sm, and preferably at least one of O, B, C, N, such as iron oxides, such as ferrites, such as magnetite, hematite and maghemite, can also be used. Although the use of magnetic materials mainly allows separation by means of magnetic attraction, many nanoparticles are too small to be fully attracted by themselves. However, by applying a magnetic field, nanoparticles may form magnetic clusters, which are more easily separated by magnetic force. For magnetic nanoparticle catalysts and non-magnetic nanoparticle catalysts, larger-sized nanoparticle clusters can also be produced by adding other compounds. The present invention provides an improved solution.
[0022] A class of suitable catalysts includes transition metals in metallic or ionic form. Ionic forms include free ions in solution and ionic bonds or covalent bonds. Ionic bonds are formed when one atom donates one or more electrons to another atom. Covalent bonds are formed using interatomic bonds generated by sharing electron pairs between two atoms. The transition metal can be selected from the first series of transition metals, also known as 3d orbital transition metals. More particularly, the transition metal is selected from iron, nickel and cobalt. However, since cobalt is unhealthy and iron and nickel particles can be formed in pure form, iron and nickel particles are most preferred. In addition, alloys of various transition metals can be used.
[0023] The nanoparticles of the present invention are preferably magnetic, either comprising a magnetic material, or having the ability to be fully magnetized under a relatively moderate magnetic field, such as that used in the method of the present invention. Suitably, the magnetic nanoparticles comprise iron, nickel and / or cobalt in oxide or metal form, or a combination thereof. Preferred iron oxides are in the form of, for example, but not limited to, Fe3O4. Another suitable example is Fe2O3. A suitable example from an alloy is CoFe2O4. Other preferred examples are NiFe2O4, Ni2Fe2O5 or NiO.
[0024] If the nanoparticle is made of a metal, it may be provided with an oxide surface, which may further enhance the catalytic effect. The oxide surface may be formed by itself, in contact with air, in contact with water, or may be applied intentionally.
[0025] It has been found that for the catalyst complex, the nanoparticles should be small enough to act as a catalyst, thereby degrading the polymer into smaller units, wherein the yield of these smaller units, in particular its monomers, is high enough for commercial reasons. It has further been found that the nanoparticles should be large enough to be able to be reused by recovering the catalyst of the present invention. It is economically disadvantageous to remove the catalyst together with the waste or degradation products obtained. Suitable nanoparticles have an average diameter in the range of 2 to 500nm, more preferably in the range of 3 to 200nm, and even more preferably in the range of 4 to 100nm. It has been found that, for example, a relatively small particle size of 5 to 10nm is optimal in terms of the yield and recovery of the catalyst complex. It should be noted that the term "size" refers to the average diameter of the particles, wherein the actual diameter of the particles may vary slightly due to their characteristics. In addition, aggregates may be formed, for example in solution. These aggregates generally have a size in the range of 50 to 200nm, such as in the range of 80 to 150nm, for example about 100nm. Preferably, nanoparticles containing iron oxides are used.
[0026] The particle size and its distribution can be measured by light scattering, for example using a Malvern dynamic light scattering device, such as the NS500 series. In a more laborious manner, usually applied to smaller particle sizes, and equally well applicable to large sizes, a representative electron microscope photograph is taken and the size of each particle is measured on the photograph. For the average particle size, a number weight average can be taken. In approximate cases, the average can be taken as the size with the highest number of particles or the median size.
[0027] Most preferably, iron or iron-containing particles are used. In addition to being magnetic, iron or iron-containing particles have been found to catalyze the depolymerization of PET, e.g., with conversions to monomers of 70 to 90% in acceptable reaction times of up to 6 hours, depending on catalyst loading and other processing factors, such as the PET / solvent ratio. The desired catalyst concentration is 1 wt% or less relative to the amount of PET. Good results have also been obtained using catalyst loadings of less than 0.2 wt%, even less than 0.1 wt%, relative to the amount of PET. Such low loadings of catalyst are very beneficial, and the process of the invention allows for the recovery of increased amounts of nanoparticle catalyst.
[0028] Non-porous metal particles, particularly transition metal particles, can be suitably prepared by thermal decomposition of carbonyl complexes such as iron pentacarbonyl and nickel tetracarbonyl. Alternatively, iron oxides and nickel oxides can be prepared by exposing the metal to oxygen at higher temperatures such as 400°C and above. Non-porous particles may be more suitable than porous particles because exposure to alcohols may be less, and therefore corrosion of the particles may also be less, and the particles may be reused for catalysis more often. In addition, due to the limited surface area, any oxidation at the surface may result in lower amounts of metal ions, thereby resulting in lower levels of ions present in the product stream as contaminants to be removed therefrom.
[0029] The non-porous particles according to the invention are suitably of a surface area less than 10 m 2 / g, more preferably at most 5m 2 / g, even more preferably at most 1m 2 / g of particles. The porosity is appropriately less than 10 -2 cm 3 / g or even smaller, for example up to 10 -3 cm 3 / g.
[0030] Another class of suitable catalysts includes nanoparticles based on alkaline earth elements selected from beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr) and barium (Ba) and their oxides. The preferred alkaline earth metal oxide is magnesium oxide (MgO). Other suitable metals include, but are not limited to, titanium (Ti), zirconium (Zr), manganese (Mn), zinc (Zn), aluminum (Al), germanium (Ge) and antimony (Sb), and their oxides and other alloys thereof. Noble metals are also suitable, such as palladium (Pd) and platinum (Pt). MgO and ZnO have been found to catalyze the depolymerization of PET, for example, with a conversion rate to monomers of 70 to 90% within an acceptable reaction time, depending on the catalyst loading and other processing factors, such as the PET / solvent ratio. Suitable catalysts based on hydrotalcite are also contemplated.
[0031] Preferably, the nanoparticles are selected such that they are substantially insoluble in the (alcohol) reactive solvent also at higher temperatures above 100° C. Oxides such as, for example, amorphous SiO 2 , which tend to dissolve readily in alcohols such as ethylene glycol at higher temperatures, are less suitable.
[0032] Suitable catalysts according to the present invention may be coated. For example, Fe3O4 particles may be coated with a material to prevent the particles from oxidizing to Fe2O3, which includes different magnetic properties. Thus, the surface of the catalyst particles may be coated with materials such as polyethyleneimine (PEI), polyethylene glycol (PEG), silicone oil, fatty acids (such as oleic acid or stearic acid), silane, mineral oil, amino acids or polyacrylic acid or polyvinyl pyrrolidone (PVP). Carbon may also be used as a coating material.
[0033] The coating can be removed before or during the catalytic reaction. The coating can be removed, for example, by a separate solvent washing step before using the coating in the reactor, or by burning the coating in air.
[0034] Particularly preferred catalysts relate to catalyst complexes (ABC) comprising three distinguishable elements: (nano) particles (A), bridging moieties / linking groups (B) chemically (such as by covalent bonds) or physically (such as by adsorption) attached to the particles, and catalyst entities (C) associated with the particles (A), such as by chemically (e.g. covalently) bonding to the linking groups. The linking groups preferably do not completely cover the nanoparticle surface, such as in core-shell particles. The nanoparticles of the catalyst complex are preferably based on ferromagnetic and / or ferrimagnetic materials. Antiferromagnetic materials, synthetic magnetic materials, paramagnetic materials, superparamagnetic materials, such as materials comprising at least one of Fe, Co, Ni, Gd, Dy, Mn, Nd, Sm, and preferably at least one of O, B, C, N, such as oxides of iron, such as ferrites, such as magnetite, hematite and maghemite, can also be used. Considering the cost, relatively cheap particles are preferred, such as particles comprising Fe, even when the catalyst complex of the present invention is fully or largely recovered. Another advantage of particles of iron or iron oxide is that they have the highest saturation magnetization, making it easier to separate particles by magnetic separators. Even more importantly, iron oxide nanoparticles have a positive effect on the degradation reaction. The iron oxide may further contain additional elements, such as cobalt and / or manganese, for example CoFe2O4.
[0035] Preferably, the nanoparticles are selected such that they are substantially insoluble in the (alcohol) reactive solvent also at higher temperatures above 100° C. Oxides such as, for example, amorphous SiO 2 , which tend to dissolve readily in alcohols such as ethylene glycol at higher temperatures, are less suitable.
[0036] The functional group of the bridging part is, for example, a weak organic acid, such as a carboxylic acid or a dicarboxylic acid, but preferably a silanol, including silanediol and silanetriol. The bridging part can be introduced as a reactant in the form of a silyl-containing group, such as a silyl ether, such as triethoxysilylpropyl halide. The linking group is, for example, an alkylene chain, wherein the alkylene group is usually between C2 and C 10 The bridging moiety is suitably provided as a reactant, wherein the linking group is functionalized to react chemically with the catalyst entity, and the functional group can be protected. For example, the appropriate functionalization of the linking group is provided as a substituted alkyl halide. The appropriate protection of the functional group can be in the form of an ester or an alkoxysilane. Although methoxy or propoxy are not excluded, the alkoxy is preferably an ethoxy.
[0037] In another embodiment, the alkoxysilane is provided as a trialkoxysilane with an alkylene group constituting a linking group. In an alternative embodiment, a dialkyl-dialkoxysilane is used, in which one of the alkyl groups is a linking group. In a further embodiment, a monoalkoxy-trialkylsilane is used, in which one of the alkyl groups is a linking group. In the latter case, the alkyl group is preferably a lower alkyl group, such as a C1-C4 alkyl group, thus a methyl, ethyl, propyl, n-butyl, isobutyl group. Then, at least one alkyl group is functionalized, for example with a halide, as defined above. Linear alkyl groups appear to more preferably limit steric hindrance.
[0038] In embodiments, the use of dialkyl-dialkoxysilane and / or monoalkoxy-trialkylsilane is understood to be conducive to producing better separation between the hydrophilic solution and the second phase, and in embodiments using phase separation, it is ensured that the complex enters the second phase rather than the hydrophilic solution, where the complex will be lost. It is believed that not all alkoxy groups of trialkoxysilane are bonded to the surface of the nanoparticle aggregates. Some alkoxy groups can even remain protected. However, when water is added to the complex, the protecting group may be removed. As a result, the hydrophilicity of the complex may increase. By using silanes with fewer alkoxy groups, the remaining groups are essentially non-polar and cannot become unprotected. Therefore, the entire complex becomes more hydrophobic. Instead of using only one type of bridging part (also referred to as a silane coupling agent), a mixture of those bridging parts can be used, such as a mixture of alkyltrialkoxysilane and dialkyl-dialkoxysilane, wherein one of the alkyl groups is functionalized as a halide to react with the catalyst entity, and then-after the reaction of the two-carrying the catalyst entity. The addition of dialkyldialkoxysilanes can very well reduce the size of the layer of groups bonded to the surface. This is not considered a disadvantage.
[0039] This part can be aromatic or aliphatic, and heterocyclic. The aromatic heterocyclic part suitably comprises a heterocycle having at least one, preferably at least two nitrogen atoms. The heterocycle can have 5 or 6 atoms, preferably 5 atoms. Suitable aromatic heterocycles are pyrimidines, imidazoles, piperidines, pyrrolidines, pyridines, pyrazoles, oxazoles, triazoles, thiazoles, methimazoles (methimazol), benzotriazoles, isoquinolines and viologen compounds (e.g., having two coupled pyridine ring structures). Particularly preferred is the imidazole structure, which produces imidazolium ions. The negatively charged part can be related to anionic complexes, but is instead a simple ion, such as a halide. Preferably, the alkyl halide of the bridging part and the reaction of the uncharged aromatic heterocyclic part including at least one nitrogen atom produce positive charges on the aromatic part, particularly on the nitrogen atom therein, and produce negatively charged halides. Negatively charged halides can be enhanced by adding Lewis acids thereafter to form metal salt complexes. An example is the conversion of chloride to FeCl4 - In one example, the aromatic moiety has at least one tail. The at least one tail preferably has a C1-C 10 The length of the at least one tail is suitably attached to a nitrogen atom, such as C2-C4. More particularly, the tail is the tail that extends into the carrier liquid and away from the bridging portion. Longer tails are believed to be beneficial for increasing the hydrophobicity of the complex. This can counteract the tendency of the complex to enter the hydrophilic phase.
[0040] According to the present invention, the bridging moieties and the catalyst entities bonded thereto are present in an amount of (mol bridging moieties / g magnetic particles) 5×10 -6 to 0.1, preferably 1×10 -5 to 0.01, more preferably 2×10 -5 Up to 10 -3 , such as 4×10 -5 Up to 10 -4 In terms of efficient optional recovery of the catalyst complex, it is preferred to have a relatively large available amount, while in terms of the amount of catalyst and its cost, a slightly smaller amount may be more preferred.
[0041] It has been found that limited coverage of the surface of a nanoparticle or an aggregate of such particles by catalyst groups is sufficient to obtain an effective catalyst. It is assumed that if a predetermined amount (number of moles) of bridging moieties are attached to a predetermined amount (g) of nanoparticles, then virtually all of the bridging moieties are attached to the nanoparticles and remain substantially attached during the method of the invention.
[0042] In step c of the method, degradation of the polymer occurs in the reaction mixture to form monomers under reaction conditions using a catalyst. Preferably, the reaction mixture is heated to a suitable temperature, which is preferably maintained during depolymerization. The temperature may be selected in the range of 170°C to 250°C. In a preferred embodiment, the degradation step may include forming monomers at a temperature in the range of 185°C to 225°C. Suitable pressures in the reactor are 1 to 5 bar, with pressures above 1.0 bar being preferred, more preferably below 3.0 bar.
[0043] The catalyst can be recovered to a large extent to the extent that it is insoluble in the solvent but heterogeneous. In step d, the catalyst is recovered from the reaction mixture. Separation occurs, for example, in a centrifuge. The presence of any aggregates is considered to be advantageous because it can make the phase separation more effective.
[0044] The method also includes adding at least one base to at least one reaction step in reaction steps a, b, c or d. The effect of adding a base is to improve the degradation reaction of polymer degradation to its oligomers and monomers by reducing the reaction time and / or reducing the formation of by-products. The base can be added to step a together with the polymer or solvent or separately. According to the nature of the base, the base can be added as a solid, or dissolved in water or a solvent. In the case of using a non-volatile base, it is preferred that the base is added in solid form, or it is at least partially dissolved in the solvent used in step a of the method. In the case of adding a volatile base, it is preferably dissolved in water or the solvent of the reaction mixture. The base can also be added to step b of the method together with a reusable catalyst or separately. The base can also be added in step c of the method before or during the degradation of the polymer in the reaction mixture.
[0045] The base can also be added in step d of the process before or during the recovery of the catalyst from the reaction mixture. The base has an effect on the separation of the catalyst from the reaction mixture. The separation is improved and the catalyst can be recovered more easily.
[0046] The amount of base added to the reaction mixture relative to the amount of catalyst is preferably in the range of 0.1:1 to 40:1, more preferably in the range of 1:1 to 35:1, and most preferably in the range of 2:1 to 5:1.
[0047] Advantageously, before or during the recovery of the catalyst, water is added to the reaction mixture. Water can be added separately, or added with alkali. The step of adding water with or without alkali in the reaction mixture has produced a first aqueous phase comprising monomer and dimer, and a second phase comprising oligomer, catalyst complex and aggregate, and the first phase is separated from the second phase. This has been shown to be an effective way to remove various pollutants. In a preferred embodiment of the present invention, the second phase is processed to reduce its water content, and is recycled in the reactor vessel thereafter. The reduction of water content can be carried out in several ways, for example, by means of evaporation, such as by distillation and / or membrane distillation.
[0048] The recovery step according to the method preferably comprises separating the catalyst from the reaction mixture. The separation step is more preferably carried out using a centrifuge. Alternatively, the separation step is preferably carried out using magnetic separation and / or applying an electric field. In a preferred embodiment in which water is added to the reaction mixture, the separation is preferably carried out at a temperature between 60°C and 100°C, more preferably between 75°C and 95°C. If water is not present, the separation can be carried out at a higher temperature.
[0049] Advantageously, water or aqueous solution added to the reaction mixture before or during the recovery of the catalyst can serve as a coolant. It can be provided at ambient temperature or any higher temperature, and is preferably a liquid. However, it is not excluded that a separate cooling device is provided. Due to the addition of water or aqueous solution, two phases will occur, wherein the first phase is an aqueous phase comprising a solvent, a monomer and at least some dimers and trimers. The second phase is a slurry comprising various solids, which includes a catalyst, an oligomer, a trimer and a solvent.
[0050] The amount of water added to the reaction mixture in step d is preferably such that the weight ratio of water to solvent is in the range of 0.2 to 5.0, more preferably in the range of 0.5 to 1.5, even more preferably in the range of 0.7 to 1.3, and most preferably in the range of 0.9 to 1.1. The more water is added, the more precipitation of catalyst and oligomers generally occurs. However, this also generally means that more water needs to be distilled to separate or reuse the catalyst and oligomers.
[0051] In preferred embodiments where both base and water are added, the weight ratio of base to water is in the range of 0.01 to 1.0, more preferably in the range of 0.05 to 0.5, and most preferably in the range of 0.08 to 0.12. Preferably, an amount of water and / or base is added to raise the pH of the reaction mixture to above 6.
[0052] The amount of catalyst relative to the amount of polymer is quite low. Preferably, it is in the range of 0.001:10 to 1:10, more preferably in the range of 0.005:10 to 0.3:10, and most preferably in the range of (0.008 to 0.015):10.
[0053] The base added to at least one reaction step is preferably a volatile base comprising an aqueous solution of ammonia and / or trialkylamine. Suitable amine-containing compounds are disclosed, for example, in WO2015056377A1, which is expressly incorporated herein for the listed amine-containing compounds. The use of a volatile base is advantageous because the aqueous phase is recycled and less or no elemental contamination of the product is observed.
[0054] In alternative embodiments, the base added to the reaction mixture before or during the recovery of the catalyst is preferably a non-volatile base comprising a metal hydroxide. More preferably, the metal hydroxide comprises lithium hydroxide (LiOH), sodium hydroxide (NaOH), potassium hydroxide (KOH), rubidium hydroxide (RbOH), cesium hydroxide (CsOH), magnesium hydroxide (Mg(OH)), calcium hydroxide (Ca(OH)), strontium hydroxide (Sr(OH)), barium hydroxide (Ba(OH)), tetramethylammonium hydroxide (N(CH3)4OH), potassium tert-butoxide, sodium bicarbonate and guanidine (HNC(NH2)2).
[0055] If the base is a non-volatile base comprising a metal hydroxide, the base is preferably added in step a or step b of the process. In addition, a non-volatile base or a volatile base may also be added to step d of the process to improve the recovery of the catalyst from the reaction mixture. Thus, the base may be the same base, or the base added in step d may be a volatile base. The base added in step a or b acts as a co-catalyst for the depolymerization reaction. Due to the presence of the base, the depolymerization rate is increased and the formation of by-products is also suppressed.
[0056] According to other embodiments of the present invention, the recovery step d is preferably carried out directly after the addition of water and / or base.
[0057] In an embodiment of the invention, water and base are added to the reaction mixture before or during recovery of the catalyst in step d at a temperature below 160° C., preferably below 100° C. For optimal aggregate formation and oligomer precipitation, it is advantageous to perform this addition at lower temperatures.
[0058] Advantageously, after the degradation step, the reaction mixture is cooled to below 170°C before the step of adding water and / or a base. The water is preferably water at a temperature of at least 85°C.
[0059] The invention also relates to the use of a base as described above as a co-catalyst for a catalyst for degrading a polymer in a reaction mixture. The base is active in the reaction and, since it preferably remains in the system, it may have an effect on both the depolymerization reaction and the recovery of the catalyst.
[0060] We have found that, for example, NaOH is a promising co-catalyst, since the addition of NaOH increases the activity of the depolymerization catalyst in the depolymerization reaction, while, for example, the yield of BHEET remains unchanged. Furthermore, the separability of the catalyst is improved with the addition of NaOH.
[0061] It may be important to avoid excessive production of BHEET in the reactor during depolymerization. BHEET is defined by Formula I:
[0062]
[0063] It has been demonstrated that the claimed catalyst (i.e., a reusable catalyst complex capable of degrading a polymer into oligomers and / or monomers), preferably comprising a catalyst entity, metal-containing particles, a bridging moiety for connecting the catalyst entity to magnetic particles, and a base, produces a reduced amount of BHEET for the same BHET yield when compared to other catalysts. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] The above and other advantages of the features and objects of the present invention will become more apparent and the invention will be better understood from the following detailed description when read in conjunction with the accompanying drawings, in which:
[0065] Figure 1 The separation efficiency of the catalyst with the addition of several bases is shown.
[0066] Figure 2 The results of Experiment 11, ie, the yield of BHET, are shown graphically.
[0067] Figure 3 The formation of the by-product BHEET is shown schematically.
[0068] Figure 4 The separation efficiency of the ABC catalyst complex with the addition of other bases is shown.
[0069] Figure 5 The separation efficiency of the ABC catalyst complex with the addition of a specific base is shown. DETAILED DESCRIPTION
[0070] The following non-limiting examples are provided to illustrate the invention.
[0071] experiment
[0072] Comparative experiment A: Separation efficiency - catalyst ABC
[0073] A 600 ml flask was used for the separation experiment. An amount of 0.017 g of the iron-based ABC catalyst complex was used in combination with 16.7 g of bis(2-hydroxyethyl)terephthalate (BHET). 125 g of ethylene glycol (EG) and 125 g of water were added to the reaction mixture.
[0074] The flask was heated to 80 to 100°C and mixed at this temperature to ensure that the BHET was dissolved. The depolymerized mixture was transferred to a 50 ml centrifuge tube. The mixture was centrifuged at 4000 rpm for 3 min. The supernatant was separated by decantation and then cooled to crystallize the BHET product present in the supernatant. The BHET crystals were filtered out from the mother liquor using a Büchner filter and dried in a vacuum oven at 60°C. The dried BHET and mother liquor were then analyzed by XRF to estimate the separability of the catalyst from the mixture. Figure 1 The separation efficiency expressed as % of catalyst present is depicted.
[0075] Example 1: Separation efficiency - catalyst ABC + ammonia
[0076] A 600 ml flask was used for the separation experiment. An amount of 0.017 g of the iron-based ABC catalyst complex was used in combination with 16.7 g of bis(2-hydroxyethyl)terephthalate (BHET). 125 g of ethylene glycol (EG) and 125 g of water were added to the reaction mixture. 0.125 g of 28% ammonia solution was added to the mixture. The same procedure for the depolymerization reaction described in Comparative Experiment A was used. Figure 1 The separation efficiency expressed as % of catalyst present is depicted.
[0077] Example 2: Separation efficiency - Catalyst ABC + NaOH
[0078] A 600 ml flask was used for the separation experiment. An amount of 0.017 g of the iron-based ABC catalyst complex was used in combination with 16.7 g of bis(2-hydroxyethyl)terephthalate (BHET). 125 g of ethylene glycol (EG) and 125 g of water were added to the reaction mixture. 0.05 g of sodium hydroxide was added to the mixture. The same procedure for the depolymerization reaction described in Comparative Experiment A was used. Figure 1 The separation efficiency expressed as % of catalyst present is depicted.
[0079] Example 3: Separation efficiency - Catalyst ABC + LiOH
[0080] A 600 ml flask was used for the separation experiment. An amount of 0.017 g of the iron-based ABC catalyst complex was used in combination with 16.7 g of bis(2-hydroxyethyl)terephthalate (BHET). 125 g of ethylene glycol (EG) and 125 g of water were added to the reaction mixture. 0.1 g of lithium hydroxide was added to the mixture. The same procedure for the depolymerization reaction described in Comparative Experiment A was used. Figure 1 The separation efficiency expressed as % of catalyst present is depicted.
[0081] Example 4: Separation efficiency - catalyst ABC + Na2CO3
[0082] A 600 ml flask was used for the separation experiment. An amount of 0.017 g of the iron-based ABC catalyst complex was used in combination with 16.7 g of bis(2-hydroxyethyl)terephthalate (BHET). 125 g of ethylene glycol (EG) and 125 g of water were added to the reaction mixture. 0.5 g of sodium carbonate was added to the mixture. The same procedure for the depolymerization reaction described in Comparative Experiment A was used. Figure 1 The separation efficiency expressed as % of catalyst present is depicted.
[0083] Example 5: Separation efficiency - catalyst ABC + triethylamine (TEA)
[0084] A 600 ml flask was used for the separation experiment. An amount of 0.017 g of the iron-based ABC catalyst complex was used in combination with 16.7 g of bis(2-hydroxyethyl)terephthalate (BHET). 125 g of ethylene glycol (EG) and 125 g of water were added to the reaction mixture. 0.5 g of triethylamine was added to the mixture. The same procedure of the depolymerization reaction described in Comparative Experiment A was used. Figure 1 The separation efficiency expressed as % of catalyst present is depicted.
[0085] Example 6: Separation efficiency - catalyst ABC + tripropylamine (TPA)
[0086] A 600 ml flask was used for the separation experiment. An amount of 0.017 g of the iron-based ABC catalyst complex was used in combination with 16.7 g of bis(2-hydroxyethyl)terephthalate (BHET). 125 g of ethylene glycol (EG) and 125 g of water were added to the reaction mixture. 0.05 g of tripropylamine was added to the mixture. The same procedure for the depolymerization reaction described in Comparative Experiment A was used. Figure 1 The separation efficiency expressed as % of catalyst present is depicted.
[0087] Example 7: Separation efficiency - Catalyst ABC + 1-methylimidazole (NMI)
[0088] A 600 ml flask was used for the separation experiment. An amount of 0.017 g of the iron-based ABC catalyst complex was used in combination with 16.7 g of bis(2-hydroxyethyl)terephthalate (BHET). 125 g of ethylene glycol (EG) and 125 g of water were added to the reaction mixture. 0.05 g of 1-methylimidazole was added to the mixture. The same procedure for the depolymerization reaction described in Comparative Experiment A was used. Figure 1 The separation efficiency expressed as % of catalyst present is depicted.
[0089] Example 8: Separation Efficiency - Catalyst ABC + N"-pentamethyldiethylenetriamine (PMDETA)
[0090] A 600 ml flask was used for the separation experiment. An amount of 0.017 g of the iron-based ABC catalyst complex was used in combination with 16.7 g of bis(2-hydroxyethyl)terephthalate (BHET). 125 g of ethylene glycol (EG) and 125 g of water were added to the reaction mixture. 0.5 g of N″-pentamethyldiethylenetriamine was added to the mixture. The same procedure for the depolymerization reaction described in Comparative Experiment A was used. Figure 1 The separation efficiency expressed as % of catalyst present is depicted.
[0091] Comparative experiment B: Separation efficiency - Fe3O4
[0092] A 600 ml flask was used for the separation experiment. An amount of 0.017 g of Fe3O4 was used in combination with 16.7 g of bis(2-hydroxyethyl)terephthalate (BHET). 125 g of ethylene glycol (EG) and 125 g of water were added to the reaction mixture. The same procedure of the depolymerization reaction described in Comparative Experiment A was used. Figure 1 The separation efficiency expressed as % of catalyst present is depicted.
[0093] Example 9: Separation efficiency - Fe3O4+NaOH
[0094] A 600 ml flask was used for the separation experiment. An amount of 0.017 g of Fe3O4 was used in combination with 16.7 g of bis(2-hydroxyethyl)terephthalate (BHET). 125 g of ethylene glycol (EG) and 125 g of water were added to the reaction mixture. 0.05 g of sodium hydroxide was added to the mixture. The same procedure of the depolymerization reaction described in Comparative Experiment A was used. Figure 1 The separation efficiency expressed as % of catalyst present is depicted.
[0095] Example 10: Depolymerization reaction
[0096] The depolymerization experiments were carried out in a 500 ml round bottom flask. 0.034 g of the iron-based ABC catalyst complex or 0.05 g of NaOH or a combination thereof was mixed with 33.4 g of polyethylene terephthalate (PET) flakes (0.3 × 0.3 cm 2 The reaction mixture was followed in time by collecting process control samples to measure the concentration of the monomer (bis(2-hydroxyethyl)terephthalate or BHET) and by-products (such as 2-(2-hydroxyethoxy)ethyl(2-hydroxyethyl)terephthalate or BHEET) produced over time. The concentrations of BHET and BHEET were determined using HPLC.
[0097] The results are Figure 2 and Figure 3 Given in Figure 2 In the figure, the yield of BHET as a function of reaction time for various catalyst systems is shown. The ABC catalyst with NaOH as a cocatalyst is faster in the conversion of polymer to BHET. Figure 3 In Figure 1, the formation of the byproduct BHEET is shown as a function of reaction time for various catalyst systems. The presence of sodium hydroxide as a co-catalyst significantly inhibits the formation of BHEET.
[0098] Comparative Example C: Separation Efficiency - Catalyst ABC
[0099] The same procedure as the depolymerization reaction described in Example 10 was used with 0.034 g of the iron-based ABC catalyst complex. After 240 min at 197°C, the reaction was stopped by cooling to below 160°C. The reaction mixture was transferred to a beaker through a mesh filter to remove the remaining solids. Water was added to obtain a 1:1 water:EG ratio. The mixture was mixed. A sample was collected before centrifugation. The mixture was transferred to a centrifuge tube and centrifuged at 4000 rpm for 3 min. A sample was collected after centrifugation. The sample was analyzed by XRF to estimate the separability. The results are shown in Table 1. Figure 4 Shown in.
[0100] Example 11: Separation Efficiency - Catalyst ABC + NaOH and Water
[0101] The same procedure as the depolymerization reaction described in Example 10 was used with 0.034 g of the iron-based ABC catalyst complex and 0.05 g of NaOH. After 240 min at 197°C, the reaction was stopped by cooling to below 160°C. The reaction mixture was transferred to a beaker through a mesh filter to remove the remaining solids. Water was added to obtain a 1:1 water:EG ratio. The mixture was mixed. A sample was collected before centrifugation. The mixture was transferred to a centrifuge tube and centrifuged at 4000 rpm for 3 min. A sample was collected after centrifugation. The sample was analyzed by XRF to estimate the separability. The results are in Figure 4 Shown in.
[0102] Example 12: Separation efficiency - Catalyst ABC + NaOH (anhydrous)
[0103] The same procedure as the depolymerization reaction described in Example 10 was used with 0.034 g of the iron-based ABC catalyst complex and 0.05 g of NaOH. After 240 min at 197°C, the reaction was stopped by cooling to below 160°C. The reaction mixture was transferred to a beaker through a mesh filter to remove the remaining solids. The mixture was mixed. A sample was collected before centrifugation. The mixture was transferred to a centrifuge tube and centrifuged at 4000 rpm for 3 min. A sample was collected after centrifugation. The sample was analyzed by XRF to estimate the separability. The results are in Figure 4 Shown in.
[0104] Example 13: Separation efficiency - Catalyst ABC + KOH (anhydrous)
[0105] The same procedure as the depolymerization reaction described in Example 10 was used with 0.034 g of the iron-based ABC catalyst complex and 0.05 g of KOH. After 240 min at 197°C, the reaction was stopped by cooling to below 160°C. The reaction mixture was transferred to a beaker through a mesh filter to remove the remaining solids. The mixture was mixed. A sample was collected before centrifugation. The mixture was transferred to a centrifuge tube and centrifuged at 4000 rpm for 3 min. A sample was collected after centrifugation. The sample was analyzed by XRF to estimate the separability. The results are in Figure 4 Shown in.
[0106] Comparative Example D: Catalyst ABC
[0107] The depolymerization experiment was carried out using a 600 ml stainless steel high pressure reactor. 0.4 g of the iron-based ABC catalyst complex was mixed with 40 g of polyethylene terephthalate (PET) flakes (0.1 × 0.02 cm 2The reactor was placed in a heating unit. Heating was started and after 25 minutes the reaction mixture reached a reaction temperature of 210°C. After 240 min at 210°C the reaction was stopped by cooling to below 160°C. The reaction mixture was transferred to a beaker through a mesh filter to remove the remaining solids. Water was added to obtain a water:EG ratio of 0.8:1. The mixture was mixed. A sample was collected before centrifugation. The mixture was transferred to a centrifuge tube and centrifuged at 4000 rpm for 3 min. A sample was collected after centrifugation. The sample was analyzed by XRF to estimate the separability. Figure 1 The separation efficiency is shown.
[0108] Example 14: Catalyst ABC + NaOH
[0109] The same procedure for the depolymerization described in Comparative Example D was used with 0.4 g of the iron-based ABC catalyst complex and 0.6 of NaOH. Figure 5 Shown are the separation efficiencies obtained in Comparative Example D and Example 14. The results show that the separation efficiency of the ABC catalyst increases significantly with the addition of NaOH, also at a higher reaction temperature of 210°C.
Claims
1. A method for obtaining a monomer by degrading a polymer, wherein the polymer is a homopolymer or a copolymer of the monomer, the method comprising the following steps: a. providing the polymer and a solvent as a reaction mixture in a reactor, wherein the solvent is a reactant capable of reacting with the polymer to degrade the polymer into oligomers and at least one monomer; b. providing a reusable catalyst capable of degrading said polymer into said oligomers and said at least one monomer; c. degrading the polymer in the reaction mixture using the catalyst under reaction conditions to form the at least one monomer; and d. recovering the catalyst from the reaction mixture; The method further comprises adding at least one base to the reaction mixture in at least one of reaction steps a to d.
2. The process according to claim 1, wherein water is added to the reaction mixture before or during recovery of the catalyst.
3. The process according to claim 2, wherein the water is added to the reaction mixture in an amount such that the weight ratio of water to solvent is in the range of 0.2 to 5.0, preferably in the range of 0.5 to 1.5, more preferably in the range of 0.7 and 1.3 and even more preferably in the range of 0.9 and 1.
1.
4. The process according to claim 2 or 3, wherein the base is added to the reaction mixture in an amount such that the weight ratio of base to water is in the range of 0.01 to 1.0, preferably in the range of 0.05 to 0.5 and more preferably in the range of 0.08 to 0.
12.
5. The process according to any one of the preceding claims, wherein the amount of the catalyst is in the range of 0.001:10 to 1:10, preferably in the range of 0.005:10 to 0.3:10, and more preferably in the range of (0.008 to 0.015):10 relative to the amount of the polymer.
6. The process according to claim 5, wherein the base is added to the reaction mixture in an amount in the range of 0.1:1 to 40:1, preferably in the range of 1:1 to 35:1 and more preferably in the range of 2:1 to 5:1, relative to the amount of the catalyst.
7. A process according to any one of the preceding claims, wherein the base is a volatile base comprising an aqueous solution of ammonia and / or a trialkylamine.
8. The process according to any one of claims 1 to 6, wherein the base is a non-volatile base comprising a metal hydroxide.
9. The method of claim 8, wherein the metal hydroxide comprises at least one of lithium hydroxide (LiOH), sodium hydroxide (NaOH), potassium hydroxide (KOH), rubidium hydroxide (RbOH), cesium hydroxide (CsOH), magnesium hydroxide (Mg(OH)), calcium hydroxide (Ca(OH)), strontium hydroxide (Sr(OH)), barium hydroxide (Ba(OH)), tetramethylammonium hydroxide (N(CH3)4OH) and guanidine (HNC(NH2)2).
10. The process according to claims 7 to 9, wherein the base is added in step a or step b.
11. The process of claim 2, wherein water is added to the reaction mixture before recovering the catalyst in step d.
12. The process according to any one of the preceding claims, wherein after the degradation step, the reaction mixture is cooled to below 170°C.
13. The process according to claim 2, wherein the addition of water to the reaction mixture before or during the recovery of the catalyst in step d is carried out at a temperature below 160°C, preferably below 100°C.
14. A process according to any one of the preceding claims, wherein the base is added in an amount to raise the pH of the reaction mixture to above 6.
15. The process according to any one of the preceding claims, wherein the recovery step comprises separating the catalyst from the reaction mixture.
16. The method of claim 15, wherein the separation step is performed using a centrifuge.
17. The method of claim 15, wherein the separation step is performed using magnetic separation and / or application of an electric field.
18. The process according to any one of claims 15 to 17, wherein the separation is performed at a temperature between 60°C and 100°C, preferably between 75°C and 95°C.
19. A method according to any of the preceding claims, wherein the reusable catalyst comprises a catalyst complex comprising a catalyst entity, metal-containing nanoparticles and a bridging portion connecting the catalyst entity to magnetic nanoparticles, wherein the catalyst entity comprises a cationic portion having a positive charge and an anionic portion having a negative charge and preferably providing a negative counterion.
20. The method according to any one of the preceding claims, wherein the weight ratio of the solvent, preferably ethylene glycol, to the polymer is in the range of 20:10 to 100:10, more preferably in the range of 40:10 to 90:10, and most preferably in the range of 60:10 to 80:
10.
21. A process according to any one of the preceding claims, wherein the polymer concentration in the dispersion is from 1 to 30% by weight, based on the total weight of the reaction mixture.
22. The method according to any one of the preceding claims, wherein the degradation step c comprises forming the monomer at a temperature higher than 170°C and preferably at most 250°C, at a pressure higher than 1.0 bar and preferably lower than 3.0 bar.
23. Use of a base according to claims 7 to 9 as a cocatalyst for a catalyst for degrading a polymer in a reaction mixture under reaction conditions.
24. Use according to claim 23, wherein the base is a non-volatile base.
25. Use according to claim 23 or 24 as a co-catalyst for the catalyst according to claim 19.