Light diffusing thermoplastic composition

By adding an ultraviolet stabilizer to the resin composition of the light-diffusing particles and adding an appropriate amount of ultraviolet stabilizer to the polymer composition, the problem of the light-diffusing thermoplastic composition turning yellow under ultraviolet radiation is solved and its stability is improved. properties and transmission properties.

CN118786173APending Publication Date: 2024-10-15SABIC GLOBAL TECHNOLOGIES BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024487.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-15
Filing Date
2023-04-12
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing light-diffusing thermoplastic compositions are prone to yellowing under UV radiation, affecting their color properties and transmission properties. Especially in polycarbonate and acrylic resins, deeper penetration of UV radiation leads to more serious yellowing problems.

Method used

Adding an ultraviolet stabilizer to the resin composition of the light-diffusing particles, combined with an appropriate proportion of the ultraviolet stabilizer in the polymer composition, can reduce the undesired effects of ultraviolet radiation and improve the ultraviolet stability of the composition.

Benefits of technology

Significantly reduces the impact of UV radiation on light-diffusing thermoplastic compositions, reduces color changes and loss of transmission properties, and extends the service life and stability of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a thermoplastic composition comprising 92.5-99.9% by weight of a polymer composition and 0.1-7.5% by weight of light diffusing particles wherein at least part of the light diffusing particles consist of a resin composition comprising at least one ultraviolet stabilizer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a light-diffusing thermoplastic composition comprising a polymer composition and light-diffusing particles dispersed therein. The present invention further relates to an article comprising or consisting of the light-diffusing thermoplastic composition and the light-diffusing particles.

[0002] Light-diffusing thermoplastic compositions are known per se and are used in particular in lighting applications. Thus, by way of example, the light-diffusing thermoplastic composition can be used in light-diffusing sheets or panels and as daylighting covers, in particular for LED lighting applications.

[0003] Articles comprising or consisting of the light diffusing composition can be used in applications exposed to ultraviolet radiation, which may affect the color properties of the article. For example, polycarbonate has a tendency to yellow after prolonged exposure to ultraviolet radiation. Solutions to minimize this problem are known in the art. For example, it is well known to add UV stabilizers to polymers and / or to apply UV absorbing protective coatings or protective layers to or on the article. Alternatively, colorants such as, in particular, blue dyes can be used to counteract the yellowing so that the observer does not notice the yellow / yellowish color of the material.

[0004] An important property of a light diffusing composition is that for a certain amount of diffusivity, the transmittance, i.e. the fraction of visible light that passes through the material, is as high as possible. For example, in LED lighting applications, it is desirable that on the one hand the actual LED light source is not observed, while at the same time the amount of light transmitted by the LED source and passing through the light diffusing article is as high as possible. Otherwise, the loss in transmittance must be compensated by a more powerful light source or less satisfactory light diffusion.

[0005] Therefore, the light diffusing particles are preferably made of a transparent resin such as acrylate, silicone, or polystyrene, which allows incident light to pass through the polymer composition as well as the resin of the light diffusing particles.

[0006] Although the use of transparent resins for light diffusing particles allows for a high transmission of visible light, it also means that ultraviolet light can pass through the particles, at least to some extent. Therefore, the resin of the light diffusing particles may be affected by ultraviolet radiation, or, depending on the resin, ultraviolet radiation may penetrate deeper into the polymer in which the light diffusing particles are dispersed, thereby risking a higher degree of yellowing over long periods of exposure to ultraviolet radiation. Light diffusing particles have been described in various publications in the past. WO2016190560 relates to a light diffusing powder comprising a polystyrene-based resin and polyorganosilsesquioxane particles having an average diameter (D50) of about 0.1-0.9 μm.

[0007] KR20080071673 relates to a light-resistant light-diffusing plate, a backlight device and a liquid crystal display device having the same. The patent application also describes a method for preparing light-diffusing particles composed of a cross-linked polymethyl methacrylate resin ultraviolet absorber.

[0008] However, there remains a need to further mitigate the effects of ultraviolet radiation on light diffusing thermoplastic compositions based on polymer compositions and resin-based light diffusing particles dispersed therein.

[0009] It is an object of the present invention to further mitigate the effects of ultraviolet radiation on light diffusing thermoplastic compositions based on polymer compositions and resin-based light diffusing particles dispersed therein.

[0010] In particular, the aim is to reduce the influence of ultraviolet radiation on light-diffusing thermoplastic compositions comprising polycarbonate as polymer and light-diffusing particles based on acrylate resins.

[0011] The present inventors have discovered that the undesirable effects of ultraviolet radiation can be reduced by adding an ultraviolet stabilizer to the resin composition that makes up the one or more light diffusing particles.

[0012] Therefore, the present invention relates to a thermoplastic composition, which comprises A) 92.5-99.9 wt % of a polymer composition and B) 0.1-7.5 wt % of light diffusing particles, based on the weight of the composition, wherein at least part of the light diffusing particles consists of a resin composition comprising at least one UV stabilizer. In the composition of the present invention, preferably the sum of components (A) and (B) is 100 wt %.

[0013] More specifically, the present invention relates to a thermoplastic composition comprising, based on the weight of the composition: A) 92.5-99.9 wt. % of a polymer composition comprising polycarbonate, and B) 0.1-7.5 wt. % of light diffusing particles, wherein at least a portion of the light diffusing particles are composed of a cross-linked acrylic resin composition comprising at least one UV stabilizer.

[0014] Although the basic concept of the present invention does not impose any restrictions on the polymer composition (A) or the resin composition (B) of the light diffusing particles in principle, the present invention is particularly applicable to thermoplastic compositions in which the polymer composition comprises or consists of polycarbonate, polymethyl (meth)acrylate or a mixture of polycarbonate and polymethyl (meth)acrylate.

[0015] These materials are known to have high visible light transmission combined with good mechanical properties and processability. Polycarbonate and polymethyl (meth)acrylate are therefore generally the polymers used for lighting applications.

[0016] The basic concept is particularly useful in compositions in which the transmission of UV radiation is different for the polymer composition and the resin composition of the light diffusing particles. Thus, the invention is particularly relevant to compositions in which the polymer composition has a lower transmission of UV radiation than the UV transmission of the resin composition of the light diffusing particles.

[0017] For the purposes of the present invention, the visible spectrum is assumed to be in the range of 400-800nm, so that the UV range starts from 400nm. Bisphenol A polycarbonate allows transmission of UV radiation as low as about 300nm, but below about 300nm polycarbonate becomes opaque to UV radiation. It is important that the transparency of polycarbonate has been significantly reduced from 400-300nm. On the other hand, polymethyl (meth) acrylate only becomes opaque to UV radiation below about 250nm, meaning that polymethyl (meth) acrylate allows more UV radiation to pass through. In practice, materials on the surface of the earth are mainly exposed to radiation referred to as UV-A and UV-B. UV-A radiation generally has a wavelength of 315-400nm, while UV-B radiation is 280-315nm. Lower wavelengths are generally blocked by the earth's atmosphere. This means that polymethyl (meth) acrylate is generally considered to be "transparent" to ultraviolet radiation.

[0018] As a result of the above, acrylate-based particles embedded near the outer surface of a polycarbonate polymer composition tend to allow UV radiation to penetrate deeper into the polycarbonate, thereby increasing the amount of polycarbonate that may be affected by the effects of UV radiation, such as, for example, yellowing of the polymer. Additionally, because these particles are generally spherical, more polycarbonate may be exposed to UV radiation.

[0019] Polycarbonate

[0020] Particularly preferred polymers for lighting applications are polycarbonates. Therefore, the polymer composition (A) preferably comprises at least 60 wt.-%, more preferably at least 70 wt.-%, 80 wt.-%, 90 wt.-%, 95 wt.-% or 99 wt.-% of polycarbonate (A1), and at most 30 wt.-%, 20 wt.-%, 10 wt.-%, 5 wt.-%, 1 wt.-% of additional component (A2), based on the weight of the polymer composition (A).

[0021] Polycarbonate A1 preferably includes bisphenol A polycarbonate homopolymer, which can be an interfacial polycarbonate or a molten polycarbonate. As is well known to the technician, the interfacial polycarbonate is made by reacting bisphenol A and phosgene in a two-phase liquid reaction system, then separating the two phases and isolating the polycarbonate. The interfacial polycarbonate usually has a very small amount of phenolic hydroxyl groups, such as up to 150ppm, up to 100ppm, up to 50ppm or preferably up to 25ppm of ~OH groups based on the weight of the polymer. In contrast to molten polycarbonate, the interfacial polycarbonate usually does not contain any Fries branching units. Molten polycarbonate is usually obtained by reacting bisphenol A and diphenyl carbonate in a molten state via ester exchange. The reaction involves relatively high temperature and low pressure in order to promote ester exchange. In view of the process, the molten polycarbonate essentially has a much higher phenol end group and contains a large amount of Fries branching units.

[0022] In one aspect, the polymer composition (A) comprises polycarbonate as the only polymer component and thus contains no further polymers. In another aspect, the polymer composition comprises further polymer components comprised in one or more further components A2.

[0023] The polycarbonate in the polymer composition (A) may be an interfacial polycarbonate, a molten polycarbonate, or a mixture of a molten polycarbonate and an interfacial polycarbonate.

[0024] The melt flow rate (MFR) of the polycarbonate is not particularly limited and may be 3-60 g / 10 min, preferably 5-40 g / 10 min (ISO 1133, 300° C., 1.2 kg). Because lighting applications are usually complex parts with at least partially thin wall thicknesses, the polycarbonate preferably has an MFR of 18-40, such as 20-35 g / 10 min.

[0025] The polycarbonate may be a mixture of two or more polycarbonates having mutually different MFRs. If the polycarbonate is a mixture, the melt flow rate of the mixture is preferably 5-40 g / 10 min (ISO 1133, 300° C., 1.2 kg), and more preferably 18-40, such as 20-35 g / 10 min.

[0026] The polycarbonate may comprise or consist of a partially branched polycarbonate, which is typically obtained by reacting bisphenol A and phosgene or diphenyl carbonate in the presence of a branching agent such as 1,1,1-tris(4-hydroxyphenyl)ethane (THPE). Branched polycarbonates are known per se and are advantageously used for applications requiring high melt strength. For example, the polycarbonate may be a mixture of 10-90% by weight of a linear polycarbonate and 90-10% by weight of a branched polycarbonate, based on the combined weight of the linear polycarbonate and the branched polycarbonate.

[0027] In one aspect of the present invention, wherein the polymer composition (A) comprises the polycarbonate in an amount of at least 60 wt.-%, 70 wt.-%, 80 wt.-%, 90 wt.-%, 95 wt.-% or 99 wt.-%, the melt flow rate of the polymer composition (A) is preferably 3-60, preferably 5-40 g / 10 min (ISO 1133, 300° C., 1.2 kg), and more preferably 18-40, such as 20-35 g / 10 min.

[0028] The additional component A2 comprises additional polymer components, non-polymer components and additives, as known to the technicians themselves. For example, additives as part of the additional component A2 may include antioxidants, flame retardants, flame retardant synergists, anti-drip agents, heat stabilizers, release agents, colorants such as pigments or dyes, and ultraviolet stabilizers. The present invention is not limited in this regard, and any additive commonly used in similar applications can be included in the polymer composition (A), provided that it retains the suitability for the intended application. In one aspect of the present invention, the polymer composition comprises 0.05-0.5% by weight, preferably 0.1-0.3% by weight of ultraviolet stabilizers. The polymer composition may also be free of ultraviolet stabilizers. Preferably, the polymer composition is free of ultraviolet stabilizers. The wording "free of" used herein means that the polymer composition has less than 0.1% by weight, preferably less than 0.01% by weight of ultraviolet stabilizers. Additives are included in the additional component A2.

[0029] The polymer composition preferably comprises at least 50 wt %, more preferably at least 75 wt % polycarbonate based on the weight of the polymer composition. More preferably, the polymer composition comprises at least 85 wt %, at least 90 wt % or at least 95 wt % polycarbonate. Preferably, the polycarbonate is the only polymer contained in the polymer composition, and the thermoplastic composition does not contain any other polymer.

[0030] Poly(methyl meth)acrylate

[0031] Another polymer commonly used in lighting applications is polymethyl (meth)acrylate.

[0032] Poly(methyl methacrylate) polymers are known per se to the technician, including their use for optical applications. Poly(methyl methacrylate) is generally obtained via free radical polymerization of a mixture comprising methyl methacrylate. These mixtures generally contain at least 40% by weight, preferably at least 60% by weight and particularly preferably at least 80% by weight of methyl methacrylate based on the weight of the monomer. Together with this, these mixtures for the preparation of poly(methyl methacrylate) may contain other (meth) acrylates that can be copolymerized with methyl methacrylate. The term (meth) acrylate encompasses methacrylates and acrylates, as well as mixtures of the two. These monomers are well known to the technician. Poly(methyl methacrylate) is not particularly limited, and any commercially available material can be used. Various poly(meth) acrylates that differ, for example, in their molecular weight or monomer composition can be used.

[0033] The weight average molecular weight of polymethyl (meth)acrylate may be 20,000-1,000,000 g / mol, preferably 50,000 to 500,000 g / mol and particularly preferably 80,000 to 300,000 g / mol. Light diffusing applications based on polymethyl (meth)acrylate formulations are disclosed, for example, in US Pat. Nos. 7,629,041 and 8,609,011.

[0034] The additional components included in the polymer composition (A) may be additional polymer components, non-polymer components and additives, as known to the technician per se. For example, the additive may include an antioxidant, a flame retardant, a flame retardant synergist, an anti-drip agent, a heat stabilizer, a release agent, a colorant such as a pigment or a dye, and a UV stabilizer. The present invention is not limited in this regard, and any additive commonly used in similar applications may be included in the polymer composition (A), provided that it retains suitability for the intended application. In one aspect of the invention, the polymer composition comprises 0.05-0.5 wt %, preferably 0.1-0.3 wt % of a UV stabilizer. The polymer composition may be free of a UV stabilizer.

[0035] Mixture of polycarbonate and polymethyl (meth)acrylate

[0036] In one aspect of the invention, the polymer composition is a mixture A1 based on polymethyl (meth)acrylate and polycarbonate, wherein the mixture consists of 40-60% by weight of polycarbonate and 60-40% by weight of polymethyl (meth)acrylate, based on the weight of the mixture.

[0037] In this aspect, the polymer composition (A) preferably comprises at least 60 wt.-%, more preferably at least 70 wt.-%, 80 wt.-%, 90 wt.-%, 95 wt.-% or 99 wt.-% of this mixture (A1), and at most 30 wt.-%, 20 wt.-%, 10 wt.-%, 5 wt.-%, 1 wt.-% of a further component (A2), based on the weight of the polymer composition (A).

[0038] Further mixtures of polymethyl (meth)acrylate and polycarbonate are considered part of the aspect wherein the polymer composition comprises at least 60 wt. % of polymethyl (meth)acrylate or polycarbonate, as the case may be and as described above.

[0039] Other component A2 comprises other polymer components, non-polymer components and additives, as known to the technicians themselves. For example, additives as the part of other component A2 may include antioxidants, flame retardants, flame retardant synergists, anti-drip agents, heat stabilizers, release agents, colorants such as pigments or dyes, and ultraviolet stabilizers. The present invention is not limited in this respect, and any additive commonly used in similar applications can be included in polymer composition (A), provided that it retains the suitability for the intended application. In one aspect of the present invention, polymer composition comprises 0.05-0.5 weight %, preferably 0.1-0.3 weight % ultraviolet stabilizer. Polymer composition also may not contain ultraviolet stabilizer. Additives are included in other component A2.

[0040] Light Diffusing Particles

[0041] The light-diffusing particles are known to the technicians themselves and are easily commercially available. Preferably, the light-diffusing particles are composed of an acrylate-based resin composition or a silicone-based resin composition, both of which are known to the technicians themselves. In one aspect of the present invention, at least part of the light-diffusing particles are composed of a resin composition comprising at least one UV stabilizer. The light-diffusing particles are composed of an acrylate-based resin composition or a silicone-based resin composition. Preferably, the light-diffusing particles are composed of an acrylate-based resin composition. Preferably, the acrylate-based resin composition is a cross-linked (meth) acrylic resin. Preferably, the light-diffusing particles are composed of a cross-linked (meth) acrylic resin.

[0042] Silicone-based resins are also commonly referred to as polyorganosilsesquioxanes. Such resin compositions are typically crosslinked, which allows the particles to substantially retain their shape during melt blending with the polymer composition and not become elongated, deformed, or even diluted by the polymer composition.

[0043] For the purpose of providing the desired light diffusion, the particles preferably have a diameter of at most 100 μm, such as at most 80 μm, preferably 0.5 to 50 μm, more preferably 0.5 to 10 μm, even more preferably 1 to 5 μm, wherein the diameter is determined by laser diffraction according to ISO 13320: 2020. Light diffusing particles having a relatively large diameter, such as 10-50 μm, are not excluded per se, but may be less preferred for use in light diffusing sheets based on polycarbonate.

[0044] The particle size indicates the 50% value (D50) of the integrated distribution of particle sizes obtained by the laser diffraction / scattering method. The number of particle size distributions may be singular or plural. That is, it is possible to combine two or more types of light diffusing particles that differ in average particle size and / or resin composition. Preferably, the light diffusing particles have a narrow particle size distribution.

[0045] The preferred shape of the particles is spherical.The light diffusing particles may have a maximum diameter (Dmax) and a minimum diameter (Dmin), wherein Dmax ≥ Dmin and the ratio Dmax / Dmin is 1-1.5, preferably 1-1.2, more preferably 1-1.05, most preferably 1-1.01.

[0046] Examples of the cross-linked silicone resin light-diffusing particles include KMP590 manufactured by Shin-Etsu Chemical Co. Ltd., Tospearl 120, Tospearl 145 manufactured by Momentive Performance Materials.

[0047] Examples of crosslinked (meth) acrylic resin light diffusing particles include TECHPOLYMER MBX series manufactured by SEKISUI PLASTICS CO. Ltd., such as MBX-5, MBX-8, MBX-12, MBX-20, MBX-30, MBX-2H, MB30X-5, MB30X-8, MB30X-20, MB30X-30, MBX-25H and the like. The light diffusing particles of the MBX series contain crosslinked polymethyl methacrylate, are substantially spherical and have a refractive index of 1.49. As described above, the light diffusing particles are optically transparent.

[0048] The resin composition of the light diffusing particles comprises at least one UV stabilizer. Preferably, when the light diffusing particles comprise a UV stabilizer, the polymer composition does not contain a UV stabilizer.

[0049] Depending on the type of resin, any known UV stabilizer for similar materials, i.e. polymers, may be used, and the invention is not limited to any particular type. Examples include hindered amine light stabilizers (HALS) and benzotriazole-based light stabilizers, benzophenone-based light stabilizers, triazine-based light stabilizers, cyanoacrylate-based light stabilizers, benzoxazine-based light stabilizers. The amount of UV stabilizer is preferably 0.01-5% by weight, preferably 0.03-3% by weight, more preferably 0.05-1% by weight, based on the weight of the resin composition of the light diffusing particles.

[0050] The amount of light diffusing particles is 0.1-7.5 wt % based on the weight of the thermoplastic composition. Preferably, the amount of light diffusing particles is 0.1-5 wt %, more preferably 0.2-3 wt %.

[0051] Thermoplastic composition

[0052] For the desired light diffusion, it is preferred that the refractive index of the light diffusing particles and the refractive index of the polymer composition are different. Thus, when measured according to ISO 489 at a wavelength of 589 nm and a temperature of 23° C., it is preferred that the absolute difference between the refractive index of the polymer composition and the refractive index of the light diffusing particles is at least 0.01, preferably 0.03-0.3, more preferably 0.05 to 0.2, even more preferably 0.08-0.15. Typically the refractive index of the polymer composition is higher than the refractive index of the light diffusing particles.

[0053] The polymer composition preferably comprises or consists of polycarbonate, polymethyl (meth)acrylate or a mixture of polycarbonate and polymethyl (meth)acrylate, preferably polycarbonate.

[0054] The light diffusing particles are uniformly dispersed in the polymer composition, which can be achieved by known compounding techniques.

[0055] Preferably, the thermoplastic composition comprises, based on the weight of the composition: (A) 92.5 to 99.9 weight percent of a polymer composition comprising:

[0056] A1) at least 60% by weight, more preferably at least 70%, 80%, 90%, 95% or 99% by weight of polycarbonate (A1), and

[0057] A2) up to 30 wt. %, 20 wt. %, 10 wt. %, 5 wt. %, 1 wt. % of further components;

[0058] B) 0.1 to 7.5 wt.% of light diffusing particles, wherein at least a portion of the light diffusing particles consists of a resin composition comprising at least one ultraviolet stabilizer, and wherein the resin composition is a crosslinked (meth)acrylic resin.

[0059] With regard to the resin composition of polycarbonate and light diffusing particles, the same preferences as described above apply.

[0060] Preferably, the sum of components A and B constitutes a total of 100 wt% of the thermoplastic composition, based on the weight of the thermoplastic composition. In this preferred aspect of the invention, the amount of non-polymeric material (i.e., part of polymer composition A) may be up to 3 wt%, preferably up to 2 wt%, more preferably up to 1 wt%, based on the weight of the polymer composition.

[0061] The thermoplastic composition according to the present invention is generally substantially free of materials that reduce visible light transmission. Therefore, the thermoplastic composition disclosed herein is preferably free of inorganic particulate fillers or pigments, and / or impact modifiers. In some applications, small amounts, such as up to 2 wt%, preferably up to 1 wt%, of inorganic pigments, such as titanium dioxide, may be added to impart a desired color effect.

[0062] The present invention further relates to an article comprising or consisting of the thermoplastic composition disclosed herein. In particular, the present invention relates to a light diffusing plate or sheet obtained by molding a thermoplastic composition. Such an article, in particular such a sheet or plate, may have at least one portion having a thickness of 0.1-10 mm, preferably 0.5-5 mm. Although as mentioned above, thicker applications are not excluded per se, and the article may also have at least one portion having a thickness of at most 25 mm, at most 20 mm or at most 15 mm.

[0063] The article may be obtained by extrusion into a film, sheet, tube or profile, as known per se to the skilled person. Alternatively, the article may be moulded, such as for example by injection moulding.

[0064] The present invention will now be further illustrated based on the following non-limiting examples.

[0065] The polycarbonate (PC) used in the following experiments is commercially available from SABIC and has a 28 cm 3 Interfacial bisphenol A polycarbonate homopolymer with a melt volume rate (MVR) of / 10min. PC does not contain UV stabilizers.

[0066] The light diffusing particles (LD) are cross-linked polymethyl methacrylate resin particles having an average particle size of 5 μm, commercially available from SEKISUIPLASTICS CO. Ltd. as Techpolymer MBX-5.

[0067] UV stabilized light diffusing particles (LD_UV) are crosslinked polymethylmethacrylate resin particles having an average particle size of 5 μm and contain a UV stabilizer. The particles are similar to the LD particles except for the presence of the UV stabilizer.

[0068] The ultraviolet light stabilizer (UV) was 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol, commercially available as Tinuvin 5411.

[0069] The compositions were molded into 2.5 mm plaques and subjected to a weathering test according to ISO 11341 by exposing the plaques to a 2.5 mm ion beam having an intensity of 0.5 W / m at 340 nm at a temperature of 65°C using a quartz inner filter and a CIRA-soda lime glass outer filter. 2 The radiant power is filtered xenon arc radiation. The panels were exposed to UV radiation for 2246 hours.

[0070] Visible light transmission was measured on a Byk Gardner Dual hazeguard according to ASTM D1003-00.

[0071] The color properties L*, a*, b* and resulting dE* were measured according to ASTM E308-15 (Standard Practice for Calculating the Color of Objects Using the CIE System) on an X-rite 7000a spectrophotometer excluding the specular component, using CIE illuminant D65 and a 10° observer, in transmission mode.

[0072] Before weathering of the molded panels, the color values ​​L*_in, a*_in, b*_in and T% were determined. After weathering of the molded panels, the color difference values ​​dL*, da*, db*, dE*, dT* and dHaze were determined.

[0073] The experimental results are shown in Tables 1 and 2 below.

[0074] Table 1 CE1 CE2 CE3 CE4 CE5 E1 E2 E3 E4 PC [weight%] 100 99.70 99.25 98.50 97.0 99.70 99.25 98.50 97.0 UV [weight%] LD [weight%] 0.30 0.75 1.50 3.0 LD_UV [weight%] 0.30 0.75 1.50 3.0 L*_in 95.8 92.7 89.6 81.3 73.0 94.0 84.5 81.2 74.3 a*_in -0.04 0.06 0.29 0.63 0.39 0.02 0.54 0.64 0.22 b*_in 0.6 2.2 3.8 4.5 2.5 1.9 5.0 4.8 2.5 T% [%] 92.5 90.3 82.2 67.9 58.4 89.5 79.4 67.9 57.4 dL* -1.1 0.4 -1.6 -2.9 -1.2 -1.6 1.9 -1.4 -3.1 da* -1.97 -2.01 -1.78 -1.80 -2.07 -1.73 -1.65 -1.49 -1.54 db* 7.8 7.7 8.4 9.1 11.1 7.7 6.8 7.5 8.6 dE* 8.2 7.9 8.7 9.7 11.4 8.1 7.3 7.8 9.3 dT% [%] -4.3 -7.4 -8.6 -8.8 -9.3 -8.3 -8.7 -8.5 -8.8 dFog [%] 2.6 1.5 0.8 1.8 2.0 2.0 2.0 2.0 2.0

[0075] In the compositions of the examples, the UV stabilizer UV is part of the polymer composition, ie it is part of the polycarbonate PC.

[0076] Table 2 CE6 CE7 CE8 CE9 CE10 E5 E6 E7 E8 PC [weight%] 99.85 99.55 99.10 98.35 96.85 99.55 99.10 98.35 96.85 UV [weight%] 0.15 0.15 0.15 0.15 0.15 0.15 0.15 0.15 0.15 LD [weight%] 0.30 0.75 1.50 3.0 LD_UV [weight%] 0.30 0.75 1.50 3.0 L*_in 95.8 94.2 89.3 81.0 70.7 94.2 87.8 78.1 73.9 a*_in -0.10 -0.07 0.22 0.51 0.15 -0.10 0.32 0.57 0.07 b*_in 0.6 1.8 4.1 4.8 2.7 2.0 4.7 4.7 2.7 T% [%] 92.4 90 81.9 67.4 58.1 89.6 78.9 64.9 57.3 dL* -0.5 0.0 -0.4 -1.4 2.7 -0.5 -0.5 0.6 -2.0 da* -0.72 -0.75 -0.68 -0.74 -0.95 -0.65 -0.76 -0.84 -0.95 db* 3.1 2.9 3.1 3.9 5.2 2.9 3.6 4.1 5.2 dE* 3.2 3.0 3.2 4.2 5.9 3.0 3.7 4.3 5.6 dT% [%] -3.0 -5.4 -6.7 -7.1 -8.1 -5.8 -6.8 -7.4 -8.1 dFog [%] 1.8 1.3 1.0 2.0 1.8 2.0 1.9 2.0 2.0

[0077] From Tables 1 and 2, the inventors conclude that the presence of UV stabilizers in the light-diffusing particles does improve the weathering of molded parts consisting of polycarbonate and said particles. The inventors believe in particular that the dE* value (i.e. the result of the color change) represents this observation. When the UV stabilizer is also added to the polycarbonate, a further improvement in the color change is observed. In view of this result, the inventors believe that the amount of UV stabilizer in the polymer composition, i.e. in the polycarbonate, can be further reduced, thereby allowing a reduction in the manufacturing cost of the composition. Therefore, the inventors believe that the optimization of the type and amount of UV stabilizers in the polymer composition, in particular in the polycarbonate and in the light-diffusing particles allows cost reduction and / or improved weathering performance.

Claims

1. A thermoplastic composition comprising, based on the weight of the composition: A) 92.5 to 99.9 wt. % of a polymer composition comprising polycarbonate, and B) 0.1-7.5% by weight of light diffusing particles, At least a portion of the light diffusing particles is composed of a cross-linked acrylic resin composition comprising at least one ultraviolet stabilizer.

2. The composition according to claim 1, wherein the absolute difference between the refractive index of the polymer composition and the refractive index of the light diffusing particles when measured according to ISO 489 at a wavelength of 589 nm and a temperature of 23°C is at least 0.01, preferably 0.03-0.3, more preferably 0.05 to 0.2, even more preferably 0.08-0.

15.

3. The composition according to any one or more of claims 1 to 2, wherein the polymer composition comprises 0.05 to 0.5, preferably 0.1 to 0.3 wt. % of UV stabilizer.

4. The composition according to any one or more of claims 1 to 3, wherein the amount of UV stabilizer in the light diffusing particles containing the UV stabilizer is 0.05 to 5% by weight.

5. The composition according to any one or more of claims 1 to 4, wherein the polymer composition further comprises polymethyl (meth)acrylate.

6. The composition according to any one or more of claims 1 to 5, wherein the polycarbonate is an interfacial polycarbonate.

7. The composition according to any one or more of claims 1 to 6, wherein the polycarbonate is a bisphenol A polycarbonate homopolymer.

8. A product comprising or consisting of a composition according to any one or more of claims 1 to 7.

9. The article according to claim 8, wherein the article is a light diffusing plate or sheet obtained by molding the composition according to any one or more of claims 1 to 7.

10. The article according to claim 8, wherein the article is obtained by extrusion into a film, a sheet, a tube or a profile.

11. Use of light-diffusing particles consisting of a resin composition comprising at least one UV stabilizer for imparting light-diffusing properties and resistance to UV radiation to polymer compositions.

12. Light-diffusing particles composed of a cross-linked acrylic resin, a cross-linked polystyrene resin or a silicone resin, and comprising 0.05 to 5% by weight of an ultraviolet stabilizer based on the weight of the acrylic resin, the polystyrene resin or the silicone resin.

13. Light diffusing particles according to claim 12, wherein the particles have a diameter of 0.5 to 100 μm, preferably 0.5 to 50 μm, more preferably 1 to 5 μm, wherein the diameter is determined by laser diffraction according to ISO 13320:2020.

14. The light diffusing particles according to claim 12 or 13, wherein the particles have a maximum diameter (D max ) and minimum diameter (D min ), where D max ≥D min And the ratio D max / D min 1-1.5, preferably 1-1.2, wherein the diameter is measured by laser diffraction according to ISO 13320:2020.