Catalyst with modified active phase dispersion and method for preparing catalyst with modified active phase dispersion
By replacing aluminum atoms and loading active metals on ultra-stable Y-type zeolite, combined with an inorganic oxide binder, the problem of cost and property balance in the manufacturing of existing hydrocracking catalysts is solved, and efficient molding and excellent performance of catalyst particles are achieved. .
Patent Information
- Application Number
- CN202380017495.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-18
- Filing Date
- 2023-01-16
- Publication Date
- 2024-10-15
AI Technical Summary
Existing hydrocracking catalysts have difficulty in balancing cost and chemical and physical properties during the manufacturing process, and the shape and size of the catalyst particles have an important impact on performance, but the existing process is difficult to effectively control.
Ultra-stable Y-type zeolite containing zirconium, titanium and hafnium instead of aluminum atoms is used as the framework of the catalyst particles, and active metals are loaded on it. Through composite molding and heat treatment with inorganic oxide binders, it forms a structure with excellent mechanical properties. Properties and catalytic activity of catalyst particles.
It improves the wear resistance, surface area and pore size distribution of the catalyst, enhances the catalytic activity, reduces the blocking of mesopores, and improves the yield of the middle distillate and the hydrocracking efficiency.
Smart Images

Figure BDA0004948582380000351 
Figure BDA0004948582380000361 
Figure HDA0004948582400000011
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for producing a catalyst including a USY-type zeolite. Background Art
[0002] Catalysts, including hydrotreating / hydrocracking catalysts, such as pretreatment catalysts, typically include one or more amorphous-based catalysts, such as amorphous alumina or silica-alumina or titania matrix containing active metal Ni / Mo, Ni / W or Co / Mo metal as active phase, or amorphous catalysts, zeolite catalysts, or their composite mixtures promoted by Ni, W, Mo and Co metals. Conventional zeolites are USY. Hydrocracking catalysts include hydrogenation active metal components and acidic carrier components. In some embodiments, the hydrocracking catalyst includes any one of an amorphous alumina catalyst, an amorphous silica-alumina catalyst, a titania catalyst, a natural or synthetic zeolite-based catalyst, a modified zeolite, or a combination thereof. The hydrocracking catalyst may be provided with an active phase material, and in some embodiments, the active phase material includes any one of Ni, W, Mo, Co, or a combination thereof or a combination thereof. In other embodiments, typically in a sulfur-free environment for hydrogenation and / or reforming, the catalyst may include one or more precious metals, such as Ru, Rh, Pd, Ag, Os, Ir, Pt, or Au. In some embodiments where the purpose is hydrodenitrogenation, a catalyst based on acidic alumina or silica alumina loaded with Ni-Mo or Ni-W active metals or a combination thereof is used. In embodiments where the purpose is to remove all nitrogen and increase the conversion of hydrocarbons, silica alumina, zeolite, or a combination thereof with an active metal (including Ni-Mo, Ni-W, or a combination thereof) is used as a catalyst.
[0003] U.S. Patent Nos. 9,221,036, 10,081,009, and 10,293,332 (the '036, '009, and '332 patents, or the '036 family of patents), owned by the applicant of the present invention and incorporated by reference in their entirety, teach, inter alia, hydrocracking catalysts in which the USY framework is partially replaced with one or more of zirconium, titanium, and hafnium. In these catalysts, the replacement metal (Ti, Zr, and / or Hf) replaces a portion of the aluminum in the aluminum / silicon framework and essentially becomes part of the framework. Processes (methods) for preparing these catalysts and their uses are described in the '036, '009, and '332 patents.
[0004] Hydroprocessing (hydrotreating and hydrocracking) catalysts can be manufactured by a variety of methods. The method selected generally represents a balance between manufacturing costs and the degree to which the desired chemical and physical properties are achieved. Although there is a relationship between catalyst formulation, preparation process and catalyst properties, the details of this relationship have not been fully understood due to the complex nature of catalyst systems. The chemical composition of the catalyst plays a key role in its performance; physical and mechanical properties also play an important role. The preparation of hydrocracking catalysts involves multiple steps: precipitation, filtration (decantation, centrifugation), washing, drying, forming, calcination and impregnation. Other steps are typically required, such as kneading / grinding, grinding and screening. Described below are the steps that are part of the hydrocracking catalyst manufacturing process.
[0005] Precipitation involves mixing a solution or suspension of materials, resulting in the formation of a precipitate, which may be crystalline or amorphous. Kneading / grinding of wet solid materials generally results in the formation of a dough, which is subsequently shaped and dried. The kneaded / grinded product is subjected to heat treatment in order to obtain a closer contact between the components and better homogeneity by heat diffusion and solid state reactions. The metal component is then added by impregnation or incipient wetting methods.
[0006] The characteristics of the support determine the mechanical properties of the catalyst, such as wear resistance, hardness and crush strength. Generally, a high surface area and an appropriate pore size distribution are required. The pore size distribution and other physical properties of catalyst supports prepared by precipitation are also affected by the precipitation and aging conditions of the precipitate and the subsequent drying, shaping and calcining.
[0007] The final shape and size of the catalyst particles are determined in the manufacturing step. The catalyst and catalyst support are formed into a variety of possible shapes, such as spheres, cylindrical extrudates, or shaped forms, such as trilobes or quadrilobes. Spherical catalyst support catalysts can be obtained by the "oil drop method", whereby precipitation occurs when the liquid is poured into the second immiscible liquid. Other spherical processes include marbleization (marmurizing). Generally, due to cost and process considerations such as pressure drop, most current catalysts are formed into shapes other than spheres. Fewer spherical catalysts are used in modern hydrocracking. Non-spherical shapes are obtained as follows: mixing raw materials to form an extrudable dough-like object, which is extruded through a die with perforations. The spaghetti-like (spaghetti) extrudate is dried, calcined, and broken into small pieces. The typical aspect ratio of the catalyst substrate varies, for example, between 2 and 4.
[0008] FIG. 1 shows a typical hydrocracking catalyst manufacturing step: mixing and kneading a binder component and a zeolite component; extruding the kneaded composite mixture and forming composite particles; calcining the composite particles; impregnating the calcined composite particles with an active metal component; and calcining the impregnated composite particles to form a final catalyst product.
[0009] Examples of the shapes of catalysts and catalyst supports are shown in Figure 2. The simplest form is cylindrical, but other forms such as trilobes, twisted trilobes, or quadrilobes are also used commercially. Catalysts with multilobed cross sections have a higher surface area to volume ratio than simple cylindrical extrudates. When used in a fixed bed, these shaped catalyst particles help reduce diffusion resistance, create a more open bed, and reduce pressure drop.
[0010] Before and / or after the shaped catalyst is impregnated, a heat treatment is applied. For catalyst support materials prepared by precipitation or co-grinding of all components, it may only be necessary to dry before shaping, followed by calcining the shaped product. Heat treatment of the catalyst or support eliminates water and other volatile substances. Drying and calcining conditions are crucial for determining the physical and catalytic properties of the catalyst support material. Surface area, pore size distribution, stability, wear resistance, crushing strength and catalytic activity are affected by drying and calcining conditions.
[0011] In conventional catalyst preparation, active metals can be added to catalyst support materials using a variety of methods: (a) immersion (impregnation), (b) initial wetness, and (c) evaporation. In one method, the calcined catalyst support material is immersed in an excess of a solution containing an active metal or metal compound. The solution fills the pores and also adsorbs on the support surface, and the excess solution is removed. In another method, the initial wetness method is used to impregnate the activated support by tumbling or spraying a certain volume of solution, the metal compound concentration of which is tailored to achieve a target metal level equal to or slightly less than the pore volume of the support. The metal-loaded catalyst support material is then dried and calcined. Metal oxides are formed in the process; the calcination step is also called oxidation. In another method (evaporative impregnation), the catalyst support material is saturated with water or an acid solution and immersed in an aqueous solution containing a metal compound. The compound then diffuses into the pores of the catalyst support material through the aqueous phase. The calcined catalyst is bagged and sent to the final destination.
[0012] In the '036 family, the active metal components are added after the framework-modified USY zeolite is mixed with a binder, kneaded and extruded.While the catalyst particles produced by the methods taught in the '036 family are suitable for their intended purpose, the industry is continually seeking improved catalyst particles and methods for making the same. Summary of the invention
[0013] Catalyst particles containing one or more active metal components and methods for making such catalyst particles are provided. The particles are a composite of a granulating agent or binder material (e.g., an inorganic oxide) and an ultrastable Y (hereinafter "USY") zeolite, wherein some of the aluminum atoms in the framework are replaced by zirconium atoms and / or titanium atoms and / or hafnium atoms. One or more active phase components are incorporated before the binder is mixed with the USY zeolite after framework modification, the resulting composite mixture is extruded, and the catalyst particles are formed. Before the catalyst particles are formed, the one or more active phase components are incorporated into the USY zeolite after the framework modification.
[0014] The method for preparing catalyst particles includes: providing a framework-modified ultrastable Y-type (USY) zeolite, wherein a portion of the aluminum atoms constituting its zeolite framework are replaced by zirconium atoms and / or titanium atoms and / or hafnium atoms, wherein the framework-modified USY zeolite is characterized by an outer surface and pores defining an inner surface; impregnating one or more active metal components on the outer surface and / or the inner surface of the pores of the framework-modified USY zeolite to form a metal-loaded framework-modified USY zeolite; mixing and kneading the metal-loaded framework-modified USY zeolite with an inorganic oxide binder material to form a composite of the metal-loaded framework-modified USY zeolite and the inorganic oxide binder; molding catalyst particles from the composite of the metal-loaded framework-modified USY zeolite and the inorganic oxide binder into extrudates; heat-treating the extrudates; and collecting the calcined catalyst particles.
[0015] In some embodiments of the above method, the one or more active metal components impregnated on the USY zeolite after the skeleton modification are the first part of the total active metal component content of the one or more active metal components. The inorganic oxide binder material is characterized by an outer surface and a hole defining an inner surface, and the method further comprises: before mixing and kneading, the second part of the total active metal component content of the one or more active metal components is impregnated on the outer surface and / or the inner surface of the hole of the inorganic oxide binder material to form a metal-loaded inorganic oxide binder. Therefore, the metal-loaded skeleton-modified USY zeolite and the metal-loaded inorganic oxide binder are mixed and kneaded to form a composite of the metal-loaded skeleton-modified USY zeolite and the metal-loaded inorganic oxide binder, and the catalyst particles are formed by the composite of the metal-loaded skeleton-modified USY zeolite and the metal-loaded inorganic oxide binder.
[0016] In some embodiments of the above method, the one or more active metal components impregnated on the USY zeolite after the framework modification are the first part of the total active metal component content of the one or more active metal components. The calcined catalyst particles are intermediate calcined catalyst particles, and are characterized by an outer surface and pores defining an inner surface, and the method further includes impregnating a second part of the total active metal component content of the one or more active metal components on the outer surface and / or the inner surface of the pores of the intermediate calcined catalyst particles, heat treating the intermediate calcined catalyst particles loaded with metal, and collecting the final calcined catalyst particles.
[0017] In some embodiments of the above method, the one or more active metal components impregnated on the USY zeolite after the framework modification are the first part of the total active metal component content of the one or more active metal components. The composite of the metal-loaded USY zeolite after the framework modification and the inorganic oxide binder is characterized by an outer surface and pores defining an inner surface, and the method further includes impregnating a second part of the total active metal component content of the one or more active metal components on the outer surface and / or the inner surface of the pores of the composite of the metal-loaded USY zeolite after the framework modification and the inorganic oxide binder.
[0018] The calcined catalyst particles provided herein comprise a composite of a framework-modified ultrastable Y (USY) zeolite in which a portion of the aluminum atoms constituting the zeolite framework are replaced by zirconium atoms and / or titanium atoms and / or hafnium atoms, wherein the framework-modified USY zeolite is characterized by an outer surface and pores defining an inner surface, and wherein the outer surface and / or the inner surface of the pores are metal-loaded with one or more active metal components; and an inorganic oxide binder material. The composite is formed into an extrudate and heat-treated into a final calcined catalyst particle.
[0019] In some embodiments of the above methods and compositions, the USY zeolite after the framework modification is provided in a wet state, a dry state or a calcined state. In some embodiments of the above methods and compositions, the USY zeolite after the framework modification contains 0.1 to 5% by mass of zirconium and / or titanium and / or hafnium calculated on an oxide basis. In some embodiments of the above methods and compositions, the inorganic oxide material is selected from alumina, silica, titania, silica-alumina, alumina-titania, alumina-zirconium oxide, alumina-borium oxide, phosphorus-alumina, silica-alumina-borium oxide, phosphorus-alumina-borium oxide, phosphorus-alumina-silicon oxide, silica-alumina-titania, and silica-alumina-zirconium oxide. In some embodiments of the above methods and compositions, the USY zeolite after the framework modification of the metal load accounts for about 0.1-99% by weight of the composite catalyst particles containing active metals, wherein the remaining mass comprises an inorganic oxide component. In some embodiments of the above methods and compositions, the catalyst particles are formed by skeleton-modified USY zeolite, inorganic oxide components, and additional zeolite components. In some embodiments of the above methods and compositions, the metal-loaded skeleton-modified USY zeolite accounts for about 0.1-99% by weight of the catalyst particles, wherein the first remaining mass comprises an inorganic oxide component, and wherein the second remaining mass comprises an additional zeolite component. In some embodiments of the above methods and compositions, the active metal component is selected from a metal group consisting of platinum, palladium, and rhenium, and wherein in terms of the mass of the active metal component, the active metal component is present in an amount of 0.01-2% by weight, relative to the mass of the catalyst particles. In some embodiments of the above methods and compositions, the active metal component is selected from a metal group consisting of Mo, W, Co, Ni, and combinations thereof, and wherein in terms of the mass of the active metal component, the active metal component is present in an amount of 0.1-40% by weight, based on the mass of the catalyst particles.
[0020] Other aspects, embodiments, and advantages of these exemplary aspects and embodiments are discussed in detail below. In addition, it should be understood that the foregoing information and the following detailed description are merely exemplary examples of various aspects and embodiments, and are intended to provide an overview or framework for understanding the nature and characteristics of the claimed aspects and embodiments, and for explaining the principles and operations of the described and claimed aspects and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The invention will be described in further detail below and with reference to the accompanying drawings, in which in some cases the same or similar elements are referred to by the same reference numerals, and in which:
[0022] FIG1 is a simplified process flow diagram for producing catalyst particles according to a known method;
[0023] Figure 2 shows the shape of the catalyst particles;
[0024] FIG3 is a process flow diagram showing the steps for producing catalyst particles according to a known method;
[0025] Figure 4 A process flow diagram showing the steps for producing catalyst particles according to embodiments herein, wherein active metals are impregnated in a framework-substituted USY zeolite material;
[0026] Figure 5 A process flow diagram showing the steps for producing catalyst particles according to embodiments herein, wherein active metals are impregnated in a framework-substituted USY zeolite material and in a binder material;
[0027] Figure 6 A process flow diagram showing the steps for producing catalyst particles according to embodiments herein, wherein active metals are impregnated into framework-substituted USY zeolite materials and extrudates of metal-loaded zeolite and binder materials; and
[0028] Figure 7 is a process flow diagram showing possible steps for producing catalyst particles according to various embodiments herein. DETAILED DESCRIPTION
[0029] The present disclosure provides a method for making catalyst particles containing one or more active metal components. The particles are a composite of (a) a granulating agent or binder material (e.g., an inorganic oxide) and (b) an ultrastable Y (hereinafter "USY") zeolite, in which some of the aluminum atoms in the framework are replaced by zirconium atoms and / or titanium atoms and / or hafnium atoms. In the method of the present invention, one or more active phase components are incorporated into the USY zeolite after the framework modification before the catalyst particles are formed. In an embodiment of the method of the present invention, the one or more active phase components are incorporated before the binder is mixed with the USY zeolite after the framework modification, the resulting composite mixture is extruded, and the catalyst particles are formed. This is in contrast to the known method in which active metal components are added to the near-final particles that have been calcined and formed. In contrast, by impregnating the USY zeolite after the framework modification with one or more active metal components before mixing and kneading the zeolite with the binder, some advantages are provided to manufacturers. In the process disclosed in the '036 family of patents, when the metal impregnation is on an as-produced support of the zeolite combined with a binder, a majority of the active metal tends to be deposited on the binder. Thus, metal impregnation on framework-modified USY zeolite is effective in increasing the middle distillate yield in the hydrocracking of vacuum gas oils.
[0030] In some embodiments, the catalyst particles formed according to the present invention herein are suitable for hydrocracking heavy hydrocarbon oils obtained from crude oil, synthetic crude oil, asphalt, oil sands, shell oil or coal liquid. The above heavy hydrocarbon oil is preferably any one of the following: a) vacuum gas oil (VGO), b) deasphalted oil (DAO) or demetallized oil obtained from a solvent deasphalting process, c) light coker gas oil or heavy coker gas oil obtained from a coking process, d) cycle oil obtained from a fluid catalytic cracking (FCC) process, or e) gas oil obtained from a visbreaking process.
[0031] In some embodiments, the catalyst particles formed herein according to the present invention are suitable for use in the reforming of naphtha, as disclosed in US Patent 10,787,618, which is incorporated herein by reference in its entirety.
[0032] In some embodiments, the catalyst particles formed herein according to the present invention are suitable for hydrogenating an intermediate distillate and conditioning the intermediate distillate for steam cracking, as disclosed in US Patent Publications 2021 / 0246382A1, 2021 / 0246383A1, 2021 / 0246384A1, and 2021 / 0246389A1, the entireties of which are incorporated herein by reference; or for hydrogenating an intermediate distillate and conditioning the intermediate distillate for steam cracking and / or fluid catalytic cracking, as disclosed in US Patent Publication 2021 / 0246386A1, the entirety of which is incorporated herein by reference. In some embodiments, the catalyst particles formed herein according to the present invention are suitable for hydrogenating light cycle oil and conditioning the light cycle oil for steam cracking, as disclosed in US Patent Publication 2021 / 0246381A1, the entirety of which is incorporated herein by reference; or for hydrogenating light cycle oil and conditioning the light cycle oil for steam cracking and / or fluid catalytic cracking, as disclosed in US Patent Publication 2021 / 0246387A1, the entirety of which is incorporated herein by reference. In some embodiments, the catalyst particles formed herein according to the present invention are suitable for hydrogenating light coker gas oil and conditioning the light coker gas oil for steam cracking, as disclosed in US Patent Publication 2021 / 0246385A1, the entire text of which is incorporated herein by reference; or for hydrogenating light coker gas oil and conditioning the light coker gas oil for steam cracking and / or fluid catalytic cracking, as disclosed in US Patent Publication 2021 / 0246388A1, the entire text of which is incorporated herein by reference.
[0033] To facilitate description of the process of the present invention, FIG3 shows the process steps for producing a framework-modified USY zeolite and a catalyst particle having an active metal component on a composite support including a framework-modified USY zeolite and a binder. Some of these process steps are similar to those disclosed in the '036 patent family.
[0034] The catalyst particles produced according to the method of FIG. 3 are calcined composite support particles of the framework-modified USY zeolite described herein and a binder to which active metal components are added and subsequently calcined.
[0035] Steps 1-9 herein provide a description of a process for synthesizing a calcined USY zeolite (referred to herein as USY(c)), which is then subjected to framework modification in steps 10-13. In embodiments of the invention herein, the framework-modified USY may be obtained from another source, that is, one or more of steps 1-9 may be avoided. Steps 14-15 involve the preparation of an inorganic oxide binder, and steps 16-21 involve shaping the composite catalyst support particles (steps 16-18) and forming the final particles having an effective amount of active metal components (steps 19-21).
[0036] In step 1, Y-type zeolite (Na-Y) is prepared by forming a suspension of Na-Y at an effective concentration, for example, in a liquid / solid ratio range of about 5-20, 5-15, 8-15, 5-12 or 8-12 liters (L) of water / kilogram (kg) of zeolite, and at an effective temperature in the range of, for example, about 15-95, 15-80, 20-95, 20-90, 20-80, 40-95, 40-90 or 40-80°C.
[0037] The starting material of step 1 comprises the following Na-Y type zeolite: effective SiO2 / Al2O3 molar ratio (SAR), for example, in the range of about 3-6; effective unit cell size (UD), for example, about 2.466 nanometers (nm); effective specific surface area (SA), for example, about 600-900, 600-800, 650-900 or 650-800 square meters / gram (m 2 / g), and the effective Na2O content is, for example, about 13 mass %.
[0038] In the ion exchange step 2, a first ion-exchanged Y-type zeolite is synthesized by subjecting the Na-Y suspension from step 1 to an ion exchange of sodium ions of Na-Y with ammonium ions to prepare a first ion-exchanged Y-type zeolite (first NH4-Y). For some embodiments, in the first NH4-Y, about 50-70% of the Na contained in the Y-type zeolite is replaced by NH4, also referred to as NH4 50-70 Y.
[0039] An embodiment of the ion exchange of step 2 includes adding to the Na-Y suspension: an ammonium source at an effective concentration, such as a molar ratio of ammonium to Al in the range of about 2-8; at an effective temperature in the range of about 20-95, 20-90, 20-80, 40-95, 40-90 or 40-80° C.; and at an effective residence time in the range of, for example, about 10-600, 10-180, 30-600 or 30-180 minutes. The ammonium source can be one or more of NH4OH, (NH4)2SO4, (NH4)2CO3, or another suitable ammonium source.
[0040] The solid obtained from the ion exchange step 2 can be filtered, washed with water at an effective temperature in the range of, for example, about 20-95, 20-90, 20-80, 40-95, 40-90 or 40-80° C., and dried at an effective temperature in the range of, for example, about 80-180 or 100-180° C., for an effective residence time in the range of, for example, about 30-1800, 60-1800, 30-600 or 60-600 minutes to obtain the first ion-exchanged NH4-Y (NH4 50-70 Y).
[0041] Optionally, after washing the solids obtained from the ion exchange step 2, they may be washed with an ammonium source in one or more additional cycles at effective temperatures, concentrations and residence times (such as those of step 2), followed by water washes. The solid material washed one or more additional times is dried at effective temperatures and residence times (such as those of step 2) to obtain the first ion-exchanged NH4-Y (NH4 50-70 Y). In some cases, the one or more additional cycles of the first ion exchange step are not performed.
[0042] In the heat treatment step 3, the first ion-exchanged NH4-Y (NH4 50-70Y) synthesize hydrogen-type Y (HY) zeolite. In some embodiments, the heat treatment of step 3 includes calcining the first ion-exchanged NH4-Y at an effective temperature and for a time effective to produce HY zeolite, for example, at a temperature in the range of about 500-800, 500-700, 600-800 or 600-700°C (typically in the presence of steam, that is, in saturated water vapor, or in the presence of air or oxygen), and for a time range of about 10-600, 10-180, 30-600 or 30-180 minutes. In some embodiments, if there is still a significant amount of Na in the HY zeolite, the ion exchange can be repeated one or more times as in step 2. After additional ammonium ion exchange and steam treatment discussed below in steps 4-6, the HY zeolite is converted to USY.
[0043] In step 4-6, the HY zeolite is treated to synthesize a second ion-exchanged NH4-Y zeolite in which 80-97% of the Na contained in Na-Y is exchanged with NH4, also referred to as NH4 80-97 Y. For example, as described, in step 4, a suspension containing an effective concentration of HY zeolite is prepared, for example, in a solid / liquid mass ratio range of about 5-20, 5-15, 8-15, 5-12 or 8-12 L / kg (water / zeolite), and at an effective temperature in the range of, for example, about 15-95, 15-80, 20-95, 20-90, 20-80, 40-95, 40-90 or 40-80°C.
[0044] In the ion exchange step 5, a second ion-exchanged Y-type zeolite is synthesized by subjecting the NH4-Y suspension from step 4 to an ion exchange of 80-97 or 90-97% of the sodium ions of Na-Y with ammonium ions to prepare a second ammonium-exchanged Y-type zeolite (second NH4-Y) (NH4 80-97 Y). An embodiment of the ion exchange in step 5 includes adding and stirring an effective concentration of ammonium, such as a molar ratio of ammonium to Al in the range of about 2-8; at an effective temperature in the range of about 20-95, 20-90, 20-80, 40-95, 40-90, or 40-80° C.; and at an effective residence time in the range of, for example, about 10-600, 10-180, 30-600, or 30-180 minutes. The ammonium source may be one or more of NH4OH, (NH4)2SO4, (NH4)2CO3, or another suitable ammonium source.
[0045] In the ion exchange step 5, a second ion-exchanged Y-type zeolite is synthesized by subjecting the NH4-Y suspension from step 4 to an ion exchange of 80-97 or 90-97% of the sodium ions of Na-Y with ammonium ions to prepare a second ammonium-exchanged Y-type zeolite (second NH4-Y).80-97 Y. An embodiment of the ion exchange of step 5 includes adding and stirring an effective concentration of ammonium, such as a molar ratio of ammonium to Al in the range of about 2-8; at an effective temperature in the range of about 20-95, 20-90, 20-80, 40-95, 40-90 or 40-80° C.; and for an effective residence time in the range of, for example, about 10-600, 10-180, 30-600 or 30-180 minutes. The ammonium source can be one or more of NH4OH, (NH4)2SO4, (NH4)2CO3, or another suitable ammonium source.
[0046] The solid obtained from the ion exchange step 5 can be filtered, washed with water, for example, at an effective temperature in the range of about 20-95, 20-90, 20-80, 40-95, 40-90 or 40-80° C., and dried, for example, at an effective temperature in the range of about 80-180 or 100-180° C., for an effective residence time in the range of about 30-1800, 60-1800, 30-600 or 60-600 minutes, to obtain the second ion-exchanged NH4-Y (NH4 80-97 Y).
[0047] Optionally, after washing the solids resulting from the ion exchange step 5, they may be washed with an ammonium source in one or more additional cycles at an effective temperature, concentration, and residence time (such as those in step 5), followed by a water wash. The solids washed one or more additional times are dried at an effective temperature and residence time (such as those in step 5) to obtain the second ion-exchanged NH4-Y (NH4 80-97 Y). In some cases, the one or more additional cycles of the second ion exchange step are not performed.
[0048] In the heat treatment step 6, by calcining NH4 80-97 Y to synthesize a first ultrastable Y-type zeolite (referred to herein as USY(a)). The heat treatment in step 6 comprises calcining the second ion-exchanged NH4-Y at an effective temperature in the range of, for example, about 500-800, 500-700, 600-800 or 600-700°C (typically in the presence of steam, that is, in saturated water vapor, or in the presence of air or oxygen), and for a time in the range of about 10-600, 10-180, 30-600 or 30-180 minutes to recover USY(a). In some embodiments, NH4 80-97 The heat treatment of Y is by steam treatment.
[0049] The USY(a) from step 6 is a USY zeolite having a SAR approximately equivalent to that of the starting Na-Y. Steps 1-6 generally should not significantly change the SAR value, since these steps do not require acid treatment to target the removal of aluminum atoms from the zeolite framework. For example, the USY(a) thus obtained in step 6 may have a SAR of about 3-6.
[0050] In step 7-9, USY(a) zeolite is treated to synthesize a calcined USY zeolite with increased SAR, which is a starting material for subsequent framework modification. In step 7, an aqueous suspension containing an effective concentration of USY(a) is prepared, for example, in a solid / liquid mass ratio range of about 5-20, 5-15, 8-15, 5-12 or 8-12 L / kg (water / zeolite), and at an effective temperature in the range of, for example, about 15-95, 15-80, 20-95, 20-90, 20-80, 40-95, 40-90 or 40-80°C.
[0051] In the acid treatment step 8, an effective amount of an inorganic acid or an organic acid is dispersed in the suspension so that the pH of the suspension is maintained in the strongly acidic range to synthesize a second ultrastable Y-type zeolite (referred to herein as USY(b)) with increased SAR. Extra-framework aluminum (aluminum atoms that do not form part of the zeolite framework) is removed from USY(a) to obtain USY(b) zeolite. This is performed by acid treatment.
[0052] The inorganic acid used can generally be sulfuric acid, nitric acid, hydrochloric acid, etc. In some embodiments, the selected inorganic acid is sulfuric acid or hydrochloric acid. In addition, carboxylic acid can be suitably used as the above-mentioned organic acid. The amount of the inorganic acid or organic acid added is an amount suitable for controlling the pH of the suspension within a strongly acidic range (e.g., within the range of about 0.7-2.5, 0.7-2.0, 1.0-2.5 or 1.0-2.0). The amount can be, for example, 0.5-4.0 times, 0.5-3.5 times, 0.7-4.0 times or 0.7-3.5-0.5 times molar increase, based on the amount of Al2O3 in USY (a). The acidic suspension is maintained at an effective temperature, such as 15-95, 15-80, 20-95, 20-90, 20-80, 40-95, 40-90 or 40-80° C., and maintained for an effective residence time, such as in the range of about 10-600, 10-180, 30-600 or 30-180 minutes. The acid treatment of step 8 increases the SAR of the Y-type zeolite, for example, from a range of about 3-6 to a range of about 30-100, 40-100, 30-80 or 40-80.
[0053] The solid resulting from the acid treatment step 8 can be filtered, washed with water at an effective temperature in the range of, for example, about 15-95, 15-80, 20-95, 20-90, 20-80, 40-95, 40-90 or 40-80° C., and dried at an effective temperature in the range of, for example, about 80-180 or 100-180° C., for example, an effective residence time in the range of about 30-1800, 60-1800, 30-600 or 60-600 minutes to recover USY (b).
[0054] Optionally, after washing the solids obtained from the acid treatment step 8, they can be treated with an inorganic or organic acid in one or more additional cycles at an effective temperature, concentration and residence time (such as those in step 8), followed by washing with water. The solids treated with acid one or more times are dried at an effective temperature and residence time (such as those in step 8) to recover USY (b). In some cases, one or more additional cycles of the first acid treatment step are not performed.
[0055] In the heat treatment step 9, the USY(b) zeolite is subjected to heat treatment to prepare a third ultrastable Y-type zeolite USY(c). In some embodiments, the heat treatment of step 9 includes calcining the second USY zeolite (USY(b)) at an effective temperature in the range of, for example, about 500-700, 550-700, 500-650 or 550-650°C (typically in the presence of air or oxygen, or in the presence of steam), and for a time in the range of about 10-600, 10-180, 30-600 or 30-180 minutes to recover USY(c). If the calcination temperature is lower than about 500°C, the amount of framework substitution of zirconium atoms and / or titanium atoms and / or hafnium atoms tends to decrease; at a calcination temperature exceeding about 700°C, the specific surface area of the ultrastable Y-type zeolite may decrease, and thus the amount of framework substitution of zirconium atoms and / or titanium atoms and / or hafnium atoms decreases.
[0056] In steps 10-13, a framework substitution is performed to produce a framework-modified USY zeolite in which a portion of the aluminum atoms in the USY zeolite framework is replaced by zirconium and / or titanium and / or hafnium atoms. In some embodiments, a framework-modified USY zeolite material is produced by firing a USY zeolite having the properties described herein at about 500-700°C. A suspension containing the fired USY zeolite is formed, the suspension having a liquid / solid mass ratio of about 5-15. An inorganic acid or an organic acid is added so that the pH of the suspension is about <2.0. Subsequently, a solution containing a zirconium compound and / or a titanium compound and / or a hafnium compound is mixed. The solution is neutralized with, for example, aqueous ammonia so that the pH of the mixed solution is about 7-7.5.
[0057] The above-mentioned suitable zirconium compound includes one or more of zirconium sulfate, zirconium nitrate, zirconium chloride, etc. In some embodiments, zirconium sulfate and / or zirconium nitrate are selected. The amount of the zirconium compound added is generally about 0.1-5.0, 0.1-4.0, 0.1-3.0, 0.2-5.0, 0.2-4.0, 0.2-3.0, 0.3-5.0, 0.3-4.0 or 0.3-3.0 weight %, as calculated based on their oxide benchmark (i.e. zirconium oxide), and as measured relative to the mass of the USY zeolite component after the skeleton modification. Adding zirconium compound in an amount less than about 0.1 weight % cannot improve the solid acid characteristics of zeolite. Adding zirconium compound in an amount exceeding 5 weight % tends to cause the pores of zeolite to be blocked. The aqueous solution of the zirconium compound prepared by dissolving the zirconium compound in water can be used as the zirconium compound.
[0058] Suitable titanium compounds include one or more of titanium sulfate, titanium acetate, titanium chloride, titanium nitrate and titanium lactate. In some embodiments, titanium sulfate and / or titanium acetate are selected. The amount of the titanium compound added is generally about 0.1-5.0, 0.1-4.0, 0.1-3.0, 0.2-5.0, 0.2-4.0, 0.2-3.0, 0.3-5.0, 0.3-4.0 or 0.3-3.0 weight %, as calculated based on their oxide benchmarks (i.e. titanium oxide), and as measured relative to the mass of the USY zeolite component after the skeleton modification. Adding titanium compounds in an amount less than about 0.1 weight % cannot improve the solid acid characteristics of zeolite. Adding titanium compounds in an amount exceeding 5 weight % tends to cause the pores of zeolite to be blocked. The aqueous solution of the titanium compound prepared by dissolving the titanium compound in water can be used as the titanium compound.
[0059] The above-mentioned suitable hafnium compound includes one or more of hafnium chloride, hafnium nitrate, hafnium fluoride, hafnium bromide, hafnium oxalate, etc. In some embodiments, hafnium chloride and / or hafnium nitrate are selected. The amount of the added hafnium compound is generally about 0.1-5.0, 0.1-4.0, 0.1-3.0, 0.2-5.0, 0.2-4.0, 0.2-3.0, 0.3-5.0, 0.3-4.0 or 0.3-3.0 weight %, as calculated based on their oxide benchmark (i.e. hafnium oxide), and as measured relative to the mass of the USY zeolite component after the framework modification. Adding hafnium compounds in an amount less than about 0.1 weight % cannot improve the solid acid properties of zeolite. Adding hafnium compounds in an amount exceeding 5 weight % tends to cause the pores of zeolite to be blocked. An aqueous solution of a hafnium compound prepared by dissolving the hafnium compound in water may be used as the hafnium compound.
[0060] The pH of the above suspension is controlled to be about <2.0 to prevent the generation of precipitates during the mixing of the aqueous solution of the zirconium compound and / or hafnium compound and / or titanium compound with the above suspension of ultrastable Y-type zeolite.
[0061] In some embodiments, the mixing of the aqueous solution of the zirconium compound and / or the hafnium compound and / or the titanium compound with the suspension of the ultrastable Y-type zeolite is carried out by gradually adding the aqueous solution to the suspension. After the addition of the above-mentioned aqueous solution to the suspension is completed, the solution can be mixed by stirring for about 3-5 hours at, for example, room temperature (about 25-35° C.). In addition, after completing the above-mentioned mixing, the mixed solution is neutralized by adding an alkaline compound such as ammonia water, so that its pH is controlled to about 7.0-7.5, thereby obtaining the USY zeolite after the framework modification described herein.
[0062] In this regard: when only a zirconium compound (or its aqueous solution) is used as a compound (or its aqueous solution) and added to the above suspension, a framework-modified USY zeolite (Zr-USY) is formed, in which zirconium atoms replace a portion of the aluminum atoms forming the framework of the ultrastable Y-type zeolite; when only a titanium compound (or its aqueous solution) is used, a framework-modified USY zeolite (Ti-USY) is formed, in which titanium atoms replace a portion of the aluminum atoms forming the framework of the ultrastable Y-type zeolite; when only a hafnium compound (or its aqueous solution) is used, a framework-modified USY zeolite (Hf-USY) is formed, in which hafnium atoms replace a portion of the aluminum atoms forming the framework of the ultrastable Y-type zeolite; when a zirconium compound and a titanium compound (or their aqueous solution) are used, a framework-modified USY zeolite (Zr-Ti-USY) in the catalyst is formed, in which the zirconium atoms and the titanium atoms replace a part of the aluminum atoms forming the framework of the ultrastable Y-type zeolite; when a zirconium compound and a hafnium compound (or an aqueous solution thereof) are used, a framework-modified USY zeolite (Zr-Hf-USY) is formed in the catalyst, in which the zirconium atoms and the hafnium atoms replace a part of the aluminum atoms forming the framework of the ultrastable Y-type zeolite; when a hafnium compound and a titanium compound (or an aqueous solution thereof) are used, a framework-modified USY zeolite (Hf-Ti-USY) is formed in the catalyst, in which the hafnium atoms and the titanium atoms replace a part of the aluminum atoms forming the framework of the ultrastable Y-type zeolite; and when a zirconium compound, a titanium compound and a hafnium compound (or an aqueous solution thereof) are used, a framework-modified USY zeolite (Zr-Ti-Hf-USY) is formed in the catalyst, in which the zirconium atoms, the titanium atoms and the hafnium atoms replace a part of the aluminum atoms forming the framework of the ultrastable Y-type zeolite.
[0063] If desired, the resulting framework-substituted zeolite can be filtered, washed with water, and dried at about 80-180°C; the mixture can be quasi-equilibrated with steam, for example, at a temperature of about 600-800°C for about 10-20 hours.
[0064] For example, in step 10, the calcined USY(c) zeolite from step 9 is prepared for acid treatment by dispersing it in water at an effective temperature in the range of, for example, about 15-95, 15-80, 20-95, 20-90, 20-80, 40-95, 40-90 or 40-80° C. to form a suspension of USY(c) at an effective concentration, for example, in the range of a liquid / solid mass ratio of about 5:1-15:1, 5:1-12:1, 8:1-15:1 or 8:1-12:1.
[0065] In the acid treatment step 11, an effective amount of an inorganic acid or an organic acid is dispersed in the suspension so that the pH of the suspension is maintained in a strongly acidic range to prepare a zeolite for inserting a metal in the framework (step 12). In some embodiments, this can be performed stepwise as in the '036 patent family. In other embodiments, for example, as disclosed in co-owned US20210077985A1 (the entire text of which is incorporated herein by reference), acid treatment to prepare a zeolite for inserting a metal in the framework can be performed together with metal insertion.
[0066] The inorganic acid used can generally be sulfuric acid, nitric acid, hydrochloric acid, etc. In some embodiments, the selected inorganic acid is sulfuric acid or hydrochloric acid. In addition, carboxylic acid can be suitably used as the above-mentioned organic acid. The amount of the inorganic acid or organic acid added is an amount suitable for controlling the pH of the suspension within the strongly acidic range (e.g., in the range of about 0.7-2.5, 0.7-2.0, 1.0-2.5 or 1.0-2.0). The acidic suspension is maintained at an effective temperature, for example, in the range of about 15-80, 15-60, 15-35, 15-30 or 20-60 ° C, and maintains an effective residence time, and maintains an effective residence time, for example, in the range of about 10-600, 10-180, 30-600 or 30-180 minutes.
[0067] In the metal insertion step 12, framework substitution is performed. The acid-modified USY (c) zeolite suspension is subjected to metal treatment to replace some of the aluminum atoms that form the framework of the ultrastable Y-type zeolite. In some embodiments, this is performed by adding a solution containing a transition metal compound to the acid-modified USY (c). In some embodiments, the transition metal compound comprises a zirconium compound and / or a titanium compound and / or a hafnium compound. The solution is maintained at an effective temperature, such as 15-80, 15-60, 15-35, 15-30, 20-60, 15-35 or 15-30° C., and an effective residence time, such as in the range of about 10-600, 10-180, 30-600 or 30-180 minutes. The suspension from step 12 can be neutralized to a pH in the range of about 7.0-7.5 with, for example, aqueous ammonia.
[0068] The solid obtained from the metal insertion step 12 can be filtered, washed with water at an effective temperature in the range of, for example, about 15-95, 15-80, 20-95, 20-90, 20-80, 40-95, 40-90 or 40-80°C, and dried, for example, at an effective temperature in the range of about 80-180 or 100-180°C, for example, at an effective residence time in the range of about 30-1800, 60-1800, 30-600 or 60-600 minutes, and the framework-modified USY zeolite (USYA) is recovered in step 13.
[0069] Ultrastable Y-type zeolite is used as a raw material for preparing a framework-modified USY zeolite (referred to as USY(c) above). As noted above, one or more of steps 1-9 may be used to prepare the USY introduced in step 10 or otherwise obtained. The USY introduced in step 10 generally has the properties of a known USY zeolite, which may be synthesized or modified (as in one or more of steps 1-9 or an alternative method) or sourced, so as to provide a USY zeolite having a SAR in the range of about 30-100, 40-100, 30-80 or 40-80 for efficient metal insertion.
[0070] The known USY type zeolite refers to the following zeolite: the unit cell size (UD) is generally in the range of about 2.425-2.450 or 2.430-2.450 nm; the specific surface area is generally in the range of about 600-900, 600-800, 650-900 or 650-800 m 2 / g range; and a pore volume of about 0.3-0.75, 0.4-0.75, 0.3-0.6 or 0.4-0.6 ml / g. Known USY-type zeolites also generally have a SAR in the range of about 5-100, 10-100, 20-100, 5-80, 10-80, 20-80, 25-100 or 25-80; as noted herein, the SAR can be selected or modified to provide an effective USY for metal insertion.
[0071] For example, a suitable zeolite is the FAU framework (zeolite Y), which has pores formed by 12-membered rings when viewed along the
[111] direction. UD (also known as lattice constant) can be measured with reference to ASTM method D3942A (Standard Test Method for Determination of the Unit Cell Dimension of a Faujasite-Type Zeolite). The specific surface area is a value determined by the BET (Brunauer-Emmett-Teller) method using nitrogen adsorption. The ultrastable Y-type zeolite can be prepared by any method known in the art. The ultrastable Y-type zeolite is subjected to a framework modification as described herein to form a framework-modified USY zeolite for producing composite catalyst particles.
[0072] The USY zeolite after framework modification has one or more of zirconium, titanium and hafnium incorporated into its framework. The effective concentration of Zr, Ti, and / or Hf includes about 0.1-5.0, 0.1-4.0, 0.1-3.0, 0.2-5.0, 0.2-4.0, 0.2-3.0, 0.3-5.0, 0.3-4.0 or 0.3-3.0 weight %, as calculated based on their oxide basis (i.e., ZrO2, TiO2 and / or HfO2), and as measured relative to the mass of the USY zeolite after the framework modification. In some embodiments, the amount of each material supplying Zr, Ti and / or Hf may be less than 0.1, 0.2 or 0.3 weight %, but when combined, the total amount is at least 0.1, 0.2 or 0.3 weight %. It should be understood by those skilled in the art that when the framework-substituted zeolite in the catalyst contains the above-mentioned zirconium atoms and titanium atoms and / or hafnium atoms, the mass ratio of zirconium atoms to titanium atoms and / or hafnium atoms (in terms of oxides) is not particularly limited, and any ratio of zirconium or titanium or hafnium that is effective for the intended use of the catalyst particles can be used, for example, in the hydrocracking of heavy hydrocarbon oils.
[0073] In some embodiments, the USY zeolite after framework modification is:
[0074] A framework-substituted zeolite in which only a portion of the aluminum atoms forming the zeolite framework are replaced by zirconium atoms, and is referred to as a "zirconium-substituted zeolite" or "Zr-USY";
[0075] A framework-substituted zeolite in which only a portion of the aluminum atoms forming the zeolite framework are replaced by titanium atoms, and is referred to as a "titanium-substituted zeolite" or "Ti-USY";
[0076] A framework-substituted zeolite in which a portion of the aluminum atoms forming the zeolite framework are replaced only with hafnium atoms, and is referred to as a "hafnium-substituted zeolite" or "Hf-USY";
[0077] Framework-substituted zeolites in which a portion of the aluminum atoms forming the zeolite framework are replaced only by zirconium atoms and titanium atoms, and are referred to as "zirconium-titanium substituted zeolites" or "Zr-Ti-USY");
[0078] Framework-substituted zeolites in which a portion of the aluminum atoms forming the zeolite framework are replaced only by hafnium atoms and titanium atoms, and are referred to as "hafnium-titanium substituted zeolites" or "Hf-Ti-USY");
[0079] Framework-substituted zeolites in which a portion of the aluminum atoms forming the zeolite framework are replaced only with zirconium atoms and hafnium atoms, and are referred to as "zirconium-hafnium substituted zeolites" or "Zr-Hf-USY"); and
[0080] A framework-substituted zeolite in which a part of the aluminum atoms forming the zeolite framework is substituted only with zirconium atoms, titanium and hafnium atoms, and is referred to as a "zirconium-titanium-hafnium substituted zeolite" or "Zr-Ti-Hf-USY".
[0081] The presence of zirconium atoms and / or titanium and / or hafnium atoms replacing aluminum atoms in the framework-modified USY zeolite serves as a component of the USY zeolite framework. The substitution can be confirmed by, for example, X-ray fluorescence, high-frequency plasma emission spectroscopy, atomic absorption spectroscopy, ultraviolet-visible-near infrared spectrophotometry (UV-Vis-NIR), Fourier transform infrared spectroscopy (FT-IR), and / or nuclear magnetic resonance spectroscopy (NMR).
[0082] Subsequent steps (steps 14 and 15) in the process for producing catalyst particles having active metal components on a composite support including a USY zeolite after framework modification and a binder include forming an inorganic oxide as a binder or granulating agent, which is then combined with the USY zeolite after framework modification and extruded (steps 16 and 17). In step 14, a solution is prepared that will precipitate into one or more inorganic oxides (hereinafter referred to as inorganic oxide components) used as a binder or granulating agent. For example, a suitable binder can be prepared from a gel of alumina or another inorganic oxide as known in the art. In some embodiments, a solid inorganic oxide can be used directly as a binder material.
[0083] Alternatively, a commercially available inorganic oxide component as known to those skilled in the art may be provided and prepared for mixing with the framework-modified USY zeolite, for example by kneading.
[0084] As the inorganic oxide, the porous inorganic oxide used in hydrocracking or other catalyst compositions in the related art can be used. Examples thereof include alumina, silica, titania, silica-alumina, alumina-titania, alumina-zirconia, alumina-boria, phosphorus-alumina, silica-alumina-boria, phosphorus-alumina-boria, phosphorus-alumina-silica, silica-alumina-titania, and silica-alumina-zirconia.
[0085] The USY zeolite after framework modification is combined with an inorganic binder to form a catalyst support material using known methods for shaping the catalyst, such as by mixing and kneading the components (step 16), and then by coextrusion or other means of shaping the composite support particles to form them into a desired shape (step 17). The composite support particles are calcined (step 18), and the active metal component is impregnated in the calcined composite support particles (step 19). The catalyst particles thus formed are then calcined again (step 20), and the final product, the catalyst particles with the active metal component on the composite support, is collected. In some embodiments, in addition to the impregnated active metal component of the catalyst particles, the USY zeolite material after framework modification in the final particles also serves as an active catalytic material.
[0086] The composite support material is formed from a framework-modified USY zeolite material, such as from step 13 herein, one or more inorganic oxide components (such as from step 15 herein), and optionally one or more other zeolite materials. The composite support material generally has a molecular weight of about 150-500, 150-450, 200-500, 200-450 or 300-450 m 2 The present invention relates to a catalyst particle having a surface area within the range of about 0.4-0.8, 0.4-0.75, 0.4-0.65, 0.45-0.8, 0.45-0.75 or 0.45-0.65 ml / g. The content of the USY zeolite component, the inorganic oxide component and the active metal component after the framework modification is appropriately determined according to the purpose. For example, the USY zeolite content after the framework modification of the catalyst particles formed with the composite support material can be within the range of about 0.1-99, 0.1-90, 0.1-80, 0.1-70, 2-99, 2-90, 2-80, 2-70, 20-100, 20-90, 20-80 or 20-70 weight %, and the remaining content is the inorganic oxide and the active metal component, and in some embodiments, optionally one or more other zeolite materials.
[0087] In the mixing / kneading step 16, the framework-modified USY zeolite (e.g., recovered from step 13 or otherwise provided) and the inorganic binder (e.g., recovered from step 15 or otherwise provided) are mixed together. The mixing is carried out in the effective ratio as indicated above and at a suitable temperature in the range of, for example, about 15-80, 15-60, 15-35, 15-30 or 20-60° C. The mixture is kneaded / milled together with an effective amount of water, for example, in a liquid / solid mass ratio range of about 30-80, for example, an effective kneading / milling time in the range of about 10-180 minutes. Thus, the kneading / milling of the wet solid material forms a dough-like mass, which is subsequently shaped and dried. The kneaded / milled product may be subjected to a heat treatment so as to obtain a closer contact between the components and better uniformity through heat diffusion and solid-state reactions.
[0088] The kneaded / ground material thus obtained is passed through a die having an effective cross-sectional shape and size and extruded at a suitable temperature in the range of, for example, about 15-80, 15-60, 15-35, 15-30 or 20-60° C. (forming step 17). Effective cross-sectional shapes include, for example, cylindrical, trilobal, twisted trilobal, or quadrilobal. Effective cross-sectional dimensions include, for example, diameters or effective diameters in the range of about 0.8-3 or 0.8-2.5 millimeters. The resulting extrudate is dried at an effective temperature in the range of, for example, about 80-180 or 100-180° C., for example, an effective residence time in the range of about 30-1800, 60-1800, 30-600 or 60-600 minutes to recover a dried composite extrudate. Optionally, a separate drying step can be avoided, whereby the composite extrudate is sent to a heat treatment step 18 for calcination.
[0089] In the heat treatment step 18, the composite extrudate (optionally dried) is subjected to a heat treatment to produce calcined composite particles. In some embodiments, the heat treatment in step 18 includes calcining the composite extrudate (optionally dried) at an effective temperature in the range of, for example, about 400-800, 400-700, 400-650, 500-800, 500-700, 500-650, 550-800, 550-700, 550-650, 600-800, or 600-700° C. (typically in the presence of air or oxygen, or in the presence of steam), and for a time in the range of about 10-600, 10-180, 30-600, or 30-180 minutes to recover the calcined composite particles.
[0090] The final product (calcined composite catalyst particles) has an active metal component impregnated therein, such as a hydrogenation metal. The active metal component may include one or more metals or metal compounds (oxides or sulfides) known in the hydrocracking field, including those selected from the periodic table IUPAC 6th, 7th, 8th, 9th and 10th families. In some embodiments, the active metal component includes those that are effectively used as hydrocracking catalysts, such as one or more of Mo, W, Co or Ni (oxides or sulfides). In some embodiments, the active metal component includes those that are effectively used as hydrogenation and / or reforming catalysts (typically in sulfur-free environments), such as one or more noble metals, such as Pt, Pd, Rh, Re, Ir or such a combination of noble metals. The metal component can be included in the catalyst at an effective concentration. For example, the total active metal content in the hydrocracking catalyst can exist as known in the relevant art, such as with respect to metals, oxides or sulfides, about 0.01 to 40 mass %. In the case of non-precious metals including Mo, W, Co, Ni, or combinations thereof, the effective total active metal content may be about 0.1 to 40 mass %, or 3 to 40 mass %, based on the mass of the catalyst, in terms of oxides or sulfides. In the case of precious metals, typically in a sulfur-free environment for hydrogenation and / or reforming, the effective total active metal content may be about 0.01 to 2 mass %, in terms of metals.
[0091] In the active metal component impregnation step 19 in the embodiment of FIG. 3 , the active metal component is impregnated. Multiple methods can be used to add one or more active metal components to the carrier, including but not limited to immersion, initial wetness method and evaporation. In the most commonly used method, the calcined carrier is immersed in an excess of an aqueous solution containing an active metal or metal compound. The solution fills the pores and is also adsorbed on the surface of the carrier, and the excess solution is removed. In another method, the initial wetness method is used to impregnate the carrier by rolling or spraying the activated carrier with a certain volume of solution, and the metal compound concentration of the solution is customized to achieve the target metal level. In another evaporative impregnation method, the carrier is saturated with water or an acid solution and immersed in an aqueous solution containing a metal compound. The compound is then diffused into the pores of the carrier through the aqueous phase. The metal-loaded carrier is then dried and calcined to form a metal oxide.
[0092] In some embodiments, the active metal component impregnation step 19 comprises immersing the calcined composite support particles formed by the framework-modified USY zeolite and the binder in an aqueous solution containing the active metal component. The amount and concentration of the aqueous solution containing the active metal component depends on the desired amount of the active metal component to be loaded on the composite support particles. In some embodiments of the above method, the volume of the active metal solution is equal to or slightly less than the pore volume of the support. The solution is maintained at an effective temperature, such as about 40-100, 40-99, 60-100, 60-99, 60-97, 70-99, 70-97, 80-99, 80-97, or 90-99° C., and for an effective residence time, such as in the range of about 40-1200, 40-600, 40-360, 60-1200, 60-600, 60-360, 120-1200, 120-600, 120-360, 180-1200, 180-600, 180-360, or 240-360 minutes.
[0093] The resulting solid can be filtered and dried, for example, at an effective temperature in the range of about 80-180 or 100-180° C., for example, at an effective residence time in the range of about 30-1800, 60-1800, 30-600 or 60-600 minutes, to recover composite support particles formed by the framework-modified USY zeolite and the binder, which are loaded with active metals on the composite material. Optionally, a separate drying step can be avoided, thereby sending the composite material with active metals to the heat treatment step 20 for calcination.
[0094] In the heat treatment step 20, the supported composite material is subjected to heat treatment to prepare calcined composite particles having active metals on the composite material. In some embodiments, the heat treatment of step 20 includes, for example, calcining at an effective temperature in the range of about 400-800, 500-800, 500-700, 500-650, 550-800, 550-700, 550-650, 600-800, or 600-700° C., and for a time in the range of about 10-600, 10-180, 30-600, or 30-180 minutes to recover calcined composite particles having active metals on the composite material. In some embodiments, calcination occurs in the presence of air.
[0095] In step 21, the final catalyst product is recovered. In embodiments where the catalyst is a hydrocracking catalyst, a hydrogenation catalyst, or a reforming catalyst, the composite support material having the active metal supported therein generally has a carbon content of about 150-500, 150-450, 200-500, 200-450, or 300-450 m 2 / g range, and a pore volume in the range of about 0.4-1.0, 0.4-0.8, 0.4-0.75, 0.4-0.65, 0.45-1.0, 0.45-0.8, 0.45-0.75, or 0.45-0.65 ml / g.
[0096] refer to Figure 4-7 , provide embodiments for producing catalyst particles with active metals, wherein all or a portion of the metal loading occurs prior to shaping the composite catalyst particles. This provides flexibility to the catalyst manufacturer, as will be apparent herein.
[0097] In the description herein, "active metal component" is different and independent from the metal that replaces the aluminum atoms in the USY zeolite framework, and specifically refers to one or more metals or gold compounds (oxides or sulfides) impregnated in: framework-modified zeolites, binders, extrudates of framework-modified zeolites and binders, calcined extrudates of framework-modified zeolites and binders, and combinations thereof.
[0098] While not wishing to be bound by theory, it is understood that by controlling the metal loading, pore blocking is minimized by using wet USYA. If the pores of the zeolite are saturated with water, a smaller amount of metal can diffuse into the pores from the metal solution in a given period of time than if the metal solution is added to the same zeolite in a dry state.
[0099] In the embodiments described herein, the ratio of the USY zeolite component after framework modification to the inorganic oxide binder component is appropriately determined according to the purpose of the catalyst. For example, the USY zeolite content after framework modification of the catalyst particles formed with the composite support material may be in the range of about 0.1-99, 0.1-90, 0.1-80, 0.1-70, 2-99, 2-90, 2-80, 2-70, 20-100, 20-90, 20-80 or 20-70 weight %, and the remaining content is the inorganic oxide binder, and in some embodiments, optionally one or more other zeolite materials.
[0100] In one embodiment, a method for producing catalyst particles is provided, wherein the catalyst particles are formed from a composite of a granulating agent or binder material (e.g., an inorganic oxide) and a framework-substituted USY zeolite material (USYA), wherein some of the aluminum atoms in the framework are replaced by zirconium atoms and / or titanium atoms and / or hafnium atoms, and wherein the USYA contains an active metal impregnated therein (sometimes referred to herein as USYA(m)). In other descriptions of this embodiment, the catalyst particles of this embodiment are referred to as calcined extrudates formed from a composite of USYA(m) and a binder.
[0101] Figure 4 The process steps for producing the composite catalyst of a binder and USYA(m) according to this embodiment are shown, wherein the USYA includes an active metal (USYA(m)) impregnated therein.
[0102] In one embodiment of the preparation method, a framework-modified USY zeolite is prepared or provided, and then one or more active metal components are added to the surface of the framework-modified USY zeolite, including the surface of the inner wall of the pores. The metal-impregnated framework-modified USY zeolite (wet, dry or calcined) and the binder are mixed, kneaded, extruded and calcined to form catalyst particles containing active metals. Steps 19 and 20 of the process from Figure 3 are thus eliminated.
[0103] In the process description of this embodiment, it is understood that the following framework-substituted USY zeolite material (before metal loading) and binder material can be provided by any suitable source (including as described above in conjunction with FIG. 3) or by another source. Steps corresponding to those in FIG. 3 that are considered optional in some embodiments herein are Figure 4 The process is shown in dashed lines in FIG3 and can be performed as described with respect to FIG3. Both the USY zeolite and the inorganic oxide material are characterized by external and internal pore wall surfaces. Figure 4 In the embodiment of the present invention, in step 44, the active metal is attached to the outer surface and the inner pore wall surface of the USY zeolite.
[0104] In some embodiments, the process begins by providing a framework-substituted USY zeolite material USYA at step 43. The framework-modified USY zeolite incorporates one or more of zirconium, titanium and / or hafnium into its framework at an effective concentration of about 0.1-5.0, 0.1-4.0, 0.1-3.0, 0.2-5.0, 0.2-4.0, 0.2-3.0, 0.3-5.0, 0.3-4.0 or 0.3-3.0 wt %, as calculated on their oxide basis (i.e., ZrO2, TiO2 and / or HfO2) and as measured relative to the mass of the framework-modified USY zeolite; in some embodiments, the amount of each material supplying Zr, Ti and / or Hf may be less than 0.1, 0.2 or 0.3 wt %, but when combined, the total amount is at least 0.1, 0.2 or 0.3 wt %.
[0105] In some embodiments, the framework-substituted USY zeolite component is provided in a "wet" state, whereby the solid material from the framework substitution step (step 12) is filtered / washed and provided in a wet state, whereby the drying step typically utilized is not performed (performed to a lesser extent) so that water remains entrained in the solid. In some embodiments, the framework-substituted USY zeolite component is provided in a "dry" state, whereby the solid material from the framework substitution step (step 12) is filtered and dried, but is provided in an uncalcined state, whereby the heat treatment step typically utilized to calcine the material is not performed. In some embodiments, the framework-substituted USY zeolite component is provided in a "dry" state, whereby the solid material from the framework substitution step (step 12) is filtered, dried and calcined. Therefore, in Figure 4 In some embodiments, the USYA of step 43 is provided as a wet, dry (uncalcined) or calcined zeolite material.
[0106] In step 44, USYA as a wet, dry (uncalcined) or calcined zeolite material is impregnated with one or more active metal components, such as hydrogenation-active metal components, to produce USYA (m). The active metal component may include one or more metals or metal compounds (oxides or sulfides) known in the field of hydrocracking, including those selected from the 6th, 7th, 8th, 9th and 10th groups of the periodic table IUPAC. In some embodiments, the active metal component is one or more of Mo, W, Co or Ni (oxide or sulfide). In some embodiments, typically in a sulfur-free environment, the active metal component includes those that are effective as hydrogenation and / or reforming catalysts, such as one or more precious metals Pt, Pd, Rh, Re, Ir, or a combination of such precious metals.
[0107] The active metal component may be included in the USYA(m) zeolite material at an effective concentration to provide an effective overall active metal content in the composite catalyst of the binder and USYA(m). Figure 4 The catalyst for hydrocracking (e.g., hydrocracking of heavy hydrocarbon oil) produced by the embodiment of the present invention may contain about 0.01 to 40% by mass of one or more active metal components, relative to the total mass of the composite catalyst material, which is similar to the range used in conventional hydrocracking catalysts. In the case of non-precious metals including Mo, W, Co, Ni or a combination thereof, in terms of oxides or sulfides, the effective total active metal content may be about 0.1 to 40% by mass, or 3 to 40% by mass, based on the mass of the catalyst. In the case of precious metals, typically in a sulfur-free environment for hydrogenation and / or reforming, in terms of metals, the effective total active metal content may be about 0.01 to 2% by mass.
[0108] exist Figure 4In the active metal component impregnation step 44 in the embodiment of the present invention, an effective amount of one or more active metal components is impregnated into the wet, dry (uncalcined) or calcined USYA zeolite as the support component. In this embodiment, the active metal components of the final catalyst particles are provided only in the USYA zeolite, and therefore, the effective amount covers the total active metal content of the catalyst particles, for example, within the range as indicated above.
[0109] In some embodiments of the active metal component impregnation step 44, two or more active metal components are impregnated into wet, dry (uncalcined), or calcined USYA zeolite as a support component, whereby one or more active metal components act as promoters for one or more other active metal components.
[0110] As the active metal component impregnation step 44, one or more active metal components may be added to the USYA zeolite support using a variety of methods including, but not limited to, impregnation, incipient wetness and evaporation, or any other suitable method.
[0111] In some embodiments of the active metal component impregnation step 44, an effective amount of wet, dry (uncalcined) or calcined USYA zeolite support material is impregnated with an excess of a solution containing an active metal or metal compound. The solution fills the pores and also adsorbs on the support surface, and the excess solution is removed to recover the metal-loaded USYA zeolite support, wet USYA (m).
[0112] In another method, the active metal component impregnation step 44 is performed using the incipient wetness method by tumbling or spraying an effective amount of wet, dry (uncalcined) or calcined USYA zeolite support material with a volume of solution having a metal compound concentration tailored to achieve the target metal level. The metal loaded USYA support - wet USYA (m) is recovered.
[0113] In another method, the active metal component impregnation step 44 is carried out by evaporative impregnation, wherein an effective amount of wet, dry (uncalcined) or calcined USYA zeolite support material is saturated with water or an acid solution and immersed in an aqueous solution containing a metal compound. The compound is then diffused into the pores of the support through the aqueous phase. The metal-loaded USYA support, wet USYA (m), is collected. In some embodiments, the wet USYA (m) collected in this way is then dried and calcined.
[0114] In the active metal component impregnation step 44, the amount and concentration of the aqueous solution containing the active metal component depends on the desired amount of active metal component to be loaded on the composite support particles. In some embodiments of the above method, the volume of the active metal solution is equal to or slightly less than the pore volume of the USYA support. The solution is maintained at an effective temperature, e.g., about 40-100, 40-99, 60-100, 60-99, 60-97, 70-99, 70-97, 80-99, 80-97, or 90-99° C., and an effective residence time, e.g., in the range of about 40-1200, 40-600, 40-360, 60-1200, 60-600, 60-360, 120-1200, 120-600, 120-360, 180-1200, 180-600, 180-360, or 240-360 minutes.
[0115] In some embodiments of the active metal component impregnation step 44, when wet, dry (uncalcined) or calcined USYA zeolite is used, the metal loading can be obtained by loading up to the available pore volume of the USYA zeolite with a metal solution of appropriate concentration. In further embodiments of the active metal component impregnation step 44, a smaller amount is used to control the metal loading. For example, the effective volume of the loaded metal solution can be, for example, in the range of about 1-100, 1-99, 1-90, 20-100, 20-99, or 20-90 volume % relative to the total pore volume of the USYA zeolite material.
[0116] In a further embodiment of the active metal component impregnation step 44, a wet USYA zeolite material is used. The wet USYA contains water in all or part of the pore volume, for example, in the range of about 1-100, 1-99, 1-90, 50-100, 50-99, or 50-90 volume % relative to the total pore volume. The volume can be controlled by partially drying the material to change the humidity. The metal solution - whether provided by immersion, initial wetness or evaporative impregnation - is completely or partially blocked outside the saturated pores, and therefore the metal diffuses less into the pores. Therefore, the metal can be mainly located at the outer surface of the zeolite, with a limited amount in the pores.
[0117] The solid obtained in the active metal component impregnation step 44 can be filtered and dried at an effective temperature in the range of, for example, about 80-180 or 100-180° C., for example, an effective residence time in the range of about 30-1800, 60-1800, 30-600 or 60-600 minutes to recover dry USYA (m). Optionally, a separate drying step can be avoided, thereby subjecting the composite material with active metals to heat treatment for calcination as part of the active metal component impregnation step 44. In the heat treatment, dry or wet USYA (m) is subjected to heat treatment to prepare calcined USYA (m). In some embodiments, the heat treatment comprises calcining at an effective temperature in the range of, for example, about 400-800, 400-700, 400-650, 500-800, 500-700, 500-650, 550-800, 550-700, 550-650, 600-800, or 600-700° C., and for a time in the range of about 10-600, 10-180, 30-600, or 30-180 minutes to recover calcined USYA (m). In some embodiments, calcination occurs in the presence of air.
[0118] The metal-loaded USYA(m) zeolite material from step 44 is combined with a binder material in a wet, dry (uncalcined) or calcined state (as shown in the mixing / kneading step 46), and formed into composite catalyst particles (as shown in the forming step 47). The composite catalyst particles are calcined (as shown in the heat treatment step 48), and the final product, calcined catalyst particles, are recovered (as shown in step 51).
[0119] For example, the binder material can be prepared as shown and described herein about steps 14 and 15 in Fig. 3, or a commercially available inorganic oxide component can be provided, as known to those skilled in the art. As inorganic oxide, porous inorganic oxide used in hydrocracking or other catalyst compositions in related fields can be used. Examples thereof include aluminum oxide, silicon dioxide, titanium dioxide, silicon dioxide-alumina, aluminum oxide-titania, aluminum oxide-zirconium oxide, aluminum oxide-borium oxide, phosphorus-alumina, silicon dioxide-alumina-borium oxide, phosphorus-alumina-borium oxide, phosphorus-alumina-silicon dioxide, silicon dioxide-alumina-titania and silicon dioxide-alumina-zirconium oxide.
[0120] As about Figure 4The steps 46, 47, 48 and 51 shown and described can be performed as described above with respect to steps 16, 17, 18 and 21 in Figure 3, respectively. As noted above, steps 19 and 20 from the process of Figure 3 are thereby eliminated. Thus, the final composite catalyst particles are composites of USYA(m) and an inorganic oxide used as a binder.
[0121] The final composite catalyst particles are calcined extrudates formed from a composite of USYA(m) and a binder, which generally have surface area and pore volume levels within the range of catalysts formed in conventional processes, for example, as described with respect to step 21 in FIG. 3 .
[0122] In another embodiment, a method for producing catalyst particles is provided, wherein the catalyst particles are formed from a composite of a granulating agent or binder material (e.g., an inorganic oxide containing an active metal impregnated therein) and a framework-substituted USY zeolite material (USYA), wherein some of the aluminum atoms in the framework are replaced by zirconium atoms and / or titanium atoms and / or hafnium atoms, and wherein USYA contains an active metal impregnated therein (USYA(m)). In other descriptions of this embodiment, the catalyst particles of this embodiment are referred to as calcined extrudates formed from a composite of USYA(m) and a metal-loaded binder support component.
[0123] Figure 5 The process steps for producing the composite catalyst of the metal-loaded binder and USYA(m) according to this embodiment are shown, wherein the USYA comprises an active metal impregnated therein (USYA(m)), and wherein the inorganic oxide material comprises an active metal impregnated therein. For example, this method is particularly applicable when a limited amount of zeolite is used in the catalyst formulation.
[0124] In one embodiment of the preparation method, a USY zeolite modified by a framework is prepared or provided, and the first part of the total active metal component content is added to the surface of the USY zeolite modified by the framework, including on the surface of the inner wall of the hole. The second part of the total active metal component content (as the remainder in some embodiments) is added to the inorganic oxide binder. The metal-impregnated framework-modified USY zeolite (wet, dry or calcined) and the metal-impregnated inorganic oxide binder are mixed and kneaded, extruded and calcined in a desired ratio to form a composite catalyst particle containing active metal of the first component of the USY zeolite replaced by the framework with a loaded metal and the second component of the inorganic oxide binder of the loaded metal. Steps 19 and 20 of the process from Figure 3 are thus eliminated.
[0125] In step 43, the framework-substituted USY zeolite material USYA is provided as a wet, dry (uncalcined) or calcined zeolite material, as described herein with respect to Figure 4 In the process description of this embodiment, it is understood that the following framework-substituted USY zeolite material (before metal loading) and binder material (before metal loading) can be provided by any suitable source (including as described above in conjunction with FIG. 3) or by another source. In some embodiments herein, steps corresponding to those in FIG. 3 are considered optional. Figure 5 The process is shown in dashed lines in FIG3 and can be performed as described with respect to FIG3. Both the USY zeolite and the inorganic oxide material are characterized by external and internal pore wall surfaces. Figure 5 In an embodiment of the present invention, at step 54, the active metal is attached to the outer surface and inner pore wall surface of the USY zeolite, and at step 65, the additional active metal is attached to the outer surface and inner pore wall surface of the inorganic oxide binder.
[0126] In step 54, a framework-substituted USY zeolite material USYA is prepared to form USYA(m), as described above with respect to Figure 4 In step 65, a metal-loaded binder material is prepared, as described above with respect to Figure 4 In step 54, an effective amount of active metal component is added to USYA, for example, such that a first portion of about 0.1-99, 0.1-90, 0.1-70, 0.1-60, 1-99, 1-99, 1-90, 1-70, 1-60, 1-99, 5-90, 5-70, 5-60, 20-99, 20-90, 20-70, 20-60, 40-99, 40-90, 40-70, or 40-60 mass % of the total active metal component content contained in the final composite catalyst particles is in USYA (m), and the remainder of the total active metal is constituted by the second portion of the active metal component content in the metal-loaded binder.
[0127] All or a portion of the binder material used in the final catalyst particles is impregnated with an effective amount of active metal component in step 65. The effective amount of active metal component in step 65 is generally the second portion, which may constitute the remainder of the total active metal component content contained in the final composite catalyst particles relative to the first portion contained in USYA(m). In some embodiments, the second portion is less than the remainder of the total active metal component content contained in the final composite catalyst particle, relative to the first portion contained in USYA(m), wherein the third and optionally the fourth portion, based on the one or more active metal components added, is included in the particle: after mixing USYA(m) and the metal-loaded binder together (as described in co-pending U.S. patent application serial number 17 / 577,794, entitled “Catalysts With Modified Active Phase Dispersion And Method To Prepare Catalysts With Modified Active Phase Dispersion,” filed on January 18, 2022, the entirety of which is incorporated herein by reference); and / or after extrudate shaping (e.g., as discussed herein with respect to step 19 in the process described with respect to FIG. 3, and as described in the '036 patent family).
[0128] The metal-loaded USYA(m) zeolite material from step 54 is combined with the metal-loaded binder support component from step 65 in a wet, dry (uncalcined) or calcined state (as shown by mixing / kneading step 46), and formed into composite catalyst particles (as shown by forming step 47). The composite catalyst particles are calcined (as shown by heat treatment step 48), and the final product, calcined catalyst particles, are recovered (as shown by step 51). Figure 5 Steps 46, 47, 48 and 51 shown and described may be performed as described above with respect to steps 16, 17, 18 and 21, respectively, in Figure 3. As noted above, steps 19 and 20 from the process of Figure 3 are thus eliminated in some embodiments, and the final composite catalyst particles are composites of USYA(m) and a metal-loaded binder support component that are coextruded and formed into catalyst particles.
[0129] The final composite catalyst particles are a composite of USYA(m) and a metal-loaded binder carrier component that are mixed, coextruded and formed into particles that generally have surface area and pore volume levels within the range of catalysts formed in conventional processes, for example, as described with respect to step 21 in FIG. 3 .
[0130] In a further embodiment, a method for producing catalyst particles is provided, wherein the catalyst particles are formed from a composite of a granulating agent or binder material (e.g., an inorganic oxide) and a framework-substituted USY zeolite material (USYA), wherein some of the aluminum atoms in the framework are replaced by zirconium atoms and / or titanium atoms and / or hafnium atoms, and wherein the USYA contains an active metal impregnated therein (USYA(m)), and further, wherein the additional active metal is impregnated in an extrudate formed by USYA(m) and the binder. In other descriptions of this embodiment, the catalyst particles of this embodiment are referred to as calcined metal-loaded extrudates, wherein the extrudates are formed from a composite of a binder and USYA(m).
[0131] Figure 6 The process steps for producing the composite catalyst of binder and USYA(m) are shown, wherein the additional active metal is impregnated in the extrudate. This method is particularly applicable, for example, when a limited amount of zeolite is used in the catalyst formulation.
[0132] In one embodiment of the preparation method, a USY zeolite modified by a framework is prepared or provided, and a first portion of the total active metal component is added to the zeolite surface, including on the inner wall surface of the pore. The metal-impregnated USY zeolite modified by a framework (wet, dry or calcined) is mixed, kneaded, extruded and calcined with an inorganic oxide as a binder in a desired ratio to form catalyst particles containing active metals with a portion of active metals in the USY zeolite component modified by a framework. After the catalyst particles are formed with a binder, the second portion of the total active metal component content (as the remainder in some embodiments) is added to the extrudate, and the composite catalyst particles of the metal-loaded USY zeolite component modified by a framework with a metal-loaded metal are calcined to form a final product.
[0133] In step 43, the framework-substituted USY zeolite material USYA is provided as a wet, dry (uncalcined) or calcined zeolite material, as described herein with respect to Figure 4 In the process description of this embodiment, it is understood that the following framework-substituted USY zeolite material (before metal loading) and binder material can be provided by any suitable source (including as described above in conjunction with FIG. 3) or by another source. In some embodiments herein, steps corresponding to those in FIG. 3 are considered optional. Figure 6 The process is shown in dashed lines in FIG. 3 and can be performed as described with respect to FIG. 3. Both the USY zeolite and the inorganic oxide material are characterized by an outer surface and an inner pore wall surface. In addition, the shaped extrudate is characterized by an outer surface and an inner pore wall surface. Figure 6In an embodiment of the present invention, at step 54, the active metal is attached to the outer surface and inner pore wall surfaces of the USY zeolite, and at step 49, the additional active metal is attached to the outer surface and inner pore wall surfaces of the shaped extrudate.
[0134] In step 54, a framework-substituted USY zeolite material USYA is prepared to form USYA(m), as described above with respect to Figure 4 In step 54, an effective amount of active metal component is added to USYA, for example, such that a first portion of about 0.1-99, 0.1-90, 0.1-70, 0.1-60, 1-99, 1-99, 1-90, 1-70, 1-60, 1-99, 5-90, 5-70, 5-60, 20-99, 20-90, 20-70, 20-60, 40-99, 40-90, 40-70, or 40-60 mass % of the total active metal component content contained in the final composite catalyst particles is within USYA (m), and the remainder of the total active metal is composed of a second portion of the active metal component content added to the extrudate as a composite support in step 49 described below.
[0135] The metal-loaded USYA(m) zeolite material from step 54 is combined with a binder material in a wet, dry (uncalcined) or calcined state (as shown by mixing / kneading step 46) and formed into composite catalyst particles (as shown by forming step 47). The binder material can be prepared or provided as described herein, and except for the modification to the impregnation at step 49, the same is true with respect to Figure 6 The shown and described steps 46 , 47 , 48 , 49 , 50 , and 51 may be performed as described above with respect to steps 16 , 17 , 18 , 19 , and 21 , respectively, in FIG. 3 .
[0136] The composite catalyst particles having the first part of the active metal component in the USYA zeolite carrier component and subjected to heat treatment in step 48 are subjected to an impregnation step 49, wherein the second part of the total active metal component content is impregnated in the composite extrudate particles as a carrier. The second part is an effective amount to make up for the difference in order to obtain the required total active metal component content. In some embodiments, an effective amount of composite extrudate particles is immersed in an excess of a solution containing an active metal or a metal compound. The solution fills the pores and is also adsorbed on the surface of the carrier, and the excess solution is removed to recover the metal-loaded composite, which is a composite of the metal-loaded USYA (m) zeolite and an inorganic oxide used as a binder. The metal-loaded composite catalyst particles from step 49 are calcined (as shown in the heat treatment step 50), and the final product, calcined catalyst particles (as shown in step 51), are recovered.
[0137] One or more active metal components may be added to the composite extrusion particles (as the support from the calcination in step 48) using a variety of methods, including but not limited to impregnation, incipient wetness, and evaporation. Impregnation of the composite extrusion particles may follow the procedures used in conventional methods, such as described in conjunction with step 19 in Figure 3. The difference is that in the methods herein, this step requires only the second portion of the total active metal component content, rather than the entire active metal content as in conventional methods.
[0138] The procedures for the heat treatment step 50 may follow those used in conventional processes, such as described in conjunction with step 20 in Figure 3. At step 51, the final catalyst product is recovered.
[0139] The final composite catalyst particles are calcined metal-loaded extrudates formed from a composite of binder and USYA(m) having surface area and pore volume levels generally within the range of catalysts formed in conventional processes, e.g., as described with respect to step 21 in FIG. 3 .
[0140] In another embodiment, a method for producing catalyst particles is provided, wherein the catalyst particles are formed from a composite of a granulating agent or binder material (e.g., an inorganic oxide) and a framework-substituted USY zeolite material (USYA), wherein some of the aluminum atoms in the framework are replaced by zirconium atoms and / or titanium atoms and / or hafnium atoms. The USYA zeolite is impregnated with an active metal to form USYA(m) (step 54, as described herein), and;
[0141] (a) an inorganic oxide binder (step 55) (in the absence of metal impregnation steps 66 and 49) as described herein and in co-pending U.S. patent application Ser. No. 17 / 577,747, filed Jan. 18, 2022, entitled “Catalysts With Modified Active Phase Dispersion And Method To Prepare Catalysts With Modified Active Phase Dispersion” (the entirety of which is incorporated herein by reference);
[0142] (b) a composite of a binder and USYA(m) (step 66) (in the absence of a binder impregnation step 55 and a metal impregnation step 49), as described in co-pending U.S. patent application Ser. No. 17 / 577,794, filed on Jan. 18, 2022, entitled “Catalysts With Modified Active Phase Dispersion And Method To Prepare Catalysts With Modified Active Phase Dispersion” (the entirety of which is incorporated herein by reference); or
[0143] (c) a complex of a metal-loaded binder and USYA(m) (steps 55 and 66) (in the absence of a metal impregnation step 49), as described herein and in co-pending U.S. patent application serial number 17 / 577,747, entitled “Catalysts With ModifiedActive Phase Dispersion And Method To Prepare Catalysts With Modified ActivePhase Dispersion,” filed on January 18, 2022 (the entirety of which is incorporated herein by reference).
[0144] Alternatively, the active metal is impregnated into USYA zeolite to form USYA(m) (step 54, as described herein), and
[0145] (a) one of the following:
[0146] (a1) an inorganic oxide binder (step 55) (in the absence of a metal impregnation step 66), as described herein and in co-pending U.S. patent application Ser. No. 17 / 577,747, filed on Jan. 18, 2022, entitled “Catalysts With Modified Active Phase Dispersion And Method To Prepare Catalysts With Modified Active Phase Dispersion” (the entirety of which is incorporated herein by reference);
[0147] (a2) a complex of a binder and USYA(m) (step 66) (in the absence of a binder impregnation step 55), as described in co-pending U.S. patent application Ser. No. 17 / 577,794, filed on Jan. 18, 2022, entitled “Catalysts With Modified Active Phase Dispersion And Method To Prepare Catalysts With Modified Active Phase Dispersion” (the entirety of which is incorporated herein by reference); or
[0148] (a3) a complex of a metal-loaded binder and USYA(m) (steps 55 and 66) as described herein and in co-pending U.S. patent application Ser. No. 17 / 577,747, filed on Jan. 18, 2022, entitled “Catalysts With Modified Active Phase Dispersion And Method To Prepare Catalysts With Modified Active Phase Dispersion” (the entirety of which is incorporated herein by reference);
[0149] as well as
[0150] (b) in an extrudate intermediate catalyst particle formed from one of (a1), (a2) or (a3) above (step 49).
[0151] Figure 7The process steps for producing the composite catalyst impregnated with active metals in one or more stages are shown. The procedures for each step may follow those described herein with respect to Figures 3-6, or as described in co-pending U.S. patent application serial number 17 / 577,747, entitled "Catalysts With Modified Active Phase Dispersion And Method ToPrepare Catalysts With Modified Active Phase Dispersion", filed on January 18, 2022, and / or 17 / 577,794, entitled "Catalysts With ModifiedActive Phase Dispersion And Method To Prepare Catalysts With Modified ActivePhase Dispersion", filed on January 18, 2022 (both of which are incorporated herein by reference in their entirety).
[0152] In any of the above embodiments, for example, in the step where the framework-modified USY zeolite or metal-loaded framework-modified USY zeolite is mixed with an inorganic oxide, one or more additional zeolite components (i.e., zeolite materials other than the framework-modified USY zeolite or metal-loaded framework-modified USY zeolite) may be integrated. The additional zeolite materials may include, but are not limited to, mordenite, ZSM-5, ZSM-11, ZSM-12, ZSM-22, ZSM-23, ZSM 35, β-type, Y, and USY (wherein the USY zeolite component is different from the framework-modified USY zeolite described herein). For example, these may be (FAU) frameworks, which include micropores associated with 12-membered rings when viewed along the
[111] direction of USY; (MFI) framework, which includes micropores associated with the 10-membered ring when viewed along the
[100] and
[010] directions, respectively. and ZSM-5; (MEL) framework, which includes a micropore size associated with the 10-membered ring when viewed along the
[100] direction ZSM-11; (MTW) framework, which includes a micropore size associated with the 12-membered ring when viewed along the
[010] direction ZSM-12; (TON) framework, which includes a micropore size associated with the 10-membered ring when viewed along the
[001] direction ZSM-12; (MTT) framework, which includes a micropore size associated with the 10-membered ring when viewed along the
[001] direction ZSM-23; (FER) framework, which includes micropores associated with 10-membered rings and 8-membered rings when viewed along the
[001] and
[010] directions, respectively. and ZSM-35; (MOR) framework, which includes micropores associated with 12-membered rings and 8-membered rings when viewed along the
[001] and
[001] directions, respectively. and Mordenite; and (* BEA) framework, which includes micropores associated with 12-membered rings when viewed along the
[100] and
[001] directions, respectively. and Zeolite beta polymorph A.
[0153] Provided herein is a method for hydrocracking hydrocarbon oil, comprising hydrocracking the hydrocarbon oil using the above-mentioned hydrocracking catalyst.
[0154] In some embodiments, the method for hydrocracking hydrocarbon oil comprises filling a reactor vessel of a hydrocracking apparatus as a flow reactor with a hydrocracking catalyst, and treating, for example, a hydrocarbon oil having a boiling point in the range of about 370-816, 370-650° C.: in the presence of hydrogen, at a reactor temperature in the range of about 300-500, 330-450° C., at a hydrogen partial pressure in the range of about 4-30, 7-15 MPa, at about 0.1-10, 0.2-1.5 h -1 The liquid hourly space velocity (LHSV) in the range of about 500-2500, 1000-2000 normalized cubic meters of hydrogen per cubic meter of oil (Nm 3 / m 3 ) range.
[0155] In some embodiments, the method for hydrocracking a hydrocarbon oil comprises filling a reactor vessel of a hydrocracking apparatus as a flow reactor with a hydrocracking catalyst, and treating a hydrocarbon oil having a boiling point in the range of about 370-650° C. to obtain a kerosene-gas oil: in the presence of hydrogen, at a reactor temperature in the range of about 330-450° C., at a hydrogen partial pressure in the range of about 7-15 MPa, at a temperature of about 0.2-1.5 h -1 range of LHSV, and about 1000-2000Nm 3 / m 3 range of hydrogen / oil ratios.
[0156] In the method for hydrocracking hydrocarbon oil according to the present invention, the above-mentioned flow reactor can be a flow reactor selected from a stirred bath type reactor, a boiling bed type reactor, a slurry bath type reactor equipped with baffles, a fixed bed type reactor, a rotating tube type reactor and a slurry bed type reactor.
[0157] In the method for hydrocracking hydrocarbon oil according to the present invention, the above-mentioned hydrocarbon oil preferably contains heavy hydrocarbon oil obtained from: (1) crude oil, (2) synthetic crude oil, (3) asphalt, (4) oil sands, (5) Shell petroleum, or (6) coal liquefaction oil.
[0158] In the method for hydrocracking hydrocarbon oil according to some embodiments of the present invention, the above-mentioned hydrocarbon oil contains heavy hydrocarbon oil obtained from crude oil, synthetic crude oil, asphalt, oil sands, shell oil or coal liquefaction oil, and the above heavy hydrocarbon oil is preferably any one of the following: a) vacuum gas oil (VGO), b) deasphalted oil (DAO) or demetallized oil obtained from a solvent deasphalting process, c) light coker gas oil or heavy coker gas oil obtained from a coking process, d) cycle oil obtained from a fluid catalytic cracking (FCC) process, or e) gas oil obtained from a visbreaking process.
[0159] The hydrocarbon oil hydrocracking catalyst manufactured according to the present invention is characterized in that, in the hydrocarbon oil hydrocracking catalyst containing ultrastable Y-type zeolite, the above ultrastable Y-type zeolite is a framework-substituted zeolite, wherein a portion of the aluminum atoms constituting its framework is replaced by zirconium atoms and / or titanium and / or hafnium atoms. A hydrogenation active metal component is provided, wherein all or part of the metal loading occurs before the composite catalyst particles as described herein are formed.
[0160] Therefore, compared with a conventional hydrocracking catalyst comprising a zeolite carrier on which titanium fine particles or zirconium fine particles are carried, the hydrocracking catalyst of the present invention allows heavy hydrocarbons such as VGO, DAO, etc. to easily diffuse into its mesopores, and the cracking activity of hydrocarbon oil is enhanced so that middle distillates can be obtained in high yield. Using the hydrocracking catalyst of the present invention, the clogging of the mesopores is minimized, thereby enhancing the ability of heavy hydrocarbons to diffuse therein for catalytic reaction.
[0161] In addition, compared with those of conventional hydrocracking catalysts (comprising a hydrogenation metal component carried on a carrier comprising a framework-substituted zeolite in which a part of aluminum atoms constituting the framework of Y-type zeolite is substituted with titanium atoms), the hydrocracking catalyst of the present invention has a slightly lower hydrocarbon oil cracking activity, but the overcracking reaction of kerosene and gas oil is suppressed, so that middle distillates can be obtained in high yield. In addition, the hydrocarbon oil hydrocracking catalyst according to the present invention increases the number of active sites and thus provides high hydrocracking activity.
[0162] Example
[0163] Comparative Examples
[0164] Comparative Example provides a method of producing reference catalyst particles, which are calcined composite support particles of the framework-modified USY zeolite described herein and a binder, the composite support particles having an active metal component added to the particles, and subsequently calcined. The process is similar to that disclosed in the '036 patent family.
[0165] First, at a temperature of 60°C, 50.0 kg of SAR is 5.2, UD is 2.466 nm, SA is 720 nm 2 / g, and Na-Y zeolite with a Na2O content of 13.0% by mass was suspended in water (liquid / solid mass ratio of 12.5L water / kg zeolite). Then, 14.0kg of ammonium sulfate was added thereto. The resulting suspension was stirred at 70°C for 1 hour and filtered. The resulting solid was washed with water. Then, the solid was washed with an ammonium sulfate solution of 14.0kg of ammonium sulfate dissolved in 500L of water at a temperature of 60°C, washed with 500L of water at a temperature of 60°C, and dried at 130°C for 20 hours, thereby obtaining about 45kg of Y zeolite (NH4 65 Y), of which 65% of the sodium (Na) contained in Na-Y is mixed with ammonium ions (NH 41 ) was ion-exchanged. NH4 65 The content of Na2O in Y was 4.5 mass%. Next, 40 kg of NH4 65 Y was fired at 670°C for 1 hour in a saturated water vapor atmosphere to form hydrogen-Y zeolite (HY).
[0166] 40 kg of HY was suspended in 400 L of water at 60°C. Then, 49.0 kg of ammonium sulfate was added thereto. The resulting mixture was stirred at 90°C for 1 hour and washed with 200 L of water at 60°C. The mixture was then dried at 130°C for 20 hours, thereby obtaining about 37 kg of Y zeolite (NH4 95 Y), wherein 95% of the Na contained in the initial Na-Y was ion-exchanged with NH4. About 33 kg of the synthesized NH4 95 Y was calcined at 650°C for 1 hour in a saturated steam atmosphere, thereby obtaining about 15 kg of ultrastable Y zeolite (hereinafter also referred to as "USY(a)") having a SiO2 / Al2O3 molar ratio of 5.2 and a Na2O content of 0.6 mass%.
[0167] 40 kg of USY (a) was suspended in 400 L of 60° C. water. 25% by mass of sulfuric acid was gradually added to the suspension at 2.35 times the amount of zeolite, and stirred for one hour to dissolve the aluminum outside the framework and prepare a second USY zeolite (USY (b)). Then, the suspension was filtered, and the obtained material was washed with 20 liters of 60° C. purified water and dried at 130° C. for 20 hours to obtain a solid substance USY (b). USY (b) was fired at 600° C. for 1 hour, thereby preparing an ultrastable Y-type zeolite (USY (c)).
[0168] 1 kg of USY (c) was suspended in 10 L of 25°C water. The pH of the suspension was adjusted to 1.6 by gradually adding 25% by mass sulfuric acid. Then, 86 g of a solution containing 18% by mass zirconium sulfate and 45 g of a solution containing 33% by mass titanium sulfate were added thereto. The resulting mixture was stirred at room temperature for 3 hours. Then, the pH was adjusted to 7.2 with 15% by mass ammonia water. After stirring the mixture at room temperature for 1 hour, the mixture was filtered. The resulting solid was washed with 10 L of water and dried at 130°C for 20 hours, thereby obtaining about 1 kg of titanium-zirconium-substituted zeolite (Ti-Zr-USY).
[0169] In order to prepare an alumina binder, 40 kg of an aqueous solution of 6.8 mass % sodium aluminate (based on Al2O3) was mixed with 40 kg of an aqueous solution of 2.4 mass % aluminum sulfate (based on Al2O3). In addition, the mixture was stirred at 60°C for 1 hour, and then the product was washed with 150 L of a 0.3 mass % ammonia aqueous solution to remove Na2SO4. Next, water was added to the product from which Na2SO4 was removed to adjust the Al2O3 concentration to 10 mass%. The pH was adjusted to 10.5 with 15 mass % ammonia water. The mixture was stirred at 95°C for 10 hours, dehydrated, washed, and kneaded with a kneader, thereby providing an alumina mixture.
[0170] The alumina kneaded product thus prepared was mixed with Ti—Zr—USY zeolite at a dry mass ratio of 3: 7. The mixture was molded into a columnar shape of 1.8 mm in diameter and fired at 550° C. for 3 hours, thereby preparing calcined composite particles.
[0171] Next, the hydrogenation active metal component is added to the calcined composite particles. An aqueous solution containing the hydrogenation active metal component is prepared by adding 700 mL of water to 200 g of molybdenum trioxide (an example of a hydrogenation active metal component) and 91 g of nickel carbonate (an example of a hydrogenation active metal component). The aqueous solution is mixed with 500 g of calcined composite particles (a composite of Ti-Zr-USY zeolite and alumina) and dried at 250° C. for 1 hour. The collected mixture is fired at 550° C. for 3 hours to prepare calcined composite particles with active phase materials, and collected, thereby obtaining about 0.5 kg of a reference catalyst.
[0172] Example 1
[0173] The process of the comparative example is followed to obtain a titanium-zirconium-substituted zeolite Ti-Zr-USY. An aqueous solution containing a hydrogenation-active metal component is prepared by adding 300 mL of water to 100 g of molybdenum trioxide (an example of a hydrogenation-active metal component) and 45 g of nickel carbonate (an example of a hydrogenation-active metal component). The aqueous solution is mixed with 150 g of Ti-Zr-USY zeolite, thereby providing about 0.5 kg of a metal-loaded Ti-Zr-USY zeolite. The collected mixture is fired at 550 ° C for 3 hours, thereby preparing a calcined Ti-Zr-USY zeolite material impregnated with an active metal component therein.
[0174] When the kneaded product thus prepared was mixed with a metal-loaded Ti-Zr-USY zeolite at a dry mass ratio of 3:7, the alumina mixture (as prepared in Comparative Example) was molded. The mixture was molded into a columnar shape having a diameter of 1.8 mm and fired at 550° C. for 1 hour, and about 0.5 kg of catalyst particles were collected, which were calcined extrudates formed of a composite of a metal-loaded Ti-Zr-USY zeolite and alumina.
[0175] Example 2
[0176] The process of the comparative example is followed to obtain a titanium-zirconium-substituted zeolite Ti-Zr-USY. An aqueous solution containing a hydrogenation-active metal component is prepared by adding 300 mL of water to 100 g of molybdenum trioxide (an example of a hydrogenation-active metal component) and 45 g of nickel carbonate (an example of a hydrogenation-active metal component). 230 mL of the active metal component aqueous solution is mixed with 150 g of the Ti-Zr-USY zeolite, thereby providing about 0.5 kg of dry metal-loaded Ti-Zr-USY zeolite. The collected mixture is fired at 550 ° C for 3 hours, thereby preparing a calcined Ti-Zr-USY zeolite material impregnated with active metal components therein.
[0177] The metal-loaded Ti-Zr-USY zeolite and the alumina mixture (as prepared in the comparative example) were mixed at a dry mass ratio of 3: 7. The mixture was formed into a columnar shape having a diameter of 1.8 mm and fired at 550° C. for 1 hour, and about 0.5 kg of catalyst particles were recovered, which were calcined extrudates formed of a composite of the metal-loaded Ti-Zr-USY zeolite and the metal-loaded alumina.
[0178] Example 3
[0179] The process of the comparative example is followed to obtain a titanium-zirconium-substituted zeolite Ti-Zr-USY. An aqueous solution containing a hydrogenation-active metal component is prepared by adding 300 mL of water to 100 g of molybdenum trioxide (an example of a hydrogenation-active metal component) and 45 g of nickel carbonate (an example of a hydrogenation-active metal component). Half of the aqueous solution of the active metal component is mixed with 150 g of Ti-Zr-USY zeolite. The collected mixture is fired at 550° C. for 3 hours, thereby preparing a calcined Ti-Zr-USY zeolite material impregnated with an active metal component therein.
[0180] The alumina mixture (as prepared in the comparative example) was diluted with water to have 10 mass % Al2O3, and the pH was adjusted to 10.5 with aqueous ammonia. The metal-loaded Ti-Zr-USY zeolite was mixed with the metal-loaded alumina at a dry mass ratio of 3:7. The mixture was formed into a columnar shape with a diameter of 1.8 mm and fired at 550°C for 3 hours, and about 0.5 kg of intermediate catalyst particles were collected.
[0181] Next, the remaining portion of the aqueous solution containing the hydrogenation-active metal component was mixed with 500 g of calcined intermediate catalyst particles (a composite of metal-loaded Ti-Zr-USY zeolite and alumina) and dried at 250° C. for 1 hour. The recovered mixture was calcined at 550° C. for 1 hour, and about 0.5 kg of catalyst particles were recovered, which were calcined metal-loaded extrudates, wherein the extrudates were formed of a composite of metal-loaded Ti-Zr-USY zeolite and alumina.
[0182] Example Results
[0183] The properties of the catalyst formed according to Example 3 relative to the comparative example are shown in Table 1:
[0184] Table 1
[0185]
[0186] The pilot plant was loaded with 100 ml of a commercially available pretreated catalyst, followed by 100 ml of the hydrocracking catalyst of the comparative examples and Example 3 herein. The pilot plant was tested at a hydrogen partial pressure of 13.5 MPa, a hydrogen / oil ratio of 1,000 StLt / Lt oil, and a 0.50 h -1 The catalysts were tested at an LHSV of 1.30 and reaction temperatures of 360, 375, 390 and 405° C. Table 2 shows the activities and product yields of the tested catalysts.
[0187] Table 2
[0188]
[0189] The method and system of the present invention have been described above; however, modifications will be apparent to one of ordinary skill in the art, and the scope of protection of the present invention is defined by the appended claims.
Claims
1. A method for preparing catalyst particles, comprising: Providing a framework-modified ultrastable Y (USY) zeolite, wherein a portion of the aluminum atoms constituting the zeolite framework thereof are replaced by zirconium atoms and / or titanium atoms and / or hafnium atoms, wherein the framework-modified USY zeolite is characterized by an outer surface and pores defining an inner surface; impregnating one or more active metal components on the outer surface and / or the inner surface of the pores of the framework-modified USY zeolite to form a metal-loaded framework-modified USY zeolite; Mixing and kneading the metal-loaded framework-modified USY zeolite and an inorganic oxide binder material to form a composite of the metal-loaded framework-modified USY zeolite and the inorganic oxide binder; forming catalyst particles from said composite of metal-loaded framework-modified USY zeolite and inorganic oxide binder into extrudates; heat treating the extrudate; and The calcined catalyst particles are recovered.
2. The method of claim 1, wherein the one or more active metal components impregnated on the framework-modified USY zeolite is a first portion of the total active metal component content of the one or more active metal components, wherein the inorganic oxide binder material is characterized by an outer surface and pores defining an inner surface, and wherein the method further comprises, prior to mixing and kneading: impregnating a second portion of the total active metal component content of the one or more active metal components onto the exterior surface and / or interior pore surfaces of the inorganic oxide binder material to form a metal loaded inorganic oxide binder, wherein the metal-loaded framework-modified USY zeolite and the metal-loaded inorganic oxide binder are mixed and kneaded to form a composite of the metal-loaded framework-modified USY zeolite and the metal-loaded inorganic oxide binder, and The catalyst particles are formed by forming a composite of the metal-loaded framework-modified USY zeolite and the metal-loaded inorganic oxide binder.
3. The method of claim 2, wherein the recovered calcined catalyst particles are intermediate calcined catalyst particles and are characterized by an outer surface and pores defining an inner surface; The method further comprises impregnating a third portion of the total active metal component content of the one or more active metal components onto the outer surface and / or the inner surface of the pores of the intermediate calcined catalyst particles to produce metal-loaded intermediate calcined catalyst particles, heat treating the metal-loaded intermediate calcined catalyst particles, and recovering the final calcined catalyst particles.
4. The method of claim 2, wherein the composite of metal-loaded framework-modified USY zeolite and metal-loaded inorganic oxide binder is characterized by an outer surface and pores defining an inner surface; and The method further comprises impregnating a third portion of the total active metal component content of the one or more active metal components onto the outer surface and / or pore inner surface of the composite of the metal-loaded framework-modified USY zeolite and the metal-loaded inorganic oxide binder.
5. The method according to claim 1, wherein: The one or more active metal components impregnated on the framework-modified USY zeolite are a first portion of the total active metal component content of the one or more active metal components, and The calcined catalyst particles are intermediate calcined catalyst particles and are characterized by an outer surface and pores defining an inner surface; The method further comprises impregnating a second portion of the total active metal component content of the one or more active metal components onto the outer surface and / or inner pore surface of the intermediate calcined catalyst particles, heat treating the metal-loaded intermediate calcined catalyst particles, and recovering the final calcined catalyst particles.
6. The method according to claim 1, wherein: The one or more active metal components impregnated on the framework-modified USY zeolite are a first portion of the total active metal component content of the one or more active metal components, and The composite of the metal-loaded framework-modified USY zeolite and the inorganic oxide binder is characterized by an outer surface and pores defining an inner surface; The method further comprises impregnating a second portion of the total active metal component content of the one or more active metal components onto the outer surface and / or inner pore surface of the composite of the metal-loaded framework-modified USY zeolite and the inorganic oxide binder.
7. The method of claim 6, wherein the recovered calcined catalyst particles are intermediate calcined catalyst particles and are characterized by an outer surface and pores defining an inner surface; The method further comprises impregnating a third portion of the total active metal component content of the one or more active metal components onto the outer surface and / or inner pore surface of the intermediate calcined catalyst particles, heat treating the metal-loaded intermediate calcined catalyst particles, and recovering the final calcined catalyst particles.
8. The method of claim 1, wherein the pores of the framework-modified USY zeolite define a volume, wherein impregnation of one or more active metal components uses metals in a liquid solution, and wherein the volume of the liquid solution is up to the pore volume of the framework-modified USY zeolite.
9. A method for producing the catalyst particles according to any one of claims 1 to 8, wherein the framework-modified USY zeolite is provided in a wet state, a dry state or a calcined state.
10. A method for producing catalyst particles according to any one of claims 1 to 8, wherein the framework-modified USY zeolite contains 0.1 to 5 mass % zirconium and / or titanium and / or hafnium calculated on an oxide basis.
11. A method for producing catalyst particles according to any one of claims 1 to 8 above, wherein the inorganic oxide material is selected from alumina, silica, titania, silica-alumina, alumina-titania, alumina-zirconia, alumina-boria, phosphorus-alumina, silica-alumina-boria, phosphorus-alumina-boria, phosphorus-alumina-silica, silica-alumina-titania, and silica-alumina-zirconia.
12. A method for producing catalyst particles according to any one of claims 1 to 8, wherein the metal-loaded framework-modified USY zeolite accounts for about 0.1 to 99 weight % of the active metal-containing composite catalyst particles, with the remaining mass comprising the inorganic oxide component.
13. A method of producing the catalyst particles according to any one of claims 1 to 8 above, wherein the catalyst particles are formed from the metal-loaded framework-modified USY zeolite, the inorganic oxide component, and another zeolite component.
14. A method of making catalyst particles according to claim 13, wherein the metal-loaded framework-modified USY zeolite comprises about 0.1-99 weight percent of the catalyst particles, wherein a first remaining mass comprises the inorganic oxide component and a second remaining mass comprises the additional zeolite component.
15. A method for producing the catalyst particles according to any one of claims 1 to 8 above, wherein the active metal component is selected from the group consisting of platinum, palladium and rhenium, and wherein the active metal component is present in an amount of 0.01 to 2 wt. % with respect to the mass of the active metal component, based on the mass of the catalyst particles.
16. A method for producing the catalyst particles according to any one of claims 1 to 8 above, wherein the active metal component is selected from the group consisting of Mo, W, Co, Ni, and combinations thereof, and wherein the active metal component is present in an amount of 0.1 to 40 wt % with respect to the mass of the active metal component, based on the mass of the catalyst particles.
17. A calcined catalyst particle comprising a composite of: A framework-modified ultrastable Y (USY) zeolite wherein a portion of the aluminum atoms constituting the zeolite framework are replaced by zirconium atoms and / or titanium atoms and / or hafnium atoms, wherein the framework-modified USY zeolite is characterized by an outer surface and pores defining an inner surface, and wherein the outer surface and / or the inner surface of the pores are metal loaded with one or more active metal components; and Inorganic oxide binder materials; The composite is formed into extrudates and heat treated into calcined catalyst particles.
18. The calcined catalyst particle according to claim 17, wherein the framework-modified zeolite is substituted with 0.1 to 5 mass% of zirconium atoms and 0.1 to 5 mass% of titanium ions calculated on an oxide basis.
19. The calcined catalyst particles of claim 17, wherein the framework-modified USY zeolite has the following characteristics: (a) a lattice constant of 2.430 to 2.450 nm, (b) a specific surface area of 600 to 900 m 2 / g, and (c) a molar ratio of SiO2 to Al2O3 of 12 to 100.
20. The calcined catalyst particles according to claim 17, having a specific surface area of 200 to 450 m 2 / g; has or less in diameter is 0.40 to 0.75 ml / g; and wherein the one or more active metal components are 0.01 to 40 mass % relative to the total mass of the calcined catalyst particles.
21. The calcined catalyst particle according to claim 17, wherein the active metal component is selected from the group consisting of platinum, palladium and rhenium, and wherein the active metal component is present in an amount of 0.01-2 wt. % with respect to the mass of the active metal component, based on the mass of the catalyst particle.
22. The calcined catalyst particle according to claim 17, wherein the active metal component is selected from the group consisting of Mo, W, Co, Ni, and combinations thereof, and wherein the active metal component is present in an amount of 0.1-40 wt. % with respect to the mass of the active metal component, based on the mass of the catalyst particle.