Halogen-functionalized cyclotrisilazanes as precursors for deposition of silicon-containing films

By depositing silicon-containing films at low temperatures using halogen-functionalized cyclotrisilazane, using oxygen- and nitrogen-containing reactant sources, the problem of impurities in low-temperature deposited silicon oxide films is solved, the density and conformality of the films are improved, and it is suitable for Nano-laminated multi-layer structure.

CN118786243APending Publication Date: 2024-10-15VERSUM MATERIALS US LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380022696.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-26
Filing Date
2023-01-25
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing technology has impurity problems when depositing silicon oxide films at low temperatures, and conventional precursors tend to self-react when deposited at high temperatures, reducing shape retention and controllability.

Method used

Using halogen-functionalized cyclotrisilazane as the silicon precursor, silicon-containing films are deposited at lower temperatures via thermal ALD, PEALD, or PEALD-like processes using oxygen- and nitrogen-containing reactant sources to form high-density, low-impurity and highly conformal silicon oxide or silicon nitride membranes.

Benefits of technology

It achieves the deposition of high-density, low-impurity and highly conformal silicon-containing films at lower temperatures, improves the growth rate and controllability of the film, and is suitable for the deposition of nano-laminated multi-layer structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786243A_ABST
    Figure CN118786243A_ABST
Patent Text Reader

Abstract

Disclosed are halogen-functionalized cyclotrisilazane precursor compounds according to Formulae A and B, and methods of using the compounds for depositing silicon-containing films, such as silicon oxide, silicon nitride, silicon oxynitride, silicon carbonitride, silicon oxycarbonitride, or carbon-doped silicon oxide, by a thermal atomic layer deposition (ALD) or plasma enhanced atomic layer deposition (PEALD) process and combinations thereof. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Field of the Invention

[0001] Halogen-functionalized cyclotrisilazane precursor compounds, and compositions and methods containing the same, are described herein for depositing silicon-containing films (such as, but not limited to, silicon oxide, silicon nitride, silicon oxynitride, silicon carbonitride, silicon oxycarbonitride, and carbon-doped silicon oxide) by thermal atomic layer deposition (thermal ALD) or plasma enhanced atomic layer deposition (PEALD) processes or combinations thereof. The silicon-containing film can be a stoichiometric or non-stoichiometric silicon-containing film or material, and can be deposited at one or more deposition temperatures of about 600° C. or less, including, for example, a temperature in the range of about 25° C. to about 300° C. Background of the Invention

[0003] ALD and PEALD are processes for depositing, for example, conformal films of silicon oxide at low temperatures (<600°C). In the ALD and PEALD processes, precursors and reactive gases (such as oxygen or ozone) are pulsed separately for a certain number of cycles to form a monolayer of silicon oxide at each cycle. However, silicon oxide deposited at low temperatures using these processes may contain impurities, such as but not limited to nitrogen (N), at levels that may be harmful in certain semiconductor applications. To remedy this, one possible solution is to increase the deposition temperature to 600°C or higher. However, at these higher temperatures, conventional precursors used by the semiconductor industry tend to self-react, thermally decompose, and / or be deposited in a chemical vapor deposition (CVD) mode rather than an ALD mode. The CVD deposition mode has reduced conformality compared to ALD deposition, especially for high aspect ratio structures required in many semiconductor applications. In addition, the CVD deposition mode has less control over the thickness of the film or material compared to ALD mode deposition.

[0004] US 5,413,813 and US 5,424,095 describe the use of various hexamethylcyclotrisilazanes and other silazanes to coat metal or metal oxide surfaces within a reaction chamber with ceramic materials at high temperatures to prevent coking during subsequent reactions involving the pyrolysis of hydrocarbons.

[0005] US10023958 B discloses atomic layer deposition of films containing silicon, carbon and nitrogen using the discussed halogenated silicon precursor. Some methods involve exposing the substrate surface to a silicon precursor, wherein the silicon precursor is halogenated with Cl, Br or I, and the silicon precursor comprises a halogenated silane, a halogenated carbosilane, a halogenated aminosilane or a halogenated carbosilylamine. The substrate surface can then be exposed to a nitrogen-containing plasma or a nitrogen precursor and a dense plasma.

[0006] US8460753 B discloses a method for forming a silicon dioxide film having an extremely low wet etching rate in an HF solution using a thermal CVD process, an ALD process or a cyclic CVD process, wherein the silicon precursor is selected from one of the following: R1 n R 2 m Si(NR 3 R 4 ) 4-n-m ; and (R 1 R 2 SiC 3 ) p Cyclic silazane, where R 1 is an alkenyl or aromatic group, such as vinyl, allyl and phenyl; R 2 , R 3 and R 4 Selected from H, straight chain, branched chain or cyclic C1-C 10 Alkyl, linear, branched or cyclic C2-C 10 Alkenyl and aromatic groups; n=1-3, m=0-2; p=3-4.

[0007] US9583333 B describes the deposition of a silicon nitride layer on a substrate at a temperature below 300° C. in a plasma enhanced CVD process by using a remote plasma and hexamethylcyclotrisilazane or other aminosilanes.

[0008] US9793108 B describes the use of UV-assisted photochemical vapor containing different silazanes, including hexamethylcyclotrisilazane, for the purpose of pore sealing of porous low dielectric films.

[0009] US20130330482A1 describes the deposition of carbon-doped silicon nitride films by a plasma enhanced CVD process using vinyl-substituted cyclotrisilazane or other silazanes as precursors.

[0010] There is a need in the art for a method for forming uniform and conformal silicon-containing films such as silicon oxide or silicon nitride in a thermal ALD, PEALD process, or PEALD-like process using less expensive, reactive, and more stable silicon precursor compounds, the films having at least one or more of the following properties: a density of about 2.1 g / cc or more, / cycle or higher growth rates, low chemical impurities and high conformality. SUMMARY OF THE INVENTION

[0012] The present invention solves the above-mentioned needs and other problems in the art by providing compositions and methods for depositing stoichiometric or non-stoichiometric silicon-containing materials or films, such as but not limited to silicon oxide, carbon-doped silicon oxide, silicon oxynitride films, silicon nitride, carbon-doped silicon nitride and carbon-doped silicon oxynitride films, at relatively low temperatures (e.g., at one or more temperatures of 600°C or less) in the following deposition processes: PEALD, plasma enhanced cyclic CVD (PECCVD), PEALD-like processes or ALD processes, using oxygen-containing reactant sources, nitrogen-containing reactant sources or combinations thereof.

[0013] In one aspect, at least one silicon precursor compound selected from formula A and B is provided:

[0014]

[0015] Where R 1-6 are each independently selected from hydrogen, methyl and halogen (including Cl, Br and I); R 7 and R 8 are each independently selected from hydrogen, C 1-10 Straight chain alkyl, C 3-10 Branched alkyl, C 3-10 Cycloalkyl, C 2-10 Alkenyl, C 4-10 Aryl and C 4-10 Heterocyclic group; R 9-11 are each independently selected from hydrogen, C 1-10 Straight chain alkyl, C 3-10 Branched alkyl, C 3-10 Cycloalkyl, C 2-10 Alkenyl, C 4-10 Aryl, C 4-10 Heterocyclic group and halogen (including Cl, Br and I), wherein the substituent R 1-11 Two or more of the substituents R in formula A may be linked to form a substituted or unsubstituted, saturated or unsaturated cyclic group, wherein the substituent R in formula A 1-6 At least one of them is halogen, wherein R 7 and R 8 cannot all be hydrogen, and the substituent R in formula B 9-11 At least one of the compounds is a halogen. The compounds of formula A and B are halogen-functionalized cyclotrisilazane having at least 3 silicon atoms and a Si3N3 6-membered ring.

[0016] In another embodiment, a method for depositing a silicon-containing film on a substrate is provided, the method comprising the steps of: a) providing a substrate in a reactor; b) introducing into the reactor at least one silicon precursor compound selected from formula A and B:

[0017]

[0018] Where R 1-6 are each independently selected from hydrogen, methyl and halogen (including Cl, Br and I); R 7 and R 8 are each independently selected from hydrogen, C 1-10 Straight chain alkyl, C 3-10 Branched alkyl, C 3-10 Cycloalkyl, C 2-10 Alkenyl, C 4-10 Aryl and C 4-10 Heterocyclic group; R 9-11 are each independently selected from hydrogen, C 1-10 Straight chain alkyl, C 3-10 Branched alkyl, C 3-10 Cycloalkyl, C 2-10 Alkenyl, C 4-10 Aryl, C 4-10 Heterocyclic group and halogen (including Cl, Br and I), wherein the substituent R 1-11 Two or more of the substituents R in formula A may be linked to form a substituted or unsubstituted, saturated or unsaturated cyclic group, wherein the substituent R in formula A 1-6 At least one of them is a halogen (including Cl, Br and I), wherein R in formula A 7 and R 8 cannot all be hydrogen, and the substituent R in formula B 9-11 at least one of which is a halogen (including Cl, Br and I); c) purging the reactor with a purge gas; d) introducing an oxygen-containing or nitrogen-containing source (or a combination thereof) into the reactor; and e) purging the reactor with a purge gas, wherein steps b to e are repeated until a film of a desired thickness is deposited, and wherein the method is carried out at one or more temperatures in the range of about 25°C to 600°C.

[0019] In some embodiments, the oxygen-containing source used in the method is a source selected from oxygen, oxygen plasma, ozone, water vapor, water vapor plasma, nitrogen oxide (e.g., N2O, NO, NO2) plasma with or without an inert gas, carbon oxide (e.g., CO2, CO) plasma, and combinations thereof. In certain embodiments, the oxygen-containing source further comprises an inert gas. In these embodiments, the inert gas is selected from argon, helium, nitrogen, hydrogen, and combinations thereof. In an optional embodiment, the oxygen-containing source does not comprise an inert gas. In yet another embodiment, the oxygen-containing source comprises nitrogen, which reacts with the reagent under plasma conditions to provide a silicon oxynitride film.

[0020] In some embodiments, the nitrogen-containing source is introduced into the reactor. Suitable nitrogen-containing source gas can include, for example, ammonia, hydrazine, monoalkyl hydrazine, dialkyl hydrazine, nitrogen, nitrogen / hydrogen, nitrogen / argon plasma, nitrogen / helium plasma, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, organic amines such as tert-butylamine, dimethylamine, diethylamine, isopropylamine, diethylamine plasma, dimethylamine plasma, trimethylamine plasma, ethylenediamine plasma, alkoxyamines such as ethanolamine plasma and mixtures thereof. In certain embodiments, the nitrogen-containing source comprises ammonia plasma, a plasma comprising nitrogen and argon, a plasma comprising nitrogen and helium, or a plasma comprising hydrogen and nitrogen.

[0021] In the above embodiments and throughout the present invention, the inert gas is selected from argon, helium, nitrogen, hydrogen or a combination thereof. In an alternative embodiment, the oxygen-containing plasma source or the nitrogen-containing plasma source does not contain an inert gas.

[0022] One embodiment of the present invention is directed to uniform and conformal silicon-containing films, such as silicon oxide or silicon nitride, using cheaper, more reactive and more stable silicon precursor compounds in thermal ALD, PEALD processes or PEALD-like processes, having at least one or more of the following properties: a density of about 2.1 g / cc or greater, / cycle or greater growth rates, low chemical impurities, and / or high conformality.

[0023] The embodiments of the present invention may be used alone or in combination with each other. DETAILED DESCRIPTION OF THE INVENTION

[0025] All references, including publications, patent applications, and patents, cited herein are hereby incorporated by reference as if each reference were individually and specifically indicated to be incorporated by reference and were set forth in its entirety herein.

[0026] In the context of describing the present invention (especially in the context of the following claims), the use of the terms "one" and "an" and "the" and similar indications should be interpreted as covering the singular and plural, unless otherwise stated herein or clearly contradictory to the context. Unless otherwise stated, the terms "comprising", "having", "including" and "containing" should be interpreted as open terms (i.e., meaning "including, but not limited to"). Unless otherwise stated herein, the description of the numerical range herein is intended only to be used as a shorthand method for individually referring to each individual value falling within the range, and each individual value is incorporated into the specification as if it is individually described herein. Unless otherwise stated herein or clearly contradictory to the context, all methods described herein can be performed in any suitable order. The use of any and all examples or exemplary language (e.g., "such as") provided here is only to better illustrate the present invention, rather than to limit the scope of the present invention, unless otherwise stated. Any language in the specification should not be interpreted as indicating that any unclaimed element is essential to the practice of the present invention.

[0027] The preferred embodiments of the present invention described herein are illustrative and should not limit the scope of the present invention. After reading the foregoing description, the changes of those preferred embodiments are obvious to those of ordinary skill in the art. The inventor expects that a skilled person will appropriately adopt these changes, and the inventor intends to implement the present invention in a manner different from that specifically described herein. Therefore, the present invention includes all modifications and equivalents of the subject matter described in the appended claims as allowed by applicable law. In addition, the present invention includes any combination of the above-mentioned elements of all possible variations, unless otherwise stated herein or clearly contradictory to the context.

[0028] Described herein are methods associated with forming stoichiometric or non-stoichiometric silicon-containing films or materials using one or more temperatures of about 600°C or less, or about 25°C to about 600°C, and in some embodiments, 25°C to about 300°C, such as, but not limited to, silicon oxide, carbon-doped silicon oxide films, silicon oxynitride, silicon nitride, carbon-doped silicon nitride, carbon-doped silicon oxynitride films, or combinations thereof. The films described herein are deposited in a deposition process, such as atomic layer deposition (ALD) or an ALD-like process, such as, but not limited to, plasma enhanced ALD (PEALD) or a plasma enhanced cyclic chemical vapor deposition process (PECCVD). The low temperature deposition (e.g., one or more deposition temperatures ranging from about ambient temperature to 600°C) methods described herein provide films or materials that exhibit at least one or more of the following advantages: a density of about 2.1 g / cc or more, low chemical impurities, high conformality in thermal ALD, PEALD processes, or PEALD-like processes, the ability to adjust the carbon content in the resulting film; and / or a film having a rate of 5 angstroms per second ( For carbon-doped silicon oxide and carbon-doped silicon nitride films, more than 1% carbon is required to adjust the etch rate to less than 2 % in 0.5 wt% dilute HF. / second, in addition to other characteristics, such as, but not limited to, a density of about 1.8 g / cc or greater or about 2.0 g / cc or greater.

[0029] The present invention can be implemented using equipment known in the art. For example, the method of the present invention can use a conventional reactor in the field of semiconductor manufacturing.

[0030] In one embodiment, the silicon precursor composition described herein comprises at least one silicon precursor compound selected from Formula A and B:

[0031]

[0032] Where R 1-6 are each independently selected from hydrogen, methyl and halogen (including Cl, Br and I); R 7 and R 8 are each independently selected from hydrogen, C 1-10 Straight chain alkyl, C 3-10 Branched alkyl, C 3-10 Cycloalkyl, C 2-10 Alkenyl, C 4-10 Aryl and C 4-10 Heterocyclic group; R 9-11 are each independently selected from hydrogen, C 1-10 Straight chain alkyl, C 3-10 Branched alkyl, C 3-10 Cycloalkyl, C 2-10 Alkenyl, C 4-10 Aryl, C 4-10 Heterocyclic group and halogen (including Cl, Br and I), wherein the substituent R 1-11 Two or more of the substituents R in formula A may be linked to form a substituted or unsubstituted, saturated or unsaturated cyclic group, wherein the substituent R in formula A 1-6 At least one of them is a halogen (including Cl, Br and I), wherein R in formula A 7 and R 8 cannot all be hydrogen, and the substituent R in formula B 9-11 At least one of the compounds is a halogen (including Cl, Br and I). The compounds of formula A and B are halogen-functionalized cyclotrisilazane having at least 3 silicon atoms and a Si3N3 6-membered ring.

[0033] In certain embodiments, for R 1-6 The halogen for R is selected from Cl, Br and I. In other embodiments, 9-11The halogen for R is selected from Cl, Br and I. In yet other embodiments, 1-6 and R 9-11 The halogen is selected from Cl, Br and I.

[0034] In certain embodiments, for R 1-6 At least one of the halogens in R is Cl. 9 -11 In yet other embodiments, at least one of the halogens in R is Cl. 1-6 At least one and R 9-11 At least one of the halogens is Cl.

[0035] In one embodiment, R 1-6 In another embodiment, R 1 , R 3 and R 5 In another embodiment, R 9-11 In yet another embodiment, R 1-6 and R 9-11 Each of them is Cl.

[0036] In certain embodiments of the compositions described herein, a solvent is further included. Exemplary solvents include, but are not limited to, ethers, tertiary amines, alkanes, aromatic hydrocarbons, tertiary amino ethers, and combinations thereof. In certain embodiments, the difference between the boiling point of the silicon precursor and the boiling point of the solvent is 40° C. or less.

[0037] In the above formula and throughout the specification, the term "alkyl" means a straight or branched functional group having 1 to 10 carbon atoms. Exemplary straight chain alkyls include, but are not limited to, methyl, ethyl, propyl, butyl, pentyl, and hexyl. Exemplary branched alkyls include, but are not limited to, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, tert-pentyl, isohexyl, and neohexyl. In certain embodiments, the alkyl may have one or more functional groups attached thereto, such as, but not limited to, an alkoxy, a dialkylamino, or a combination thereof attached thereto. In other embodiments, the alkyl does not have one or more functional groups attached thereto.

[0038] In the above formula and throughout the specification, the term "cycloalkyl" refers to a cyclic functional group having 3 to 10 carbon atoms. Exemplary cycloalkyl groups include, but are not limited to, cyclobutyl, cyclopentyl, cyclohexyl, and cyclooctyl.

[0039] In the above formulae and throughout the specification, the term "alkenyl" denotes a group having one or more carbon-carbon double bonds and having 2 to 10 or 2 to 6 carbon atoms.

[0040] In the above formula and throughout the specification, the term "aryl" refers to an aromatic cyclic functional group having 4 to 10 carbon atoms, 5 to 10 carbon atoms, or 6 to 10 carbon atoms. Exemplary aryl groups include, but are not limited to, phenyl, benzyl, chlorobenzyl, tolyl, o-xylyl, 1,2,3-triazolyl, pyrrolyl, and furanyl.

[0041] In the above formulae and throughout the specification, when the term "halogen" refers to a substituent, the term means a halogen radical selected from the periodic table of elements, which includes fluorine, bromine, chlorine and iodine.

[0042] In the above formula and throughout the specification, the term "heterocycle" refers to a non-aromatic saturated monocyclic or polycyclic ring system of about 3 to about 10 ring atoms, preferably about 5 to about 10 ring atoms, wherein one or more atoms in the ring system are elements other than carbon, such as nitrogen, oxygen or sulfur. Preferred heterocycles contain about 5 to about 6 ring atoms. The prefix aza, oxa or thia before the heterocycle refers to at least one nitrogen, oxygen or sulfur atom present as a ring atom, respectively. The heterocyclic group is optionally substituted.

[0043] Exemplary halogen-functionalized cyclotrisilazane precursors are listed in Table 1:

[0044] Table 1

[0045]

[0046]

[0047]

[0048] The silicon precursor composition described herein comprising at least one silicon precursor compound selected from the group consisting of formula A and B according to the present invention is preferably substantially free of metal ions, such as Li + 、Na + , K + Mg 2+ , Ca 2+ 、Al 3+ , Fe 2+ , Fe 3+ 、Ni 2+ Cr 3+ As used herein, the term "substantially free" in relation to such metal ions means less than 5 ppm (by weight), preferably less than 3 ppm, more preferably less than 1 ppm, more preferably less than 0.1 ppm, and most preferably less than 0.05 ppm as measured by ICP-MS or other analytical methods for measuring metals. In addition, when used as a precursor for depositing a silicon-containing film, the silicon precursor composition having formula A and / or B has a purity of 98 wt % or more, more preferably 99 wt % or more, as measured by GC.

[0049] Without intending to be bound by theory, it is believed that the advantage of these precursors over non-functionalized or amino-functionalized cyclotrisilazanes is that they have at least one Si-halogen anchor unit. This Si-X (X = Cl, Br or I) bond should be able to react much more easily with NH-terminated surfaces to convert Si x N y Environmentally anchored to the surface, and thus grow silicon- and nitrogen-containing films, such as silicon nitride or carbon-doped silicon nitride, after repeated cycles of [precursor→purge→nitridation→purge] at much lower temperatures than previously disclosed cyclotrisilazanes. It is also believed that the multiple Si-N bonding networks pre-built into the Si3N3 rings of these precursors can allow for more robust and therefore higher quality silicon- and nitrogen-containing films, such as stoichiometric silicon nitride having the formula Si3N4 to be deposited, and higher growth per cycle compared to conventional chlorosilane precursors under the same deposition conditions. It is also believed that these halogen-functionalized cyclotrisilazane precursors can also be suitable for high growth rate deposition of conformal silicon- and oxygen-containing films, such as silicon oxide, carbon-doped silicon oxide, silicon oxynitride, and carbon-doped silicon oxynitride, when an oxygen-containing reactant source is used in combination with, together with, or in place of a nitrogen-containing reactant source. This dual functionality allows these precursors to be used in applications where multiple alternating layers of silicon nitride and silicon oxide are deposited, for example in nanolaminated multilayer structures, without changing the silicon-containing precursor.

[0050] In addition to conventional methods for synthesizing cyclotrisilazane molecules (such as the reaction of chlorosilane with amine or metal amide to form Si-N bonds), compounds having formula A or B can be prepared by the reaction

[0051] The synthesis was carried out by the reactions illustrated in Formulas 1 and 2.

[0052]

[0053] It will be clear to those skilled in the art that the use of other phosgene, phosgene or phosgene reagents, as well as various other amino-functionalized cyclotrisilazanes starting materials, in Reaction Scheme 1, allows for the synthesis of a variety of combinations of halogen-functionalized cyclotrisilazanes having Formula A. It will also be clear to those skilled in the art that the use of other deprotonating agents, such as alkali or alkaline earth metals, metal hydrides or metal alkyls, in the first step of Reaction Scheme 2, and the use of other simple halosilane reagents, such as SiCl4, Cl3SiH, Cl2SiMeH, Cl3SiMe, Br2SiH2 or I2SiH2, in the second step of Reaction Scheme 2, can provide various other halogen-functionalized cyclotrisilazanes having Formula B.

[0054] An alternative synthetic method to generate halogen-functionalized cyclotrisilazanes of formula B involves the direct reaction of simple halosilanes (such as those mentioned above) with NH-functionalized cyclotrisilazane starting materials (optionally in the presence of a Lewis base), as illustrated in Scheme 3.

[0055]

[0056] Another alternative method for synthesizing halogen functionalized cyclotrisilazanes of formula A or B involves directly converting at least one Si-H bond on the hydride functionalized cyclotrisilazanes to a Si-X bond (X = Cl, Br, I) as illustrated in Equations 4 and 5. Many halogenating agents known in the literature for such conversions that can be used in such halogenation reactions include, but are not limited to, Cl2, Br2, I2, HCl, HBr, HI, acetyl halides, alkyl halides, aryl halides, trityl halides, tin halides, antimony halides, mercury halides, iron halides, nickel halides, palladium halides, phosphorus halides, boron halides, N-halosuccinimide, other organic halides, other main group element halides, or transition metal halides. Some of these Si-H to Si-X halogenation reactions may require a catalyst.

[0057]

[0058] In another embodiment of the present invention, a method of depositing a silicon-containing film on at least one surface of a substrate is described herein, wherein the method comprises the following steps:

[0059] a. providing a substrate in a reactor;

[0060] b. introducing into the reactor at least one silicon precursor compound having a structure selected from the group consisting of formula A and B as defined above;

[0061] c. purging the reactor with a purge gas;

[0062] d. introducing an oxygen-containing source comprising a plasma into the reactor; and

[0063] e. Purge the reactor with purge gas.

[0064] In this method, steps b to e are repeated until a film of desired thickness is deposited on the substrate.

[0065] The method of the present invention is carried out by using an ALD process with an ozone or oxygen-containing source comprising a plasma, wherein the plasma may further comprise an inert gas, such as one or more of the following: an oxygen plasma with or without an inert gas, a water vapor plasma with or without an inert gas, a nitrogen oxide (e.g., N2O, NO, NO2) plasma with or without an inert gas, a carbon oxide (e.g., CO2, CO) plasma with or without an inert gas, and combinations thereof.

[0066] The oxygen-containing plasma source may be generated in situ, or remotely. In a particular embodiment, the oxygen-containing source comprises oxygen gas and is flowed or introduced during method steps b to e along with other reagents such as, but not limited to, the at least one silicon precursor compound and optionally an inert gas.

[0067] For those embodiments in which at least one silicon precursor compound having a structure selected from formula A and B is used in a composition comprising a solvent, the selected solvent or mixture thereof does not react with the silicon precursor. The amount of the solvent in the composition by weight percentage is in the range of 0.5 wt % to 99.5 wt % or 10 wt % to 75 wt %. In this or other embodiments, the boiling point (bp) of the solvent is similar to the boiling point of the silicon precursor compound of formula A or B, or the boiling point of the solvent differs from the boiling point of the silicon precursor of formula A or B by 40°C or less, 30°C or less, or 20°C or less, or by 10°C. Alternatively, the difference in boiling point is within the range of any one or more of the following endpoints: 0, 10, 20, 30 or 40°C. Examples of suitable boiling point difference ranges include, but are not limited to, 0°C to 40°C, 20°C to 30°C or 10°C to 30°C. Examples of suitable solvents in the composition include, but are not limited to, ethers (e.g., 1,4-dioxane, dibutyl ether), tertiary amines (e.g., triethylamine, pyridine, 1-methylpiperidine, 1-ethylpiperidine, N,N'-dimethylpiperazine, N,N,N',N'-tetramethylethylenediamine), nitriles (e.g., acetonitrile or benzonitrile), alkyl hydrocarbons (e.g., octane, nonane, dodecane, ethylcyclohexane), aromatic hydrocarbons (e.g., toluene, xylene, mesitylene), tertiary amino ethers (e.g., bis(2-dimethylaminoethyl) ether), or mixtures thereof.

[0068] Throughout the specification, the term "ALD or ALD-like" refers to a process including but not limited to the following processes: a) various reactants including silicon precursors and reactive gases are sequentially introduced into a reactor, such as a single wafer ALD reactor, a semi-batch ALD reactor or a batch furnace ALD reactor; b) various reactants including silicon precursors and reactive gases are exposed to a substrate by moving or rotating the substrate to different parts of the reactor, and each part is separated by an inert gas curtain, i.e., a spatial ALD reactor or a roll-to-roll ALD reactor.

[0069] In certain embodiments, the silicon oxide or carbon-doped silicon oxide film deposited using the methods described herein is formed in the presence of an oxygen-containing source, the oxygen-containing source comprising ozone, water (H2O) (e.g., deionized water, purified water and / or distilled water), hydrogen peroxide (H2O2), oxygen (O2), oxygen plasma, NO, N2O, NO2, carbon monoxide (CO), carbon dioxide (CO2) and combinations thereof. The oxygen-containing source can be provided by, for example, an in-situ or remote plasma generator containing oxygen, such as an oxygen plasma, a plasma containing oxygen and argon, a plasma containing oxygen and helium, an ozone plasma, a water plasma, a nitrous oxide plasma or a carbon dioxide plasma. In certain embodiments, the oxygen-containing plasma source comprises an oxygen source gas introduced into the reactor at a flow rate ranging from about 1 to about 2000 standard cubic centimeters (sccm) or from about 1 to about 1000 sccm. The oxygen-containing plasma source can be introduced for a time ranging from about 0.1 to about 100 seconds. In a specific embodiment, the oxygen-containing plasma source comprises water having a temperature of 10°C or higher. In embodiments where the film is deposited via a PEALD or plasma enhanced cyclic CVD process, depending on the volume of the ALD reactor, the precursor pulse may have a pulse duration greater than 0.01 seconds (e.g., from about 0.01 to about 0.1 seconds, from about 0.1 to about 0.5 seconds, from about 0.5 to about 10 seconds, from about 0.5 to about 20 seconds, from about 1 to about 100 seconds), and the oxygen-containing plasma source may have a pulse duration less than 0.01 seconds (e.g., from about 0.001 to about 0.01 seconds).

[0070] Deposition methods disclosed herein may relate to one or more purge gases. The purge gas used to purge unconsumed reactants and / or reaction byproducts is an inert gas that does not react with the precursor, thereby forming a composition comprising the aforementioned substances. Exemplary purge gases include, but are not limited to, argon (Ar), nitrogen (N2), helium (He), neon, hydrogen (H2) and mixtures thereof. In certain embodiments, a purge gas such as Ar is supplied to the reactor for about 0.1 to 1000 seconds at a flow rate of about 10 to about 2000 sccm, thereby purging unreacted materials and any byproducts that may remain in the reactor.

[0071] The corresponding steps of supplying precursors, oxygen sources, and / or other precursors, source gases, and / or reagents may be performed by varying the time at which they are supplied to change the stoichiometric composition of the resulting dielectric film.

[0072] Energy is applied to at least one silicon precursor compound having a structure selected from Formulas A and B, an oxygen-containing source, or a combination thereof to induce a reaction and form a dielectric film or coating on the substrate. Such energy may be provided by, but is not limited to, heat, plasma, pulsed plasma, helicon plasma, high density plasma, inductively coupled plasma, X-ray, electron beam, photon, remote plasma methods, and combinations thereof. In certain embodiments, a secondary RF frequency source may be used to alter the plasma characteristics at the substrate surface. In embodiments where the deposition involves plasma, the plasma generation process may comprise a direct plasma generation process, in which the plasma is generated directly in the reactor, or alternatively a remote plasma generation process, in which the plasma is generated outside the reactor and supplied to the reactor.

[0073] The at least one silicon precursor compound can be delivered to the reaction chamber in various ways, such as a plasma enhanced cyclic CVD or PEALD reactor or a batch furnace reactor. In one embodiment, a liquid delivery system can be utilized. In an optional embodiment, a combined liquid delivery and flash process unit can be used, such as, for example, a turbo evaporator manufactured by MSP Corporation of Shoreview, MN, so that low volatility materials can be delivered by volume, which results in reproducible delivery and deposition without thermal decomposition of the precursor compound. In the liquid delivery mode, the precursor compound described herein can be delivered in a neat liquid form, or can be used in a solvent formulation or a composition comprising it. Therefore, in certain embodiments, the precursor formulation can include a solvent component of suitable properties, such as may be desirable and advantageous in a given end-use application, to form a film on a substrate.

[0074] As previously described, the purity level of at least one silicon precursor compound is high enough to be acceptable for reliable semiconductor manufacturing. In certain embodiments, at least one silicon precursor compound described herein contains less than 2% by weight, or less than 1% by weight, or less than 0.5% by weight of one or more of the following impurities: free amines, free halides or halogen ions, and higher molecular weight species. The higher purity levels of the silicon precursor compounds described herein can be obtained by one or more of the following processes: purification, adsorption, crystallization and / or distillation.

[0075] In one embodiment of the methods described herein, a plasma enhanced cyclic deposition process such as PEALD-like or PEALD can be used, wherein deposition is performed using at least one silicon precursor compound and an oxygen plasma source. A PEALD-like process is defined as a plasma enhanced cyclic CVD process, but still provides highly conformal silicon-containing films.

[0076] In certain embodiments, the gas line connecting the precursor tank to the reaction chamber is heated to one or more temperatures, and the container of at least one silicon precursor compound is maintained at one or more temperatures for bubbling, depending on the process requirements. In other embodiments, the solution containing at least one silicon precursor compound is injected into a vaporizer maintained at one or more temperatures for direct liquid injection.

[0077] Argon and / or other gas streams may be used as carrier gases to facilitate delivery of the vapor of at least one silicon precursor compound to the reaction chamber during the precursor pulse. In certain embodiments, the reaction chamber process pressure is between about 50 mTorr and 10 Torr. In other embodiments, the reaction chamber process pressure may be as high as 760 Torr (e.g., between about 50 mTorr and about 100 Torr).

[0078] In a typical PEALD or PEALD-like process (eg, PECCVD process), a substrate, such as a silicon oxide substrate, is heated on a heater stage in a reaction chamber and initially exposed to a silicon precursor compound to allow the complex to chemisorb onto the surface of the substrate.

[0079] A purge gas such as argon purges the unadsorbed excess compound from the process chamber. After sufficient purge, an oxygen-containing source can be introduced into the reaction chamber to react with the adsorbed surface, followed by another gas purge to remove the reaction byproducts from the reaction chamber. This process cycle can be repeated to obtain the desired film thickness. In some cases, pumping can replace the inert gas purge, or both can be used to remove unreacted silicon precursor compounds.

[0080] In this or other embodiments, it should be understood that the steps of the methods described herein can be performed in various orders, can be performed sequentially, can be performed simultaneously (e.g., during at least a portion of another step), and in any combination thereof. For example, the respective steps of supplying a precursor compound and an oxygen-containing source can be performed by varying the duration of supplying them to change the stoichiometric composition of the resulting dielectric film. In addition, the purge time after the precursor or oxidant step can be minimized to <0.1 seconds, thereby improving throughput.

[0081] In a specific embodiment, the method described herein deposits a high quality silicon-containing film, such as, for example, a film containing silicon and oxygen, on a substrate. The method comprises the following steps:

[0082] a. providing a substrate in a reactor;

[0083] b. introducing into the reactor at least one silicon precursor compound having a structure selected from Formula A and B described herein;

[0084] c. purging the reactor with a purge gas to remove at least a portion of the unadsorbed precursor compound;

[0085] d. introducing an oxygen-containing plasma source into the reactor, and

[0086] e. purging the reactor with a purge gas to remove at least a portion of the unreacted oxygen-containing source,

[0087] Steps b to e are repeated until a silicon-containing film of a desired thickness is deposited.

[0088] Another method disclosed herein forms a carbon-doped silicon oxide film using at least one silicon precursor compound having a structure selected from Formula A and B as defined above plus an oxygen source.

[0089] Another exemplary process is described as follows:

[0090] a. providing a substrate in a reactor;

[0091] b. contacting a vapor generated by at least one silicon precursor compound having a structure selected from Formula A and B as defined above, with or without co-flowing an oxygen source, so that the precursor compound is chemically adsorbed on the heated substrate;

[0092] c. Purge any unadsorbed precursor compounds;

[0093] d. introducing an oxygen source onto the heated substrate to react with the adsorbed precursor; and

[0094] e. Purge any unreacted oxygen source,

[0095] Repeat steps b to e until the desired thickness is achieved.

[0096] In another specific embodiment, the method described herein deposits a high quality silicon-containing film, such as, for example, a silicon nitride film, on a substrate. The method comprises the following steps:

[0097] a. providing a substrate in a reactor;

[0098] b. introducing into the reactor at least one silicon precursor compound having a structure selected from Formula A and B described herein;

[0099] c. purging the reactor with a purge gas to remove at least a portion of the unadsorbed precursor compound;

[0100] d. introducing a nitrogen-containing plasma source into the reactor, and

[0101] e. purging the reactor with a purge gas to remove at least a portion of the unreacted nitrogen source,

[0102] Steps b to e are repeated until a silicon-containing film of a desired thickness is deposited.

[0103] Another exemplary process is described as follows:

[0104] a. providing a substrate in a reactor;

[0105] b. contacting a vapor generated by at least one silicon precursor compound having a structure selected from the group consisting of formula A and B as defined above, with or without co-flowing a nitrogen source, so that the precursor compound is chemically adsorbed on the heated substrate;

[0106] c. Purge any unadsorbed precursor compounds;

[0107] d. introducing a nitrogen-containing source onto the heated substrate to react with the adsorbed precursor compound; and

[0108] e. Purge any unreacted nitrogen source,

[0109] Repeat steps b to e until the desired thickness is achieved.

[0110] In some embodiments, the methods described herein also use a volatile amine catalyst, such as triethylamine, trimethylamine, dimethylamine, methylamine, 4-dimethylaminopyridine, N,N'-dimethylethylenediamine, ethylenediamine or pyridine, which is co-flowed during the silicon precursor pulse step or the oxygen-containing and / or nitrogen-containing source pulse step, or during both chemical source pulse steps to promote the reaction of the precursor with the substrate surface and / or the anchor precursor compound with the co-reactant gas.

[0111] An exemplary method using a volatile amine catalyst comprises the following steps:

[0112] a. providing a substrate in a reactor;

[0113] b. introducing into the reactor at least one silicon precursor compound having a structure selected from Formula A and B described herein, and also introducing into the reactor a volatile amine catalyst such as pyridine;

[0114] c. purging the reactor with a purge gas to remove at least a portion of the unadsorbed precursor compound;

[0115] d. introducing a nitrogen and / or oxygen source into the reactor, and

[0116] e. purging the reactor with a purge gas to remove at least a portion of the unreacted nitrogen-containing and / or oxygen-containing source,

[0117] wherein steps b through e are repeated until a silicon-containing film of a desired thickness is deposited. A further exemplary method may include introducing a volatile amine catalyst into the reactor during steps b and d, or only during step d.

[0118] Various commercial ALD reactors, such as single wafer, semi-batch, batch furnaces or roll-to-roll reactors, can be used to deposit solid silicon oxide, silicon nitride, silicon oxynitride, carbon-doped silicon nitride, carbon-doped silicon oxynitride or carbon-doped silicon oxide.

[0119] The process temperatures of the methods described herein use one or more of the following temperatures as endpoints: 0° C., 25° C., 50° C., 75° C., 100° C., 125° C., 150° C., 175° C., 200° C., 225° C., 250° C., 275° C., 300° C., 325° C., 350° C., 375° C., 400° C., 425° C., 450° C., 475° C., 500° C., 525° C., 550° C., 575° C., 600° C. Exemplary temperature ranges include, but are not limited to, the following: about 0° C. to about 300° C.; or about 25° C. to about 300° C.; or about 50° C. to about 290° C.; or about 25° C. to about 250° C.; or about 25° C. to about 200° C.

[0120] In certain embodiments, the oxygen-containing source is selected from water vapor, ozone, oxygen, hydrogen peroxide, organic peroxides and mixtures thereof. In other embodiments, the oxygen-containing source is an oxygen-containing plasma source selected from water plasma, oxygen plasma, oxygen / helium plasma, oxygen / argon plasma, nitrogen oxide plasma, carbon dioxide plasma, carbon monoxide plasma and mixtures thereof. In other embodiments, the nitrogen source is selected from, for example, ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine, nitrogen, nitrogen / hydrogen, nitrogen / argon plasma, nitrogen / helium plasma, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, organic amines such as tert-butylamine, dimethylamine, diethylamine, isopropylamine, diethylamine plasma, dimethylamine plasma, trimethyl plasma, trimethylamine plasma, ethylenediamine plasma and alkoxyamines such as ethanolamine plasma and mixtures thereof. Still in other embodiments, the nitrogen-containing source is a nitrogen-containing plasma source selected from ammonia plasma, a plasma comprising nitrogen and argon, a plasma comprising nitrogen and helium or a plasma comprising hydrogen and nitrogen source gas and a combination thereof. In this or other embodiments, the method steps are repeated until the surface features are filled with a silicon-containing film. In embodiments where water vapor is used as the oxygen source, the substrate temperature is in the range of about -20°C to about 40°C or about -10°C to about 25°C.

[0121] In yet further embodiments of the methods described herein, a film deposited from an ALD, ALD, PEALD, or PEALD-like process or an as-deposited film is subjected to a treatment step (post-deposition). The treatment step may be performed during at least a portion of the deposition step, after the deposition step, and combinations thereof. Exemplary treatment steps include, but are not limited to, treatment by high temperature thermal annealing; plasma treatment; ultraviolet (UV) light treatment; laser; electron beam treatment, and combinations thereof to affect one or more properties of the film.

[0122] Films deposited with the silicon precursor compounds of Formula A or B described herein have improved properties, such as, but not limited to, a relatively lower wet etch rate of the film prior to the treatment step or a relatively higher density prior to the treatment step, when compared to films deposited with previously disclosed silicon precursor compounds under the same conditions. In a specific embodiment, the as-deposited film is treated intermittently during the deposition process. These intermittent or mid-deposition treatments can be performed, for example, after every ALD cycle, after every certain number of ALD cycles, such as, but not limited to, one (1) ALD cycle, two (2) ALD cycles, five (5) ALD cycles, or after every ten (10) or more ALD cycles.

[0123] Precursor compounds of formula A and B may exhibit / cycle or higher film growth rate.

[0124] In embodiments where the film is treated with a high temperature annealing step, the annealing temperature is at least 100° C. or higher than the deposition temperature. In this or other embodiments, the annealing temperature ranges from about 400° C. to about 1000° C. In this or other embodiments, the annealing process is performed in a vacuum (<760 Torr), an inert environment, an oxygen-containing environment (such as H2O, N2O, NO2, or O2), or a nitrogen-containing environment (such as H2 / N2, hydrazine, triethylamine, pyridine, or ammonia).

[0125] In embodiments where the film is subjected to UV treatment, the film is exposed to broadband UV, or a UV source having a wavelength range of about 150 nanometers (nm) to about 400 nm. In a specific embodiment, after the desired film thickness is achieved, the as-deposited film is exposed to UV in a chamber different from the deposition chamber.

[0126] In embodiments where the film is treated with plasma, a passivation layer such as SiO2 or carbon-doped SiO2 is deposited to prevent chlorine and nitrogen contaminants from penetrating into the film during subsequent plasma treatment. The passivation layer can be deposited using atomic layer deposition or cyclic chemical vapor deposition.

[0127] In embodiments where the film is treated with plasma, the plasma source is selected from hydrogen plasma, plasma containing hydrogen and helium, plasma containing hydrogen and argon. Hydrogen plasma reduces the film dielectric constant and improves damage resistance to subsequent plasma ashing treatment while still keeping the carbon content in the bulk almost unchanged.

[0128] Without intending to be bound by a particular theory, it is believed that the silicon precursor compound having a chemical structure represented by Formula A or B as defined above can be anchored by a halogenated group (such as chlorine) reacting with NH or hydroxyl groups on the substrate surface to provide Si-N-Si or Si-O-Si fragments, thereby increasing the growth rate of silicon nitride, silicon carbonitride, silicon oxide or carbon-doped silicon oxide compared to conventional silicon precursors such as bis(tert-butylamino)silane or bis(diethylamino)silane having only one silicon atom. Using the halogen-functionalized cyclotrisilazane having Formula A or B, up to 3 to 4 silicon atoms per molecule can be anchored to the substrate during the silicon precursor pulse step.

[0129] In certain embodiments, silicon precursor compounds having formula A or B as defined above may also be used as dopants for metal-containing films, such as, but not limited to, metal oxide films or metal nitride films. In these embodiments, the metal-containing film is deposited using an ALD or CVD process, such as those described herein using metal alkoxides, metal amides, or volatile organometallic precursors. Examples of suitable metal alkoxide precursors that can be used for the methods disclosed herein include, but are not limited to, Group 3-6 metal alkoxides, Group 3-6 metal complexes with alkoxy and alkyl-substituted cyclopentadienyl ligands, Group 3-6 metal complexes with alkoxy and alkyl-substituted pyrrolyl ligands, Group 3-6 metal complexes with alkoxy and diketone ligands; Group 3-6 metal complexes with alkoxy and ketoester ligands.

[0130] Examples of suitable metal amide precursors that can be used in the methods disclosed herein include, but are not limited to, tetrakis(dimethylamino)zirconium (TDMAZ), tetrakis(diethylamino)zirconium (TDEAZ), tetrakis(ethylmethylamino)zirconium (TEMAZ), tetrakis(dimethylamino)hafnium (TDMAH), tetrakis(diethylamino)hafnium (TDEAH), and tetrakis(ethylmethylamino)hafnium (TEMAH), tetrakis(dimethylamino)titanium (TDMAT), tetrakis(diethylamino)titanium (TDEAT), tetrakis(ethylmethylamino)titanium (TEMAT), tert-butyliminotris(diethylamino)tantalum (TBTDET), tert-butyliminotris(dimethylamino)tantalum (TBTDMT), tert-butyliminotris(dimethyl ... -butyliminotris(ethylmethylamino)tantalum (TBTEMT), ethyliminotris(diethylamino)tantalum (EITDET), ethyliminotris(dimethylamino)tantalum (EITDMT), ethyliminotris(ethylmethylamino)tantalum (EITEMT), tert-pentyliminotris(dimethylamino)tantalum (TAIMAT), tert-pentyliminotris(diethylamino)tantalum, penta(dimethylamino)tantalum, tert-pentyliminotris(ethylmethylamino)tantalum, bis(tert-butylimino)bis(dimethylamino)tungsten (BTBMW), bis(tert-butylimino)bis(diethylamino)tungsten, bis(tert-butylimino)bis(ethylmethylamino)tungsten, and combinations thereof. Examples of suitable organometallic precursors that can be used in the methods disclosed herein include, but are not limited to, Group 3 metal cyclopentadienyl or alkylcyclopentadienyl. Exemplary Group 3 to 6 metals herein include, but are not limited to, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Er, Yb, Lu, Ti, Hf, Zr, V, Nb, Ta, Cr, Mo, and W.

[0131] In certain embodiments, the silicon-containing films described herein have a dielectric constant of 6 or less, 5 or less, 4 or less, and 3 or less. In these or other embodiments, the film has a dielectric constant of about 5 or less, or about 4 or less, or about 3.5 or less. However, it is contemplated that films with other dielectric constants (e.g., higher or lower) may be formed depending on the desired end use of the film. Examples of silicon-containing films formed using silicon precursor compounds having formula A and / or B and the methods described herein have a dielectric constant of about 5 or less, or about 4 or less, or about 3.5 or less. x O y C z N v H w%, wherein Si ranges from about 10 at.% to about 40 at.%; O ranges from about 0 at.% to about 65 at.%; C ranges from about 0 at.% to about 75 at.% or about 0 at.% to about 50 at.%; n ranges from about 0 at.% to about 75 at.% or about 0 at.% to 50 at.%; and H ranges from about 0 at.% to about 50 at.%, wherein x+y+z+v+w=100 atomic weight percent, such as determined by XPS or other means. Another example of a silicon-containing film formed using silicon precursor compounds of formula A and / or B and the methods described herein is silicon carbonitride, wherein the carbon content is 1 at.% to 80 at.% as measured by XPS. And yet another example of a silicon-containing film formed using silicon precursor compounds having formulas A and B and the methods described herein is amorphous silicon, wherein the sum of nitrogen and carbon content is <10 at.%, preferably <5 at.%, and most preferably <1 at.% as measured by XPS. The ratio of nitrogen to silicon ranges from 1.20 to 1.40, preferably from 1.25 to 1.35, most preferably from 1.27 to 1.34.

[0132] As previously mentioned, the methods described herein can be used to deposit a silicon-containing film on at least a portion of a substrate. Examples of suitable substrates include, but are not limited to, silicon, SiO2, Si3N4, OSG, FSG, silicon carbide, hydrogenated silicon carbide, silicon nitride, hydrogenated silicon nitride, silicon carbonitride, hydrogenated silicon carbonitride, boron nitride, anti-reflective coatings, photoresists, germanium, germanium-containing, boron-containing, Ga / As, flexible substrates, organic polymers, porous organic and inorganic materials, metals such as copper and aluminum, and diffusion barriers such as, but not limited to, TiN, Ti(C)N, TaN, Ta(C)N, Ta, W or WN. The film is compatible with a variety of subsequent processing steps, such as, for example, chemical mechanical planarization (CMP) and anisotropic etching processes.

[0133] Applications of deposited films include, but are not limited to, computer chips, optical devices, magnetic information storage, coatings on support materials or substrates, microelectromechanical systems (MEMS), nanoelectromechanical systems, thin film transistors (TFT), light emitting diodes (LED), organic light emitting diodes (OLED), IGZO and liquid crystal displays (LCD). Potential uses of the resulting solid silicon oxide or carbon-doped silicon oxide include, but are not limited to, shallow trench isolation, interlayer dielectrics, passivation layers, etch stop layers, portions of dual spacers, and sacrificial layers for patterning.

[0134] The methods described herein provide high quality silicon oxide, silicon nitride, silicon oxynitride, carbon-doped silicon nitride, carbon-doped silicon oxynitride, or carbon-doped silicon oxide films. The term "high quality" refers to films that exhibit one or more of the following properties: a density of about 2.1 g / cc or greater, 2.2 g / cc or greater, 2.25 g / cc or greater; a wet etch rate measured in a solution of dilute HF (0.5 wt % dHF) acid having a HF to water ratio of 0.5:100; a wet etch rate of about 1.5 g / cc or greater, 1.5 g / cc or greater, 2.2 g / cc or greater, 2.25 ... or smaller, or smaller, or smaller, or smaller, or smaller, or smaller, or smaller, Or less, leakage current is about 1e-8A / cm at most 6mv / cm 2 or less; about 5e20 at / cc or less of hydrogen impurities as measured by SIMS; and combinations thereof. With respect to etch rate, thermally grown silicon oxide films have an etch rate of about 1.5 wt. % Hf. The etching rate.

[0135] In certain embodiments, one or more silicon precursor compounds having Formula A and / or B described herein can be used to form silicon- and oxygen-containing films and silicon- and nitrogen-containing films that are solid and non-porous or substantially non-porous.

[0136] The following examples illustrate the methods described herein for depositing silicon oxide films and are not intended to limit the appended claims. Example

[0137] Example 1. Synthesis of 1-chloro-1,2,3,4,5,6-hexamethylcyclotrisilazane

[0138] Under nitrogen protection, acetyl chloride (31.4 g, 0.400 mol) was added dropwise to 1-dimethylamino-1,2,3,4,5,6-hexamethylcyclotrisilazane (100 g, 0.381 mol) at 5 ° C and stirring within 1 hour. The reaction solution was allowed to slowly warm to room temperature. The reaction was repeated a second time and the two reaction solutions were combined. The N,N-dimethylacetamide by-product was removed under reduced pressure (1-2 torr, 20-35 ° C), and the crude product was purified by vacuum distillation (1.0 torr, 60-62 ° C) to obtain 159 g of + 98% purity 1-chloro-1,2,3,4,5,6-hexamethylcyclotrisilazane. The standard boiling point determined by differential scanning calorimetry (DSC) was 230 ° C. Analysis by GC-MS showed the following mass peaks: m / z=253 (M+), 239, 219, 209, 195, 179, 165, 152, 145, 138, 131, 119, 102, 93, 86, 79, 72, 59, 45.

[0139] Example 2. Synthesis of 1,3-dichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane

[0140] Under nitrogen protection, acetyl chloride (30.6 g, 0.390 mol) was added dropwise to 1,3-bis(dimethylamino)-1,2,3,4,5,6-hexamethylcyclotrisilazane (56.7 g, 0.186 mol) at 5°C and stirring over 1 hour. The reaction solution was allowed to slowly warm to room temperature. The N,N-dimethylacetamide by-product was removed under dynamic vacuum at room temperature, and the crude product was purified by vacuum distillation (0.4 torr, 52-54°C) to obtain 39.6 g of 1,3-dichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane. The standard boiling point determined by differential scanning calorimetry (DSC) was 256°C. Analysis by GC-MS showed the following mass peaks: m / z=287 (M+), 273, 252, 244, 230, 210, 199, 179, 166, 152, 145, 138, 131, 122, 106, 93, 86, 79, 72, 59, 45.

[0141] Example 3. Synthesis of 1,3,5-trichloro-1,3,5-trimethylcyclotrisilazane

[0142] A mixture of hexamethyldisilazane (5.0 g, 0.031 g), trichloromethylsilane (23.2 g, 0.155 mol) and FeCl3 (0.05 g, 0.0003 mol) was stirred in a 40 ml scintillation vial at room temperature for 3 days. The resulting reaction mixture was filtered to remove solids, and the filtrate was determined to contain unreacted trichloromethylsilane and the following products by GC-MS analysis: chlorotrimethylsilane (major), 1,1-dichloro-1,3,3,3-tetramethyldisilazane (major), 1,1,3,3-tetrachloro-1,3-dimethyldisilazane (major), 1,3,5-trichloro-1,3,5-trimethylcyclotrisilazane (minor). GC-MS showed the following mass peaks of 1,3,5-trichloro-1,3,5-trimethylcyclotrisilazane: m / z = 281 (M+), 266 (M–15), 246, 228, 214, 200, 192, 180, 171, 162, 151, 142, 137, 125, 115, 107, 101, 93, 86, 70, 63, 44.

[0143] Example 4. Synthesis of 1-bromo-1,2,3,4,5,6-hexamethylcyclotrisilazane

[0144] Under nitrogen protection, acetyl bromide (0.48 g, 0.0039 mol) was added dropwise to 1-dimethylamino-1,2,3,4,5,6-hexamethylcyclotrisilazane (1.00 g, 0.00381 mol) at room temperature with stirring. After stirring for another 30 minutes, the reaction solution was analyzed by GC-MS and found to contain 1-bromo-1,2,3,4,5,6-hexamethylcyclotrisilazane as the main product. GC-MS showed the following mass peaks: m / z=297 (M+), 285, 268, 255, 239, 219, 212, 196, 182, 175, 160, 145, 132, 118, 102, 86, 72, 59, 45.

[0145] Example 5. Synthesis of 1,3-dibromo-1,2,3,4,5,6-hexamethylcyclotrisilazane

[0146] Under nitrogen protection, acetyl bromide (0.84 g, 0.0068 mol) was added dropwise to 1,3-bis(dimethylamino)-1,2,3,4,5,6-hexamethylcyclotrisilazane (1.00 g, 0.00327 mol) at room temperature with stirring. After stirring for another hour, the reaction solution was analyzed by GC-MS and found to contain 1,3-dibromo-1,2,3,4,5,6-hexamethylcyclotrisilazane and several other products. GC-MS showed the following mass peaks: m / z=377 (M+), 371, 357, 341, 329, 313, 299, 285, 270, 256, 242, 235, 219, 206, 192, 178, 165, 146, 132, 118, 104, 86, 72, 55, 41.

[0147] Example 6. Synthesis of 1-iodo-1,2,3,4,5,6-hexamethylcyclotrisilazane

[0148] Under nitrogen protection, a 50 wt% solution of acetyl iodide (0.65 g, 0.0038 mol) in Et2O was added dropwise to a stirred solution of 1-dimethylamino-1,2,3,4,5,6-hexamethylcyclotrisilazane (1.00 g, 0.00381 mol) in Et2O (1 ml) at room temperature. After stirring for 30 minutes, the reaction solution was analyzed by GC-MS and found to contain 1-iodo-1,2,3,4,5,6-hexamethylcyclotrisilazane. GC-MS showed the following mass peaks: m / z=345 (M+), 331, 316, 301, 287, 271, 257, 244, 230, 219, 203, 189, 175, 159, 159, 145, 131, 118, 102, 86, 72, 59, 45.

[0149] Example 7. Synthesis of 1-chlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane

[0150] Under nitrogen protection, n-butyl lithium solution (2.5M in hexane, 140 ml, 0.35 mol) was added dropwise to a stirred solution of 2,2,4,4,6,6-hexamethylcyclotrisilazane (100 g, 0.456 mol) in hexane (100 ml) at 0°C through an addition funnel over 90 minutes. The reaction mixture was allowed to stir while warming to room temperature. Then, about 50 ml of Et2O was added, and the resulting solution was added dropwise to a stirred solution of dichlorosilane (25 wt %, 184 g, 0.455 mol in heptane) through an addition funnel at -30°C within 2 hours. The resulting white slurry was allowed to stir while slowly warming to room temperature. The white solid was removed by filtration, and volatiles were removed under reduced pressure (5 torr). The resulting crude concentrated liquid was found to contain 1-chlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane by GC-MS analysis. GC-MS showed the following mass peaks: m / z = 282 (M–1), 268, 252, 232, 223, 216, 208, 194, 188, 174, 160, 150, 143, 136, 130, 116, 100, 93, 86, 79, 73, 59, 45.

[0151] Example 8. Synthesis of 1-chloromethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane

[0152] Under nitrogen, a 50 wt% solution of dichloromethylsilane (0.35 g, 0.0030 mol) in hexane was added dropwise to a stirred solution of 2,2,4,4,6,6-hexamethylcyclotrisilazane (2.00 g, 0.00911 mol) and triethylamine (0.62 g, 0.0061 mol) in hexane (7 ml). After stirring for 3 hours, the white slurry was filtered to remove solids, and the resulting solution was analyzed by GC-MS and found to contain the desired product, 1-chloromethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane. GC-MS showed the following mass peaks: m / z=297 (M+), 283, 267, 247, 231, 208, 194, 189, 174, 158, 151, 141, 131, 116, 100, 93, 86, 79, 73, 59, 45.

[0153] Example 9. Synthesis of 1-chlorodimethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane

[0154] A solution of lithium-2,2,4,4,6,6-hexamethylcyclotrisilazane (0.60 g, 0.0027 mol) in toluene (3 ml) and THF (0.1 ml) was added dropwise to a stirred solution of dichlorodimethylsilane (0.39 g, 0.0030 mol) in hexane (5 ml) at room temperature under nitrogen. After additional stirring for 1 hour, the mixture was filtered to remove the white solid. The filtrate was analyzed by GC-MS and found to contain the desired product, 1-chlorodimethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane. GC-MS showed the following mass peaks: m / z=311 (M+), 297, 281, 261, 245, 228, 224, 209, 189, 172, 157, 150, 141, 131, 115, 100, 93, 86, 73, 59, 45.

[0155] Example 10. Synthesis of 1-dichloromethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane

[0156] Under nitrogen protection, a 50 wt% solution of trichloromethylsilane (0.45 g, 0.0030 mol) in hexane was added dropwise to a stirred solution of 2,2,4,4,6,6-hexamethylcyclotrisilazane (2.00 g, 0.00911 mol) and triethylamine (0.62 g, 0.0061 mol) in hexane (7 ml). After stirring overnight at room temperature, the reaction mixture was heated between 60-80 ° C for 3 hours and then continued to stir overnight. The resulting white slurry was filtered to remove solids. The filtrate was analyzed by GC-MS and found to contain the desired product 1-dichloromethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane. GC-MS showed the following mass peaks: m / z=332 (M+), 317, 301, 281, 265, 245, 229, 209, 188, 172, 151, 131, 120, 115, 100, 93, 86, 73, 63, 45.

[0157] Example 11. Synthesis of 1-dichlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane

[0158] Under nitrogen, a 50 wt % solution of trichlorosilane (0.41 g, 0.0030 mol) in hexane was added dropwise to a stirred solution of 2,2,4,4,6,6-hexamethylcyclotrisilazane (2.00 g, 0.00911 mol) and triethylamine (0.62 g, 0.0061 mol) in hexane (7 ml). After stirring overnight at room temperature, the resulting white slurry was filtered to remove solids. The filtrate was analyzed by GC-MS and found to contain the desired product, 1-dichlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane. GC-MS showed the following mass peaks: m / z=317 (M+), 305, 287, 267, 251, 244, 229, 224, 214, 209, 194, 188, 179, 173, 158, 150, 144, 131, 120, 115, 100, 93, 86, 73, 59, 43.

[0159] Example 12. Synthesis of 1-trichlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane

[0160] Under nitrogen protection, a 50 wt% solution of silicon tetrachloride (0.52 g, 0.0031 mol) in hexane was added dropwise to a stirred solution of 2,2,4,4,6,6-hexamethylcyclotrisilazane (2.00 g, 0.00911 mol) and triethylamine (0.62 g, 0.0061 mol) in hexane (7 ml). After stirring at room temperature for 3 days, the resulting white slurry was filtered to remove solids. The filtrate was analyzed by GC-MS and found to contain the desired product 1-trichlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane. GC-MS showed the following mass peaks: m / z=352 (M+), 339, 322, 301, 287, 265, 248, 228, 209, 193, 172, 162, 150, 143, 131, 122, 113, 100, 93, 86, 73, 63, 45.

[0161] Unless otherwise stated, for the following examples, PEALD was performed on a commercial side flow reactor (300mm PEALD equipment manufactured by ASM) equipped with 13.56MHz direct plasma capability. Argon was used to maintain the reactor pressure. The thermal ALD process was performed on a commercial screening equipment manufactured by Picosun. In both cases, the precursor was a liquid maintained in a stainless steel bubbler and delivered to the chamber along with an Ar carrier gas. Unless otherwise stated, for the following examples, the thermal ALD process was performed on a commercial screening equipment manufactured by Picosun. The silicon precursor was delivered to the chamber by an Ar carrier gas with a flow rate of 200sccm. All gases (e.g., purge and reactant gases and precursors) were preheated to 100°C prior to entering the deposition area. Gas and precursor flow rates were controlled using an ALD diaphragm valve with high-speed actuation.

[0162] All depositions reported in the examples were performed on Si substrates containing native oxides. Film thickness and refractive index were measured using a FilmTek 3000SE ellipsometer. Growth rate per cycle (GPC) was calculated by dividing the measured thickness of the resulting silicon-containing and nitrogen-containing films by the total ALD / PEALD cycle number.

[0163] Example 13. Deposition of silicon and nitrogen containing films using 1-chloro-1,2,3,4,5,6-hexamethylcyclotrisilazane

[0164] Silicon and nitrogen containing films were deposited using 1-chloro-1,2,3,4,5,6-hexamethylcyclotrisilazane as silicon precursor and NH3 plasma under process conditions in a PEALD 300mm reactor. The silicon precursor was delivered from a stainless steel container at 100°C. Argon was used as carrier gas and was set to 200 sccm. The susceptor temperature was set to 300°C.

[0165] Table 2: Deposition parameters of PEALD silicon- and nitrogen-containing films using 1-chloro-1,2,3,4,5,6-hexamethylcyclotrisilazane

[0166]

[0167]

[0168] Repeat steps 3 to 6 multiple times to obtain silicon- and nitrogen-containing films of desired thickness. The film growth per cycle (GPC) is / cycle. It has a reflection index of 1.85. The composition of the obtained film was analyzed by X-ray photoelectron spectroscopy (XPS). The bulk film contains 40.8at.% Si, 52.3at.% N, 5at.% O and 1.3at.% C. The ratio of nitrogen to silicon is 1.28, which is very close to the ratio of 1.33 of stoichiometric silicon nitride of formula Si3N4, indicating that halogen-functionalized cyclotrisilazane with at least 3 silicon atoms and Si3N3 6-membered ring is suitable for producing stoichiometric silicon nitride. The deposited film has 5E-9A / cm at 1MV / cm 2 For comparison, Si- and N-containing films were deposited using SiCl4 and NH3 plasmas using the process parameters described in Table 2. The as-deposited films had a leakage current density of 5E-5 A / cm at 1 MV / cm. 2 This indicates that the film quality is much lower than that of the film from 1-chloro-1,2,3,4,5,6-hexamethylcyclotrisilazane.

[0169] Example 14. Thermal ALD deposition of silicon- and nitrogen-containing films using 1,3-dichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane and ammonia.

[0170] Silicon- and nitrogen-containing films were thermally deposited in a Picosun ALD screening tool using 1,3-dichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane and NH3. The precursors were delivered from a stainless steel container at 100°C. The substrate temperature was set to 600°C. The ALD steps are shown in Table 3.

[0171] Table 3: Thermal ALD deposition process for silicon- and nitrogen-containing films using Picosun ALD screening equipment

[0172]

[0173] Repeat steps 4 to 7 multiple times to obtain the desired thickness. The resulting silicon- and nitrogen-containing film is / cycle GPC deposition.

[0174] Example 15. Deposition of silicon- and nitrogen-containing films using 1,3,5-trichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane

[0175] The silicon- and nitrogen-containing films were deposited using 1,3,5-trichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane (as silicon precursor) and NH3 plasma under process conditions in a PEALD 300mm reactor. The precursors were delivered from a stainless steel container at 100°C. Argon with a flow rate of 200sccm was used as a carrier gas. The susceptor temperature was set to 300°C. Deposition was performed according to the ALD steps and parameters listed in Table 2. Steps 3 to 6 were repeated multiple times to obtain silicon- and nitrogen-containing films of the desired thickness.

[0176] Example 16. Thermal ALD deposition of silicon-containing films using 1,3,5-trichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane and ammonia.

[0177] Silicon- and nitrogen-containing films were deposited using 1,3,5-trichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane and ammonia using a Picosun ALD screening tool. The precursors were delivered from a stainless steel container at 100°C. The process parameters were set to 600°C. Deposition was performed according to the ALD steps and parameters listed in Table 3.

[0178] Repeat steps 4 to 7 as many times as necessary to achieve desired thickness.

[0179] The foregoing description is primarily for illustrative purposes. Although the present invention has been shown and described with respect to exemplary embodiments thereof, it will be appreciated by those skilled in the art that the foregoing and various other changes, omissions and additions to its form and details may be made without departing from the spirit and scope of the present invention.

Claims

1. A silicon precursor compound selected from formula A and B: Where R 1-6 are each independently selected from hydrogen, methyl and halogen; R 7 and R 8 are each independently selected from hydrogen, C 1-10 Straight chain alkyl, C 3-10 Branched alkyl, C 3-10 Cycloalkyl, C 2-10 Alkenyl, C 4-10 Aryl and C 4-10 Heterocyclic group; R 9-11 are each independently selected from hydrogen, C 1-10 Straight chain alkyl, C 3-10 Branched alkyl, C 3-10 Cycloalkyl, C 2-10 Alkenyl, C 4-10 Aryl, C 4-10 Heterocyclic group and halogen, wherein the substituent R 1-11 Two or more of the substituents R in formula A may be unconnected or connected to form a substituted or unsubstituted, saturated or unsaturated cyclic group, wherein the substituent R in formula A 1-6 At least one of them is halogen, wherein R 7 and R 8 cannot all be hydrogen, and the substituent R in formula B 9-11 At least one of them is a halogen.

2. The compound of claim 1, wherein at least one of the silicon precursor compounds comprises a 1-chlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, a 1-bromosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, a 1-iodosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, a 1-dichlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, a 1-trichlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, a 1-chloromethylsilyl-2,2, 4,4,6,6-hexamethylcyclotrisilazane, 1-chlorodimethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-dichloromethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-chloro-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,2-dichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3,5-trichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3,5-trichloro-2,4,6-trimethylcyclotrisilazane, 1,1,3, 3,5,5-hexachloro-2,4,6-trimethylcyclotrisilazane, 1-chloro-2,4,6-triethylcyclotrisilazane, 1,3-dichloro-2,4,6-triethylcyclotrisilazane, 1,3,5-trichloro-2,4,6-triethylcyclotrisilazane, 1,1,3,3,5,5-hexachloro-2,4,6-triethylcyclotrisilazane, 1-chloro-2,4,6-tri-isopropylcyclotrisilazane, 1,3-dichloro-2,4,6-tri-isopropylcyclotrisilazane, 1,3,5-trichloro-2,4,6-tri-isopropylcyclotrisilazane, 1,1, At least one of 3,3,5,5-hexachloro-2,4,6-tri-isopropylcyclotrisilazane, 1-bromo-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3-dibromo-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3,5-tribromo-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3,5-tribromo-2,4,6-trimethylcyclotrisilazane, 1-iodo-1,2,3,4,5,6-hexamethylcyclotrisilazane and 1,3-diiodo-1,2,3,4,5,6-hexamethylcyclotrisilazane.

3. A composition comprising at least one silicon precursor compound selected from the group consisting of formula A and B: Where R 1-6 are each independently selected from hydrogen, methyl and halogen; R 7 and R 8 are each independently selected from hydrogen, C 1-10 Straight chain alkyl, C 3-10 Branched alkyl, C 3-10 Cycloalkyl, C 2-10 Alkenyl, C 4-10 Aryl and C 4-10 Heterocyclic group; R 9-11 are each independently selected from hydrogen, C 1-10 Straight chain alkyl, C 3-10 Branched alkyl, C 3-10 Cycloalkyl, C 2-10 Alkenyl, C 4-10 Aryl, C 4-10 Heterocyclic group and halogen, wherein the substituent R 1-11 Two or more of the substituents R in formula A may be linked to form a substituted or unsubstituted, saturated or unsaturated cyclic group, wherein the substituent R in formula A 1-6 At least one of them is halogen, wherein R 7 and R 8 cannot all be hydrogen, and the substituent R in formula B 9-11 At least one of them is a halogen.

4. The composition of claim 3, further comprising at least one purge gas.

5. The composition of claim 3, further comprising a solvent.

6. The composition of claim 3, wherein the at least one silicon precursor compound selected from formula A and B comprises a compound selected from the group consisting of 1-chlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-bromosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-iodosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-dichlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-trichlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-chloromethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane. 1-chlorodimethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-dichloromethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-chloro-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,2-dichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3,5-trichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3,5-trichloro-2,4,6-trimethylcyclotrisilazane, 1, 1,3,3,5,5-hexachloro-2,4,6-trimethylcyclotrisilazane, 1-chloro-2,4,6-triethylcyclotrisilazane, 1,3-dichloro-2,4,6-triethylcyclotrisilazane, 1,3,5-trichloro-2,4,6-triethylcyclotrisilazane, 1,1,3,3,5,5-hexachloro-2,4,6-triethylcyclotrisilazane, 1-chloro-2,4,6-tri-isopropylcyclotrisilazane, 1,3-dichloro-2,4,6-tri-isopropylcyclotrisilazane, 1,3,5-trichloro-2,4,6-tri-isopropylcyclotrisilazane, 1, At least one of 1,3,3,5,5-hexachloro-2,4,6-tri-isopropylcyclotrisilazane, 1-bromo-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3-dibromo-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3,5-tribromo-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3,5-tribromo-2,4,6-trimethylcyclotrisilazane, 1-iodo-1,2,3,4,5,6-hexamethylcyclotrisilazane and 1,3-diiodo-1,2,3,4,5,6-hexamethylcyclotrisilazane.

7. A method for depositing a silicon-containing film on a substrate, the method The following steps are involved: a) providing a substrate in a reactor; b) introducing into the reactor at least one silicon precursor compound as claimed in claim 1; c) purging the reactor with a purge gas; d) introducing an oxygen-containing or nitrogen-containing source (or a combination thereof) into the reactor; and e) purging the reactor with a purge gas, wherein steps b to e are repeated until a film of desired thickness is deposited, and wherein the process is carried out in the reactor at one or more temperatures ranging from about 25°C to 600°C.

8. The method of claim 7, wherein the at least one silicon precursor compound is selected from the group consisting of 1-chlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-bromosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-iodosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-dichlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-trichlorosilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-chloromethylsilyl-2,2, 4,4,6,6-hexamethylcyclotrisilazane, 1-chlorodimethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-dichloromethylsilyl-2,2,4,4,6,6-hexamethylcyclotrisilazane, 1-chloro-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,2-dichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3,5-trichloro-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3,5-trichloro-2,4,6-trimethylcyclotrisilazane, 1,1, 3,3,5,5-hexachloro-2,4,6-trimethylcyclotrisilazane, 1-chloro-2,4,6-triethylcyclotrisilazane, 1,3-dichloro-2,4,6-triethylcyclotrisilazane, 1,3,5-trichloro-2,4,6-triethylcyclotrisilazane, 1,1,3,3,5,5-hexachloro-2,4,6-triethylcyclotrisilazane, 1-chloro-2,4,6-tri-isopropylcyclotrisilazane, 1,3-dichloro-2,4,6-tri-isopropylcyclotrisilazane, 1,3,5-trichloro-2,4,6-tri-isopropylcyclotrisilazane, 1,1,3,3,5,5-Hexachloro-2,4,6-tri-isopropylcyclotrisilazane, 1-bromo-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3-dibromo-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3,5-tribromo-1,2,3,4,5,6-hexamethylcyclotrisilazane, 1,3,5-tribromo-2,4,6-trimethylcyclotrisilazane, 1-iodo-1,2,3,4,5,6-hexamethylcyclotrisilazane and 1,3-diiodo-1,2,3,4,5,6-hexamethylcyclotrisilazane.

9. The method of claim 7, wherein the oxygen-containing source is selected from the group consisting of ozone, oxygen plasma, plasma comprising oxygen and argon, plasma comprising oxygen and helium, ozone plasma, water plasma, nitrous oxide plasma, carbon dioxide plasma, and combinations thereof.

10. The method of claim 7, wherein the nitrogen-containing source is selected from the group consisting of ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine, nitrogen, nitrogen / hydrogen, nitrogen / argon plasma, nitrogen / helium plasma, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, organic amines such as tert-butylamine, dimethylamine, diethylamine, isopropylamine, diethylamine plasma, dimethylamine plasma, trimethylamine plasma, trimethylamine plasma, ethylenediamine plasma, and alkoxyamines such as ethanolamine plasma, and mixtures thereof.

11. The method of claim 7, wherein the oxygen-containing source and / or the nitrogen-containing source comprises a plasma.

12. The method of claim 11, wherein the plasma is generated in situ.

13. The method of claim 11, wherein the plasma is remotely generated.

14. The method of claim 7, wherein the film has a density of about 2.1 g / cc or more.

15. The method of claim 7, wherein the film further comprises carbon.

16. The method of claim 7, wherein the film has a density of about 1.8 g / cc or more.

17. The method of claim 7, wherein the carbon content of the film is 0.5 atomic weight percent (at. %) or more as measured by X-ray photoelectron spectroscopy.

18. The method of claim 7, wherein the film has a 5E-9 A / cm at 1 MV / cm 2 or lower leakage current density.

19. A silicon-containing film formed by the method of claim 7.

20. A silicon-containing film formed by the method of claim 11.

21. A silicon precursor composition for vapor deposition of a silicon-containing film selected from the group consisting of formula A and B: Where R 1-6 are each independently selected from hydrogen, methyl and halogen; R 7 and R 8 are each independently selected from hydrogen, C 1-10 Straight chain alkyl, C 3-10 Branched alkyl, C 3-10 Cycloalkyl, C 2-10 Alkenyl, C 4-10 Aryl and C 4-10 Heterocyclic group; R 9-11 are each independently selected from hydrogen, C 1-10 Straight chain alkyl, C 3-10 Branched alkyl, C 3-10 Cycloalkyl, C 2-10 Alkenyl, C 4-10 Aryl, C 4-10 Heterocyclic group and halogen, wherein the substituent R 1-11 Two or more of the substituents R in formula A may be unconnected or connected to form a substituted or unsubstituted, saturated or unsaturated cyclic group, wherein the substituent R in formula A 1-6 At least one of them is halogen, wherein R 7 and R 8 cannot all be hydrogen, and the substituent R in formula B 9-11 At least one of them is a halogen.