Cadmium selenide-based photovoltaic devices and methods of forming same
By controlling the deposition and processing conditions of the cadmium selenide layer, efficient absorber layers and hole contacts are formed, which solves the problem of low efficiency of thin-film photovoltaic devices and achieves higher solar energy capture and conversion efficiency.
Patent Information
- Application Number
- CN202280092447.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-23
- Filing Date
- 2022-12-23
- Publication Date
- 2024-10-15
AI Technical Summary
Existing thin-film photovoltaic devices have problems with low efficiency and large absorption losses when absorbing solar radiation, making it difficult to capture or recover the maximum amount of solar radiation.
By controlling the deposition and processing conditions of the cadmium selenide (CdSe) layer, a polycrystalline film with uniform grain size and orientation is formed, reducing selenium vacancies, improving n-type charge carrier concentration and hole lifetime, and improving the performance of halogen compounds Medium heating to diffuse halogens, reduce the amount of halogens, and form efficient absorption layers and hole contacts to improve the performance of photovoltaic devices.
It is achieved to improve the conversion efficiency of photovoltaic devices, increase carrier lifetime and uniformity, reduce delamination tendency, and improve the overall performance of photovoltaic devices.
Smart Images

Figure HDA0005007367620000011 
Figure HDA0005007367620000021 
Figure HDA0005007367620000031
Abstract
Description
[0001] background
[0002] Photovoltaic devices generate electricity by converting light into direct current using semiconductor materials that exhibit the photovoltaic effect. The photovoltaic effect generates electricity when exposed to light because photons are absorbed within the semiconductor material, exciting electrons to higher energy states. These excited electrons are then able to move within the material, generating an electric current.
[0003] Thin film photovoltaic devices are typically made of layers of various different materials formed on a substrate, each layer having a different function. Thin film photovoltaic devices include front and back electrodes to provide electrical access to the photoactive semiconductor layer or to other layers sandwiched therebetween.
[0004] While many improvements have been developed to continually increase conversion efficiency, there remains a continuing need for improved thin film PV devices that minimize absorption losses while capturing or recycling the maximum amount of solar radiation practicable. BRIEF DESCRIPTION OF THE DRAWINGS
[0005] The embodiments illustrated in the drawings are schematic and exemplary in nature and are not intended to limit the subject matter defined by the claims. The following detailed description of the illustrative embodiments may be understood when read in conjunction with the following drawings, in which like reference numerals designate identical or corresponding parts throughout the views. The patent or application file may contain at least one drawing and / or one or more photographs executed in color. Copies of this patent or patent application publication with color drawing(s) will be provided by the Office upon request and payment of the necessary fee.
[0006] Figure 1 Schematically depicted is a cross-sectional view of a tandem photovoltaic device according to one or more embodiments shown and described herein.
[0007] Figure 2 Schematically depicts a schematic diagram of a system according to one or more embodiments shown and described herein. Figure 1 Example submodule of a photovoltaic device.
[0008] Figure 3A , Figure 3B and Figure 3C Schematically depicts a method according to one or more embodiments described herein. Figure 2 A cross-sectional view of a photovoltaic submodule along 3-3.
[0009] Figure 4 A substrate according to one or more embodiments shown and described herein is schematically depicted.
[0010] Figure 5 Schematically depicts a schematic diagram of a system according to one or more embodiments shown and described herein. Figure 1Cross-sectional view of a tandem photovoltaic device.
[0011] Figure 6 Schematically depicted is a cross-sectional view of a layer stack according to one or more embodiments shown and described herein.
[0012] Figure 7 Depicted are example methods according to one or more embodiments shown and described herein.
[0013] Figure 8 Plotted are transient curves of the time resolved photoluminescence intensity (TRPL) of a CdSe layer produced according to the described method.
[0014] Fig.9A , Fig. 9B and Fig. 9C An image of the processed layer is depicted.
[0015] Fig.10 Plotted are contour plots showing the logarithm of the fractional grain orientation ratio estimated from electron backscatter diffraction (EBSD) and illustrating the crystal orientation resulting from selected deposition and processing conditions.
[0016] Fig.11 Shown are measured values of O- and O2- normalized to Se- measured by time-of-flight secondary ion mass spectrometry (TOF-SIMS).
[0017] Fig.12 An image of Cl − measured by TOF-SIMS in a sample of the treated film is shown.
[0018] Fig.13 An image of O − measured by TOF-SIMS in a sample of the treated film is shown.
[0019] Fig.14 A comparison of the photoluminescence spectra of films treated with and without Se is shown.
[0020] Fig.15 Plotted are the time resolved photoluminescence intensity (TRPL) transients of CdSe layers produced with and without Se treatment.
[0021] Fig.16 Plotted are the carrier density versus depletion width relationships derived from capacitance-voltage measurements of CdSe layers produced with and without Se treatment.
[0022] Fig.17 Plotted are the changes in x-ray fluorescence spectroscopy counts before and after CHT treatment for CdSe layers produced with and without Se treatment.
[0023] Fig.18 The change in apparent charge carrier density concentration in the film corresponding to the treatment process is shown. DETAILED DESCRIPTION
[0024] Structures and compositions for use in photovoltaic (PV) devices are provided. Embodiments provide absorber layers comprising or consisting essentially of cadmium selenide.
[0025] Cadmium selenide (CdSe) layers can be formed by physical vapor deposition techniques. These deposition techniques produce as-deposited polycrystalline films with grain sizes that are smaller than desired. Annealing can be used to increase the grain size, however, because selenium evaporates at a lower temperature than cadmium and selenium can react or combine with other gases that may be present during the annealing process, some existing annealing techniques may produce an undesirable number of selenium vacancies (V vacancies) in the crystal lattice of the resulting polycrystalline film. Se ). Improved layers and photovoltaic devices can be produced by controlling aspects of the deposition process, post-deposition processing, and device fabrication.
[0026] CdSe-based absorber layers can be used in the upper submodule of a tandem module. Various embodiments and material selections for manufacturing high-performance devices are provided herein. The embodiments provided herein relate to aspects of high-quality CdSe-based solar cells, including: the effect of material quality on performance, the formation of pn junctions, and the architecture of n-type CdSe absorbers. By controlling a combination of factors, the regulation of polycrystalline grain quality in cadmium selenide can be achieved. These factors include deposition conditions and post-deposition treatment. The CdSe layer can be n-type. An absorber layer comprising n-type CdSe can form a pn junction with a hole contact comprising a p-type layer having a high band gap and a large work function.
[0027] When the conditions are controlled according to the described method, the properties of the resulting polycrystalline film will be improved. The exemplary method can be used to produce polycrystalline films having an average grain size of about 1.3 μm to 3.0 μm, incorporation of oxygen dopants, increased uniformity of grain size and orientation, selenium vacancies (V Se ) is reduced and the ratio of grains with (103) lattice orientation relative to grains with (002) lattice orientation changes. Devices incorporating the film can exhibit improved efficiency, 13 Up to 1x10 17 The present invention has an average n-type charge carrier concentration in the range of 50 Å to 100 Å, an average minority p-type charge carrier lifetime of greater than 1 nanosecond (ns), and a reduced tendency to delamination.
[0028] According to embodiments provided herein, a photovoltaic device may include an absorber layer and a hole contact. The absorber layer may include CdSe. The absorber layer may be n-type. The hole contact may form a pn junction with the absorber layer.
[0029] According to the embodiments provided herein, the tandem photovoltaic device may include an upper submodule on top of a lower submodule. The upper submodule may include an absorption layer and a hole contact. The absorption layer of the upper submodule may include CdSe. The absorption layer may be n-type. The hole contact may form a pn junction with the absorption layer.
[0030] According to the embodiments provided herein, the method of forming a photovoltaic device may include heating an absorber layer consisting essentially of CdSe in the presence of a halogen compound. The grain size of the absorber layer may grow and the halogen may diffuse into the absorber layer. After the halogen diffuses, the absorber layer may be heated in air to reduce the amount of halogen from the absorber layer. After the presence or removal of the amount of halogen, the absorber layer may be heated in a Se environment to fill the vacancies in the absorber layer.
[0031] According to the embodiments provided herein, a method for forming a photovoltaic device may include depositing a layer of CdSe on a layer stack by vapor transport deposition, and treating the layer to change its properties. Treating the layer may include contacting the CdSe layer with a halogen compound and optionally a promoter, and heating the CdSe layer on the layer stack in a controlled environment. The controlled environment may include selenium, oxygen, and nitrogen. The method may include forming a CdSe layer on a buffer layer of the layer stack and in contact with the buffer layer of the layer stack. The method may include forming a hole transport layer (HTL) on the CdSe layer and in contact with the CdSe layer.
[0032] Embodiments of the present technology relate to a tandem photovoltaic device comprising a first submodule and a second submodule; however, it should be recognized that such a tandem photovoltaic device may include additional submodules and additional submodule arrangements. The submodules in the tandem photovoltaic device can be stacked and separated by an interlayer. Incident electromagnetic radiation or light enters the device through the front surface or top surface and enters the upper submodule. Light not absorbed by the upper submodule can be transmitted to the back cell or the lower submodule. Multi-junction solar cells can achieve a higher overall conversion efficiency than single-junction cells by capturing a larger portion of the solar spectrum. These devices can be formed with materials having different bandgap properties that respond to different spectral ranges. For devices in which the primary light source comes from above, the light incident on the uppermost cell can have a large bandgap to capture high-energy short wavelengths, while the lower cell can have a smaller bandgap to capture longer wavelengths and reflected photons.
[0033] Tandem photovoltaic devices can include bifacial devices that are configured to receive incident radiation through both the front and rear surfaces. Bifacial tandem devices can be configured to receive direct solar radiation on the top or front surface and to receive radiation reflected from the external surface, including visible light and infrared light, on the back or rear surface.
[0034] Tandem photovoltaic devices can generate electricity by converting light into direct current using semiconductor materials that exhibit the photovoltaic effect. The photovoltaic effect generates electricity when exposed to light because photons are absorbed within the semiconductor material to excite electrons to a higher energy state. These excited electrons can move within the material, thereby generating an electric current. Each submodule of a tandem device can contain one or more semiconductor materials. Semiconductor materials suitable for use in photovoltaic devices can include, for example, II-VI type materials, including cadmium selenide and cadmium telluride alloys; III-V type materials, including GaAs and InGaN; I-III-VI type materials, including CIGS and CIS materials; and silicon, including amorphous silicon a-Si; and perovskites, including organic-inorganic ABX 3 Material.
[0035] The term "light" may refer to various wavelengths of the electromagnetic spectrum, such as, but not limited to, wavelengths in the ultraviolet (UV), infrared (IR), and visible portions of the electromagnetic spectrum. As used herein, "sunlight" refers to light emitted by the sun.
[0036] The term "layer" may refer to a thickness of material disposed on a surface. A layer may cover all or part of the surface. A layer may include sub-layers and may have a composition gradient within a layer. A layer may include one or more functional layers of material.
[0037] Unless otherwise stated, the values of material properties correspond to the conditions at normal temperature and pressure, 20 degrees Celsius and 1 atmosphere.
[0038] Unless otherwise stated, the values provided for ranges are inclusive of the endpoints and include all different values and further subdivided ranges within the entire range.
[0039] Although the term first, second, third, etc. can be used herein to describe various elements, components, regions, layers and / or sections, these elements, components, regions, layers and / or sections should not be limited by these terms. These terms may only be used to distinguish an element, component, region, layer or section from another region, layer or section. Unless the context clearly indicates, terms such as "first", "second" and other numerical terms do not mean order or sequence when used in this article. Therefore, without departing from the teaching of the exemplary embodiment, the first element, component, region, layer or section discussed below can be referred to as the second element, component, region, layer or section.
[0040] With respect to the disclosed methods, the order of steps presented is exemplary in nature, and thus, unless expressly stated otherwise, the order of steps may differ in various embodiments, including instances where certain steps may be performed simultaneously.
[0041] When an element or layer is referred to as being "on," "engaged to," "connected to," or "coupled to" another element or layer, it may be directly on, engaged, connected, or coupled to the other element or layer, or there may be intervening elements or layers. Conversely, when an element is referred to as being "directly on," "directly engaged to," "directly connected to," or "directly coupled to" another element or layer, there may be no intervening elements or layers. Other words used to describe the relationship between elements should be interpreted in a similar manner (e.g., "between" versus "directly between," "adjacent" versus "directly adjacent," etc.). As used herein, the term "and / or" includes any and all combinations of one or more associated listed items. As used herein, "a" and "an" indicate that there is "at least one" of the items described; where possible, there may be multiple such items.
[0042] For ease of description, spatially relative terms such as "inside," "outside," "below," "below," "lower," "above," "upper," etc. may be used herein to describe the relationship of one element or feature to another element or features as illustrated in the accompanying drawings. In addition to the orientations depicted in the figures, spatially relative terms may also be intended to cover different orientations of the device during manufacturing or in use or operation. For example, if the device in the figure is flipped, elements described as being "below" or "beneath" other elements or features will be oriented "above" the other elements or features. The device can be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially relative descriptors used herein are interpreted accordingly.
[0043] As used herein, the term "absorbing layer" refers to a semiconducting layer in which absorption of electromagnetic radiation causes electrons in the absorbing layer to be excited from a lower energy "ground state" or "valence band" where the electrons are bound to specific atoms in the solid to a higher "excited state" or "conduction band" where the electrons can move within the solid.
[0044] As used herein, an "n-type layer" refers to a semiconductor layer having an electron donor that provides an excess of electrons as majority carriers in the conduction band, while a "p-type layer" refers to a semiconductor layer having an electron acceptor that results in insufficient electrons (also referred to as excess "holes") as majority carriers in the valence band. In each case, the excess carriers (electrons or holes) can be provided by chemically doping the semiconductor with a suitable dopant, or can be generated by intrinsic properties and defects present in the material. For a junction pair in a PV device, the n-type and p-type layers or materials are joined together to form a pn junction.
[0045] Semiconductors doped as p-type or n-type are sometimes also characterized based on the density of the corresponding majority charge carriers. Although the boundaries are not strict, if the electron acceptor carriers (i.e., "holes") are approximately 1 x 10 11 cm -3 About 1x 10 17 cm -3 If the acceptor carrier density is greater than about 1×10 17 cm -3 , then the material is usually considered to be of p+ type. Similarly, if the electron donor charge is about 1x 10 11 cm -3 About 1x10 17 cm -3 If the donor carrier density is greater than about 1×10 17 cm -3 , then the material is considered to be n+ type. The boundaries are not strict and can overlap, since a layer can be p+ relative to a layer that is p-type (or n+ relative to a layer that is n-type) if the carrier concentration is at least 2 orders of magnitude higher (i.e., 100 times higher), regardless of the absolute carrier density. Alternatively, some consider that greater than about 1 x 10 19 cm -3 and therefore, a layer of n-type or p-type can be "++" relative to a layer of the same type which itself is "+" relative to a third layer, provided that the ++ layer has a carrier density of the same type exceeding 100 times that of the + layer.
[0046] Turning now to the drawings, reference is made to Figure 1 and Figure 5 , which shows one embodiment of a tandem photovoltaic device 300. The tandem photovoltaic device 300 can be configured to receive light and convert the light into electrical energy because photons are absorbed from the light and converted into current via the photovoltaic effect. For discussion and clarity, the tandem photovoltaic device 300 can define a front side 302, which is configured to face a primary light source, such as the sun. In addition, the tandem photovoltaic device 300 can also define a back side 304, which is offset from the front side 302, such as a plurality of material functional layers.
[0047] The tandem photovoltaic device 300 may have an upper submodule 100, a lower submodule 500, and an interlayer 400 therebetween. The upper submodule 100 may also be referred to as a top cell, a front cell, or a first submodule. The lower submodule 500 may also be referred to as a bottom cell, a back cell, or a second submodule. The interlayer 400 may also be referred to as an interlayer stack, a dielectric stack, or a transparent coupling layer. Each of the upper submodule 100, the lower submodule 500, and the interlayer 400 may include multiple layers. Each of the upper and lower submodules 100, 500 of the tandem photovoltaic device 300 may include one or more absorption layers for converting light into charge carriers, and a conductive layer for collecting charge carriers.
[0048] The upper submodule 100 may have a first surface 102 that generally faces the front side 302 of the tandem photovoltaic device 300 and a second surface 104 that generally faces the back side 304 of the photovoltaic device 300. The interlayer 400 may have a first surface 402 that generally faces the front side 302 of the photovoltaic device 300 and a second surface 404 that generally faces the back side 304 of the photovoltaic device 300. The lower submodule 500 may have a first surface 502 that generally faces the front side 302 of the photovoltaic device 300 and a second surface 504 that generally faces the back side 304 of the photovoltaic device 300.
[0049] like Figure 1 As shown in FIG. 1 , incident light (HV) 10 can enter the front side 302 of the tandem photovoltaic device 300 through the upper submodule 100, and a first portion 11 of the light energy can be absorbed by the upper submodule 100, while the remaining portion 12 of the light energy can pass through the upper submodule 100 to the interlayer 400. At the interlayer 400, the reflected light 13 can be directed back to the absorption region of the upper submodule 100, while the transmitted light 14 can be passed to the lower submodule 500. Optionally, in a bifacial tandem device, backside light energy 16 can enter the back side 304 of the tandem photovoltaic device 300 toward the lower submodule 500. In many embodiments, the backside light energy 16 can include visible light and near infrared light reflected from the outside. The upper submodule can absorb the first portion 11 of the light energy, which can include an absorption combination of the incident light 10 and the reflected light 13. The lower submodule can absorb the second portion 15 of the light energy, which includes the transmitted light 14 and optionally the backside light energy 16.
[0050] Reference now Figure 2, an example embodiment of an upper submodule 100 of a tandem photovoltaic device 300 is shown. The upper submodule 100 may include a plurality of layers disposed between a front side 102 and a back side 104. In some embodiments, the layers of the upper submodule 100 may be divided into an array of photovoltaic cells 200. For example, the upper submodule 100 may be scribed according to a plurality of serial scribe lines 202 and a plurality of parallel scribe lines 204. The serial scribe lines 202 may extend along a length Y of the upper submodule 100 and delimit the boundaries of the photovoltaic cells 200 along the length Y of the upper submodule 100. Adjacent cells of the photovoltaic cells 200 may be connected in series along a width X of the upper submodule 100. In other words, a monolithic interconnection of adjacent cells 200 may be formed; for example, adjacent to the serial scribe lines 202. The parallel scribe lines 204 may extend along a width X of the upper submodule 100 and delimit the boundaries of the photovoltaic cells 200 along the width X of the upper submodule 100. In operation, current 205 can flow primarily along width X through photovoltaic cells 200 connected in series by serial scribe lines 202. In operation, parallel scribe lines 204 can limit the ability of current 205 to flow along length Y. Parallel scribe lines 204 are optional and can be configured to separate serially connected photovoltaic cells 200 into groups 206 arranged along length Y.
[0051] Continue to refer Figure 2 , parallel scribe lines 204 can electrically isolate groups 206 of series-connected photovoltaic cells 200. In some embodiments, groups 206 of photovoltaic cells 200 can be connected in parallel, for example, via an electrical bus. Optionally, the number of parallel scribe lines 204 can be configured to limit the maximum current generated by each group 206 of photovoltaic cells 200. In some embodiments, the maximum current generated by each group 206 can be less than or equal to about 200 milliamps (mA), for example, less than or equal to about 100 mA in one embodiment, less than or equal to about 75 mA in another embodiment, or less than or equal to about 50 mA in yet another embodiment.
[0052] Steering FIG. 3A to FIG. 3C , the layers of the upper submodule 100 may include a thin film stack including a plurality of layers. The layers may be disposed on a substrate 110. The substrate 110 may be configured to facilitate transmission of light into the upper submodule 100. The substrate 110 may be disposed at a front side 102 of the upper submodule 100. The substrate 110 may have a first surface 112 that is generally facing the front side 102 of the upper submodule 100 and a second surface 114 that is generally facing the back side 104 of the upper submodule 100. One or more material layers may be disposed between the first surface 112 and the second surface 114 of the substrate 110.
[0053] Reference now Figure 4, the substrate 110 may include a transparent layer 120 having a first surface 122 substantially facing the front side 102 of the upper submodule 100 and a second surface 124 substantially facing the back side 104 of the upper submodule 100. In some embodiments, the second surface 124 of the transparent layer 120 may form the second surface 114 of the substrate 110.
[0054] The transparent layer 120 may include substantially transparent materials such as glass. Suitable glass may include soda-lime glass, or any glass with reduced iron content. In some embodiments, the transparent layer 120 may have any suitable transmittance range, including about 250nm to about 1,300nm. The transparent layer 120 may also have a certain transmittance percentage, including, for example, greater than about 50% in one embodiment, greater than about 60% in another embodiment, greater than about 70% in yet another embodiment, greater than about 80% in yet another embodiment, or greater than about 85% in yet another embodiment. In one embodiment, the transparent layer 120 may be formed by glass with a transmittance of about 90% or more. Optionally, the substrate 110 may include a coating 126 applied to the first surface 122 of the transparent layer 120. The coating 126 may be configured to interact with light or improve the durability of the substrate 110, such as, but not limited to, an anti-reflective coating, an anti-fouling coating, or a combination thereof.
[0055] Reference again Figures 3A-3C , the upper submodule 100 may include a barrier layer 130 configured to mitigate diffusion of contaminants from the substrate 110 that may cause degradation or delamination of other layers of the photovoltaic stack. The barrier layer 130 may have a first surface 132 that is generally facing the front side 102 of the upper submodule 100 and a second surface 134 that is generally facing the back side 104 of the upper submodule 100. In some embodiments, the barrier layer 130 may be disposed adjacent to the substrate 110. For example, the first surface 132 of the barrier layer 130 may be disposed above the second surface 114 of the substrate 110.
[0056] Typically, barrier layer 130 can be substantially transparent, thermally stable, have a reduced number of pinholes, have sodium blocking capabilities, and good adhesion properties. Barrier layer 130 can include one or more material layers. Example materials can include, but are not limited to: tin oxide, silicon dioxide, aluminum-doped silicon oxide, silicon oxide, silicon nitride, or aluminum oxide. Barrier layer 130 can have a thickness defined by first surface 132 and second surface 134. In one example, the barrier layer thickness can be greater than 5 nanometers (nm), equal to or greater than 10 nm, or equal to or greater than 15 nm. In one example, the barrier layer thickness can be less than or equal to 50 nm, less than 40 nm, or less than or equal to about 20 nm.
[0057] The upper submodule 100 may include an n-type contact layer 150. The n-type contact layer 150 may also be referred to as a negative charge transport layer, an n-type contact, an e-selective contact, an electron transport layer (ETL), or an electron selective layer. As a selective contact to the absorber, the layer helps guide electrons from the absorber to a high conductivity electronic contact while minimizing holes that can recombine at the contact. In addition, the layer includes a high conductivity region that allows electrons to be guided without significant series resistance. The n-type contact layer 150 may have a first surface 152 that is substantially facing the front side 102 of the upper submodule 100 and a second surface 154 that is substantially facing the back side 104 of the upper submodule. The n-type contact layer 150 has a thickness defined by the distance between the first surface 152 and the second surface 154. In some embodiments, the thickness of the n-type contact layer 150 is greater than 2 nm, in the range of 10 nm to 180 nm, or between 15 nm and 80 nm in an exemplary embodiment.
[0058] The n-type contact layer 150 may include n++ or n+ materials or a combination thereof. The n-type contact layer 150 may include a conductive oxide. In one example, the n-type contact layer 150 may include materials including but not limited to: tin dioxide, doped tin dioxide (e.g., F-SnO 2 ), indium tin oxide or cadmium tin oxide (Cd 2 SnO 4 ).
[0059] The upper submodule 100 includes an absorption layer 160, which includes a material configured to cooperate with adjacent layers to form a pn junction within the photovoltaic device. Accordingly, the absorbed photons of light can release electron-hole pairs and generate carrier flow, which can generate electricity. The absorption layer 160 can have a first surface 162 that is generally facing the front side 102 of the upper submodule 100 and a second surface 164 that is generally facing the back side 104 of the upper submodule. The thickness of the absorption layer 160 can be defined between the first surface 162 and the second surface 164. In an example device, the thickness of the absorption layer 160 can be between about 200nm and about 10000nm. In some examples, the thickness of the absorption layer 160 is equal to or greater than 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, 1100nm, 1200nm, 1300nm, 1500nm, 1600nm, 1800nm, 2000nm, 2200nm, or equal to or greater than 2400nm. In some examples, the thickness of the absorption layer 160 is less than or equal to 10000nm, 5000nm, 4000nm, 3500nm, 3000nm, 2800nm, 2500nm, 2000nm, 1800nm, 1600nm, 1500nm, 1300nm, or less than or equal to 1200nm. In one example, the absorbing layer has a thickness in a range of 700 nm to 1500 nm; in another example, the absorbing layer has a thickness in a range of 1200 nm to 2500 nm.
[0060] Absorption layer 160 may comprise a polycrystalline II-VI type thin film semiconductor in which electrons are excited to produce a photovoltaic effect. Absorption layer 160 may comprise an n-type material. The absorption layer may be n-type throughout its thickness. The absorption layer may comprise CdSe. The absorption layer may consist essentially of CdSe. The absorption layer may comprise cadmium, selenium, and one or more dopants. In some embodiments, absorption layer 160 comprises a dopant selected from oxygen, chlorine, rubidium, sulfur, bromine, fluorine, iodine, cesium, potassium, sodium, lithium, or a combination thereof.
[0061] In some embodiments, the absorbing layer has composition and structural properties that reduce the charge carrier recombination rate, increase the carrier diffusion length, and increase the carrier lifetime. These properties can include, for example, layer thickness, stoichiometry, dopant concentration, vacancy concentration, grain size, and polycrystalline structure and orientation. In some embodiments, the average carrier diffusion length is greater than 10nm, 20nm, 50nm, 70nm, 100nm, 200nm, 700nm, 800nm, 1000nm, 1200nm, or in the range of 20nm to 1500nm. In some embodiments, the average carrier lifetime is equal to or greater than 1ns, 2ns, 5ns, 10ns, 15ns, greater than 20ns, or in the range of 1ns to 100ns.
[0062] In some embodiments, the atomic concentration of oxygen in the central region 166 of the absorber layer 160 may be greater than about 1×10 16 cm -3 , for example in one embodiment at about 1×10 17 cm -3 About 5x10 20 cm -3 In another embodiment, between about 3x10 17 cm -3 About 1x10 19 cm -3 or in yet another embodiment between about 5x10 17 cm -3 About 5x10 18 cm -3 In some embodiments, the absorbent layer has a central region of 1×10 17 cm -3 Up to 1x10 19 cm -3 The central region 166 is the middle 50% of the absorber layer 160, which is offset from the first surface 162 and the second surface 164 of the absorber layer 160 by 25% of the thickness of the absorber layer 160. Alternatively or additionally, the concentration profile of oxygen can vary over the thickness of the absorber layer 160.
[0063] In some embodiments, the atomic concentration of chlorine in the central region 166 of the absorber layer 160 may be less than about 1×10 21 cm -3 , for example in one embodiment at about 1×10 17 cm -3 About 1x10 21 cm -3 In another embodiment, between about 5x10 17 cm -3About 1x10 20 cm -3 or in yet another embodiment between about 5x10 17 cm -3 About 5x10 19 cm -3 between.
[0064] The upper submodule 100 includes a hole contact 180. The hole contact 180 may also be referred to as a positive charge transport layer, a p-type contact, a hole transport material, a hole transport layer (HTL), an h+ selective contact, or a hole selective layer. The hole contact 180 provides electrical contact with the absorber layer 160. The hole contact 180 may have a first surface 182 that is generally facing the front side 102 of the upper submodule 100 and a second surface 184 that is generally facing the back side 104 of the upper submodule.
[0065] The thickness of the hole contact 180 can be defined between the first surface 182 and the second surface 184. In some embodiments, the thickness of the hole contact 180 can be between about 2 nm and about 200 nm, for example, between about 2 nm and about 100 nm.
[0066] In some embodiments, hole contact 180 is a polymer, a small molecule, or an inorganic compound. In some embodiments, hole contact 180 comprises a metal oxide or a metal oxynitride. In some embodiments, hole contact 180 comprises a transition metal oxide.
[0067] The hole contact 180 may include an organic hole transport material (HTM). In one example, the hole contact includes at least one of: poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine (PTAA); perylene diimide (PDI); 4,4′-bis(N-carbazolyl)-1,1′-biphenyl (CBP); tri(4-carbazol-9-ylphenyl)amine (TCTA); 1,3,5-tri(carbazol-9-yl)benzene (TCP); poly(9,9-dioctylfluorene-alt-benzothiadiazole) (F8BT). In another example, the hole contact consists essentially of an organic HTM selected from the group consisting of PTAA, PDI, CBP, TCTA, TCP, or F8BT.
[0068] The hole contact 180 may include an inorganic material having a good valence band alignment and a wide band gap. In one example, the hole contact includes at least one of the following: copper aluminum sulfide (CuAlS 2 ); copper aluminum selenide (CuAlSe 2 ); copper gallium oxide (CuGaO 2 ); magnesium germanium phosphide (GeMgP 2); boron phosphide (BP); gallium phosphide (GaP); zinc selenide (ZnSe); or tantalum oxynitride (TaO x N (1-x) ).
[0069] In some embodiments, the hole contact 180 comprises a p-type transparent conductive oxide. In some embodiments, the p-type transparent conductive oxide comprises at least one of the following: nickel oxide (NiO x ) or tin oxide (SnO x ). In some embodiments, the p-type transparent conductive oxide is doped with at least one of: boron (B); magnesium (Mg); nitrogen (N); antimony (Sb); or a combination thereof.
[0070] In some embodiments, the hole contact 180 includes a p-type alloy including at least one of: zinc (Zn), sulfur (S), selenium (Se); and tellurium (Te).
[0071] In some embodiments, the hole contact 180 comprises a material selected from nickel oxide (NiOx), cuprous thiocyanate (CuSCN), copper iodide (CuI), or copper oxide (Cu 2 O) of inorganic compounds.
[0072] The hole contact 180 may incorporate a material having a wide bandgap and a high work function. In some embodiments, the hole contact 180 includes a buffer sublayer and a contact sublayer. In one example, the buffer sublayer may include molybdenum sulfide (MoS x ) or tungsten sulfide (WS x In one example, the contact sublayer may include niobium disulfide (NbS 2 );Vanadium sulfide (V x S x ); vanadium(II) sulfide (VS); tantalum sulfide (TaS x ); Tantalum(IV) sulfide (TaS 2 );Titanium sulfide (Ti x S x ); Titanium(IV) sulfide (TiS 2 ); or a combination thereof.
[0073] The composition for the hole contact 180 or a sublayer for the hole contact 180 can be selected to provide buffering and ohmic contact, or to have a good work function and band gap alignment with adjacent layers. In some embodiments, the material of the hole contact 180 has a work function greater than 5 eV. The hole contact 180 can be p-type or p+ type.
[0074] The hole contact 180 may form a pn junction 176 with the absorber layer 160. The hole contact 180 may constitute a p-type layer of the pn junction 176, while the absorber layer constitutes an n-type layer of the pn junction.
[0075] The upper submodule 100 may include a transparent conductive layer 140 configured to provide electrical contact to transfer charge carriers generated by the first submodule 100. The transparent conductive layer 140 may have a first surface 142 that generally faces the front side 102 of the first submodule 100 and a second surface 144 that generally faces the back side 104 of the first submodule 100. The transparent conductive layer 140 may be located between the absorber layer and the front side 102 of the first submodule 100. In some embodiments, a p-type hole contact 180 may be located between the n-type absorber layer 160 and the transparent conductive layer 140. In some embodiments, for example, Figure 3B In some embodiments, for example, the transparent conductive layer 140 may be of p+ type. Figure 3A and 3C In the embodiment, the transparent conductive layer 140 may be of n-type or n+-type.
[0076] The upper submodule 100 may optionally include a conductive layer 190. The conductive layer 190 may have a first surface 192 that generally faces the energy side 102 of the photovoltaic device and a second surface 194 that generally faces the back side 104 of the photovoltaic device.
[0077] In some embodiments, upper submodule 100 may include a p+ / n+ tunnel junction or composite junction 175. In some embodiments, hole contact 180 may form a p+ layer of p+ / n+ junction 175. In some embodiments, n+ layer 170 may form an n+ layer of p+ / n+ junction 175.
[0078] The function of the p+ / n+ junction is twofold. First, it forces significant band bending resulting in a narrow depletion width across the p+ / n+ junction, which allows electron and hole tunneling or recombination. This process converts holes that are majority carriers in the p-contact into electrons that are majority carriers in the n+ region. The second function of the electron collecting side of the p+ / n+ junction is to provide a sufficiently low resistance for lateral transport of current, which can be achieved by the n+ or n++ portion of the TCO-like layer. These functions can be provided by a single layer, a layer with sublayers, or by using multiple n-type layers (including one or more n+ and / or n++ layers).
[0079] In some embodiments, the n+ side of the n+ / p+ junction 175 comprises a metal oxide doped n+ layer 170, and the metal oxide layer comprises at least one of the following materials: fluorine doped tin oxide (SnO 2 :F); indium tin oxide (ITO); cadmium tin oxide (Cd2 SnO 4 ); tungsten(VI) oxide (WO 3 ); Molybdenum(VI) oxide (MoO 3 ); Chromium(VI) oxide (CrO 3 ); Vanadium(V) oxide (V 2 O 5 ); or a combination thereof. In some embodiments, the n+ side of the n+ / p+ tunnel junction comprises at least one of the following materials: gallium phosphide (GaP); boron phosphide (BP); zinc selenide (ZnSe); or a combination thereof.
[0080] The photovoltaic device 100 may optionally include one or more interlayers, diffusion barrier layers, and / or one or more auxiliary buffer layers. The addition of one or more barrier layers or buffer layers may be used to inhibit the diffusion of dopants or contaminants between layers. Buffer layers may be used to reduce the number of irregularities that occur during the formation of the semiconductor. Buffer layers may be configured to provide an insulating layer between adjacent layers. Buffer layers may include materials having a higher resistivity than adjacent layers and may include, but are not limited to, intrinsic tin dioxide, zinc magnesium oxide (e.g., Zn 1-x Mg x O), tin dioxide (SnO 2 ), silicon dioxide (SiO 2 ), aluminum oxide (Al 2 O 3 ), aluminum nitride (AlN), zinc tin oxide, zinc oxide, tin silicon oxide, or a combination thereof. In some embodiments, the material of the buffer layer can be configured to substantially match the band gap of the adjacent semiconductor layer. The buffer layer can have a certain thickness, including, for example, greater than about 10 nm in one embodiment, between about 10 nm and about 80 nm in another embodiment, or in the range of 15 nm to 60 nm in yet another embodiment.
[0081] The submodule may also include additional layers and structural components including, but not limited to, one or more of: buffer layers, barrier layers, interface layers, dielectric layers, conductive layers, support layers, anti-reflective layers, scribing, packaging, bus connections, and combinations thereof.
[0082] In a substrate structured device, the device can be formed from back to front on the substrate. In a superstrate structured device, the device can be formed from front to back on the substrate.
[0083] Figure 3A An example submodule that can be fabricated as a substrate structured device is shown. In the example shown, in this example, an n-type CdSe absorber layer 160 is between and adjacent to a p-type hole contact layer 180 and an n-type contact 150 .
[0084] Figure 3B and 3C An example submodule that can be fabricated as a superstrate structured device is shown. An n-type CdSe absorber layer 160 is between a p-type hole contact layer 180 and an n-type contact 150. In the example shown, an n+ or n++ layer is provided by a transparent conductive layer 140.
[0085] Figure 3C An example submodule is illustrated in FIG. 1 . In this example, the p-type hole contact layer 180 is between the n-type CdSe absorber layer 160 and the transparent conductive layer 140. This configuration can be facilitated by using an n+ / p+ junction 175. In some embodiments, the hole contact also serves as the p+ layer of the p+ / n+ junction. Alternatively, in some embodiments, there is an additional p+ layer between the hole contact 180 and the absorber layer 160. The use of an n++ type of TCO can be selected as a practical choice because there are more compositional choices for good transparent conductive oxides of n-type rather than p-type. Therefore, for an n-type photovoltaic absorber to be used in a superstrate configuration, it may be advantageous to use an n+ / p+ junction to convert the carrier type to make a pn junction on the light entrance, the front side of the absorber. In a device provided with a good p++ layer comprising one or more materials, the structure can be simplified to a submodule architecture that is, from front to back: p++ / p+ / HTL / CdSe-n / ETL / n+ / n++.
[0086] Figure 6 A layer stack of a partially formed device is shown. The absorber stack 600 includes a substrate stack 610 and a semiconductor film 660. The absorber stack 600 may have a first surface 602 and a second or exposed surface 604. The substrate stack 610 includes a substrate layer and a plurality of layers formed on the substrate layer. The semiconductor film 660 includes a deposited absorber material. The semiconductor film 660 is provided as a layer at the surface of the absorber stack 600, and the deposited absorber precursor material may be treated to form an absorber layer. The semiconductor film 660 may have a first surface 662 or a stack contact surface, and may have a second surface or an exposed surface 664. The treatment of the deposited semiconductive layer 660 may be applied to the exposed surface 664 of the film, which corresponds to the exposed surface 604 of the absorber stack 600.
[0087] For embodiments formed in a superstrate configuration, the absorber stack 600 can have a first surface 602 that generally faces the front side 102 of the first submodule 100 and a second surface 604 that generally faces the back side 104 of the first submodule 100. The substrate stack 610 can have a first surface 612 that generally faces the front side 102 of the first submodule 100 and a second or exposed surface 614 that generally faces the back side 104 of the first submodule 100. A semiconductor film 660 comprising CdSe can be deposited over and adjacent to the substrate stack with a first surface 662 in direct contact with the second surface 614 of the substrate stack to form the absorber stack 600.
[0088] Photovoltaic devices may contain several material layers deposited sequentially on a substrate. The steps of manufacturing photovoltaic devices may include sequentially arranging functional layers or layer precursors in a "stack" of layers by one or more deposition processes, including but not limited to spin coating, spray coating, slit coating, blade coating, dip coating, sputtering, evaporation, molecular beam deposition, pyrolysis, closed space sublimation (CSS), pulsed laser deposition (PLD), chemical vapor deposition (CVD), electrochemical deposition (ECD), atomic layer deposition (ALD) or vapor transport deposition (VTD). One or more methods may be used to treat the deposited layer or layer stack to change the characteristics, such as by annealing, passivation, heating, vapor contact or chemical treatment. The manufacture of photovoltaic devices may also include selectively removing portions of certain layers of the layer stack (such as by scratching) to divide the photovoltaic device into a plurality of photovoltaic cells.
[0089] Figure 7 An example method is illustrated in The method includes providing a substrate layer stack 710; depositing a semiconductor film 720 to form an absorber stack; contacting the film with a halogen composition 730; and heating the absorber layer stack 740 in a controlled environment.
[0090] The step of providing a substrate layer stack 710 may include preparing an exposed surface 614 of the substrate stack 610. In some embodiments, the exposed surface 614 may be substantially smooth. In an exemplary method for preparing a substrate-oriented submodule, the substrate layer stack 610 has an n-type top layer that may include a buffer material and an electron transport layer having a smooth top surface 614. In an exemplary method for preparing a top-substrate-oriented submodule, the substrate layer stack 610 may include a p-type hole transport material. Optionally, the p-type hole transport material may also be a p+ layer of a p+ / n+ junction, on which a semiconductor film for forming an absorption layer is deposited.
[0091] The step of depositing the semiconductor film 720 may include depositing cadmium selenide by vapor transport deposition (VTD). It has been found that using VTD produces better quality films than other physical deposition methods. Controlling the deposition temperature can also adjust the quality of the resulting film. In one example, the layer is deposited at a temperature of about 520° C., in a range of 480-560° C., or in a range of 500-540° C. using N 2 Or N2 with a fractional oxygen percentage is deposited as a carrier gas.
[0092] The step 730 of contacting the film with a halogen composition may include contacting the film with an alkali metal halide. The step 730 of contacting the film with a halogen composition may include contacting the film with an alkali metal chloride. This step may also include contacting the film with a promoter. The contacting step may include providing the composition in the form of a liquid, a gel, or a vapor. In some embodiments, the halogen compound comprises at least one of: CdCl 2 NH 4 Cl, CdBr 2 , CdI 2 MgCl 2 or Ba(ClO 3 ) 2 In some embodiments, the promoter comprises at least one of: Li, Na, K, Rb, or Cs. In one example, the contacting step can include contacting the membrane with cadmium chloride and rubidium chloride.
[0093] The step 740 of heating the absorber layer stack in a controlled environment can include providing an oxygen-containing environment. In some embodiments, the environment contains Se. The step 740 of heating the absorber layer stack in a controlled environment can be performed after or simultaneously with the step of contacting the absorber layer stack with a halogen composition. The halogen composition may contain cadmium chloride or other chloride compounds. The step 740 of heating the absorber layer stack in a controlled environment can also be referred to as a chloride heat treatment (CHT) or annealing step. After or simultaneously with applying the halogen composition and optionally a promoter, heating in the presence of oxygen and optionally selenium can promote grain growth and diffusion of chlorides and oxygen to grain boundaries and into the absorber body or central region, and can reduce selenium vacancies in the film. The use of selenium in a controlled environment will further reduce selenium vacancies.
[0094] In some embodiments, the environment comprises an amount equal to or greater than 2%, 5%, 10%, 12%, 15%, 18%, or in a range of up to 25%, or in a range of up to 20%. 2In some embodiments, the environment comprises Se in an amount equal to or greater than 0.001%, 0.01%, 0.05%, 0.1%, 0.5%, 1.0%, in a range of up to 5.0%, or in a range of up to 2.5%, or in a range of up to 2.0%. In some embodiments, the controlled environment comprises a selenium vapor at a partial pressure in a range of 0.01 torr to 60 torr or in a range of 0.1 torr to 30 torr. In some embodiments, the controlled environment has a temperature equal to or greater than 300°C, 320°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, or 400°C. In some embodiments, the controlled environment has a temperature less than or equal to 520°C, 500°C, 490°C, 480°C, 470°C, 460°C, or 450°C. In some embodiments, the controlled environment has a temperature in a range of 380°C to 500°C. In some embodiments, the controlled environment has a temperature in the range of 380°C to 475°C. In some embodiments, the controlled environment has a temperature in the range of 400°C to 440°C. In some embodiments, the controlled environment has a pressure equal to or less than about 760 Torr (1 atm). In some embodiments, the controlled environment has a pressure in the range of 250 Torr to about 760 Torr. In some embodiments, the environment has a pressure in the range of 250 Torr to 500 Torr. In some embodiments, the environment has a pressure in the range of 1.0 Torr to 500 Torr. In some embodiments, the environment has a pressure in the range of 50 Torr to 500 Torr, wherein the partial pressure of oxygen is in the range of 1.0 Torr to 125 Torr, and the partial pressure of selenium is in the range of 0.1 Torr to 30 Torr. In some embodiments, the step of heating the absorber layer stack in a controlled environment is performed for a duration of at least 20 minutes, at least 40 minutes, at least 60 minutes, at least 90 minutes, at least 120 minutes, at least 180 minutes. In some embodiments, the step of heating the absorbent layer stack in a controlled environment is performed for a duration of less than 24 hours, less than 18 hours, less than 12 hours, less than 10 hours, less than 8 hours, less than 6 hours, less than 5 hours, less than 4 hours, or equal to or less than 3 hours. In some embodiments, the step of heating the absorbent layer stack in a controlled environment is performed for a duration of 1-6 hours. In some embodiments, the step of heating the absorbent layer stack in a controlled environment is performed for a duration of 1-3 hours.
[0095] Example absorber layers were prepared and processed using selected deposition methods and different post-deposition treatments, and the resulting absorber layers were characterized.
[0096] Figure 8Transient curves of the time-resolved photoluminescence intensity (TRPL) of CdSe films of the as-deposited and after CHT are shown. The slower TRPL transient decay indicates improved minority carrier lifetime. Line 810 shows the results for the untreated as-deposited film, line 820 shows the results after 1 hour of treatment, and line 830 shows the results after 3 hours of treatment. The lifetime of the as-deposited samples is poor. The CHT treatment process improves the lifetime, and longer treatment times provide further increases. Average lifetime: as-deposited = 0.04ns (40ps); 1 hour = 1ns; 2 hours = 2ns. Grain size also increases with increasing CHT time.
[0097] Fig.9A , Fig. 9B and Fig. 9C An optical microscope image at 100X magnification is shown and shows the growth of grains with increasing CHT time. In some embodiments, the absorber layer is a polycrystalline film having a thickness in the range of 0.25 μm to 2.0 μm and an average grain size in the range of 1.3 μm to 3.0 μm. In some embodiments, the average grain size is equal to or greater than the absorber layer thickness.
[0098] Fig.10 Orientation contours after CHT are shown, where the (hkl) Miller indices indicate the orientation of the crystal planes. Fig.10 The logarithm (log) of the ratio of (002) to (103) orientations is shown. For example, the contour line 1040 labeled 2-3 indicates that the area fraction of grains with (002) orientation is 100 to 1000 times that of (103) grains. The figure shows contour lines 1040, 1030, 1020, 1010, showing the transition of the area fraction of grains with (002) orientation relative to (103) grains. The data corresponds to samples deposited at 480°C, 520°C, or 460°C and not CHT treated or treated at 400°C or 440°C. The films, especially those deposited at 520°C, start out as (002) and become increasingly (103) as the CHT temperature and time increase. The sample deposited at 560°C (schematically on the right) is primarily (002). Without wishing to be bound by theory, it has been found that films with a higher percentage of (103) orientation may also have improved optoelectronic properties. During growth, the film is more likely to nucleate as (002), and when deposited at low temperatures, the film is more random in orientation (002)(103). During recrystallization, the orientation shifts toward (103) to reduce the surface energy.
[0099] In one example, the film has a first crystal structure as deposited, having a first predominant crystal orientation and a first average grain size. After treatment, the film has a treated second crystal structure, having a second predominant crystal orientation and a second average grain size. In some embodiments, the absorber layer is a polycrystalline film, wherein the ratio of grains having a (103) orientation relative to grains having a (002) orientation is equal to or greater than 1:1.
[0100] The concentrations of dopants and constituent elements of the absorption layer can be measured by secondary ion mass spectrometry (SIM). Fig.11 An example of a comparative absorber layer characterized by time-of-flight secondary ion mass spectrometry (ToF-SIMS) is shown.
[0101] like Fig.11 As shown in , post-deposition treatment can produce semiconductor films with altered oxygen levels in the bulk region of the layer. Post-deposition treatment adjusts the total oxygen as well as the depth of O 2 With Se and O - Ratio of Se to O detected in the absorber - With O 2 The large difference in comparison indicates the extent of oxygen incorporation into the film.
[0102] Fig.11 The comparative absorber layer samples measured by time-of-flight secondary ion mass spectrometry (TOF-SIMS) are shown in depth relative to Se - Standardized O - and O 2 Counts. The level of oxygen in the bulk region or central portion of the absorber's thickness may best illustrate changes due to processing, while the level of oxygen near the exposed surface (depth = 0) may be affected by incidental air exposure. The four lines show the results for the as-deposited layer 1110, a layer 1120 thermally treated with cadmium chloride in a nitrogen environment, a layer 1130 thermally treated with cadmium chloride in an air environment 1130, and a layer 1140 thermally treated with cadmium chloride followed by a vacuum annealing step. The graph shows that thermal treatments that promote grain growth result in a reduction in oxygen content, and that this can be improved by introducing oxygen in post-deposition processing.
[0103] Fig.12 Shown is Cl in the grain boundaries of a CdSe layer after post-deposition cadmium chloride heat treatment in an environment containing oxygen in the range of 5% to 20%. The left panel shows the image as captured and the right panel shows the same image color inverted and converted to grayscale.
[0104] Fig.13 Oxygen in the grain boundaries is shown. The left panel shows the image as captured, the right panel shows the same image color inverted and converted to grayscale. Fig.12 and13 The same sample area is shown with the same scale bar. Fig.12 and 13 The presence of both chlorine and oxygen in the film after CHT is shown, and higher concentrations of both chlorine and oxygen along the grain boundaries are shown.
[0105] Fig.14 The measurement results of CdSe semiconductor films produced with halogen treatment and selenium vapor treatment or with halogen treatment but without selenium vapor treatment are shown. Data line 1410 shows the results with Se treatment, while data line 1420 shows the results without Se treatment. The data shows that the addition of Se vapor treatment will reduce the sub-bandgap intensity and improve the optoelectronic properties.
[0106] Fig.15 Transient curves of the time-resolved photoluminescence intensity (TRPL) of a CdSe layer produced with and without post-deposition Se treatment are shown. Line 1510 shows the data corresponding to the Se treatment. Line 1520 shows the data corresponding to the control without Se treatment. As shown, the Se treatment improves TRPL, indicating an improved minority carrier lifetime.
[0107] Fig.16 Capacitance-voltage (CV) measurements of CdSe absorbers after thermal treatment are shown, where the charge carrier concentration per cubic centimeter of depth is plotted. The data set on the right shows the results after treatment in an environment containing Se, and the data set on the left shows the results after treatment without Se. The top data set shows the results after thermal treatment at about 280°C, and the bottom data set shows the results after thermal treatment at about 380°C. Se reduces the apparent doping at either Se temperature. The results show that thermal treatment in an environment containing Se will reduce Se vacancies in the polycrystalline lattice.
[0108] Fig.17 A comparison of selenium levels in the absorber layer bulk region of CdSe layer samples after cadmium chloride heat treatment at 440°C or 460°C and with (right data bar) or without (left data bar) selenium vapor is shown. The increase in Se can be detected using x-ray fluorescence. The data shows an increase in selenium in the CdSe layer for layers treated with selenium vapor treatment.
[0109] Fig.18 The apparent charge carrier concentration changes associated with the processing are shown. Annealing with cadmium chloride in a nitrogen environment produces the desired grain growth but has the detrimental effect of introducing a large number of selenium vacancies. The increase in apparent charge carrier concentration associated with a nitrogen environment is not primarily due to a change in dopant concentration but rather to an increase in selenium vacancies and corresponds to 1x10 18 cm-3 The high apparent n-type charge carrier concentration of about 1000 Å is caused by the increase of Se vacancies, which leads to a shorter carrier lifetime, increased recombination rate, and shorter carrier diffusion length, resulting in lower overall efficiency. Providing a halogen heat treatment in the presence of oxygen, or oxygen and Se, can improve defects and reduce Se vacancies. This post-deposition treatment is consistent with the apparent charge carrier concentration level of CdSe films moving toward about 1x10 16 cm -3 associated with changes in levels within a range.
[0110] The results show that post-deposition treatment of n-type CdSe absorber layers deposited by vapor transport deposition at temperatures in the range of about 400°C to about 490°C in an oxygen-containing and / or selenium-rich environment will produce devices with fewer defects, less recombination, and longer mobile charge carrier lifetimes. Thermal treatment of doped devices generally improves efficiency, increases V OC , increase short circuit current density, improve fill factor, reduce resistance, reduce shunt and improve performance.
[0111] It should now be appreciated that embodiments of the present disclosure provide n-type CdSe absorber layers and methods of making and processing absorber layers.
[0112] According to embodiments provided herein, a photovoltaic device may include an absorber layer and a back contact. The absorber layer may include cadmium and selenium.
[0113] The tandem photovoltaic device may include an upper submodule on top of a lower submodule. The upper submodule may include an absorber layer comprising cadmium and selenium or consisting essentially of CdSe, and a hole contact forming a pn junction with the absorber layer. In an embodiment, the absorber layer is n-type and has a carbon nanotube structure of less than 1×10 17 cm -3 In some embodiments, the absorption layer has an n-type carrier concentration equal to or greater than 1×10 13 cm -3 Levels of chlorine are included in the grain boundaries as measured by secondary ion mass spectrometry.
[0114] A method of forming an absorber layer for a photovoltaic device may include providing a layer stack including a p-type layer; depositing a polycrystalline film over the p-type layer, wherein the polycrystalline film includes cadmium and selenium or consists essentially of CdSe. The method may include contacting an exposed surface of the polycrystalline film with a halogen compound and optionally a promoter. The method may include heating the polycrystalline film in a controlled environment to form an absorber layer, wherein the controlled environment includes oxygen, whereby the absorber layer has a carbon content of less than 1×10 17 cm -3In some embodiments, the controlled environment comprises selenium. In some embodiments, the method produces an n-type carrier concentration equal to or greater than 1×10 13 The method produces an absorber layer of chlorine at a level of 0.0407 W / m2 in the grain boundaries as measured by secondary ion mass spectrometry. In some embodiments, the method produces an absorber layer of a polycrystalline film having an average grain size that is larger than the thickness of the film.
[0115] Although specific embodiments have been illustrated and described herein, it will be appreciated that various other changes and modifications may be made without departing from the spirit and scope of the claimed subject matter. In addition, although various aspects of the claimed subject matter have been described herein, such aspects need not be used in combination. Therefore, the appended claims are intended to cover all such changes and modifications within the scope of the claimed subject matter.
Claims
1. A tandem photovoltaic device, comprising an upper submodule on top of a lower submodule, wherein the upper submodule comprises: An absorber layer consisting essentially of CdSe, wherein: The absorber layer is n-type; The absorption layer has a thickness less than 1x10 17 cm -3 n-type carrier concentration; and The absorber layer has a density of equal to or greater than 1×10 13 cm -3 A level of chlorine is included in said grain boundaries; and A hole contact forms a pn junction with the absorption layer. 2 . The tandem photovoltaic device according to claim 1 , wherein the absorber layer has a carrier diffusion length greater than or equal to 50 nm.
3. The tandem photovoltaic device according to claim 1 or claim 2, wherein the absorber layer has a carrier lifetime greater than or equal to 1 ns.
4. The tandem photovoltaic device according to claim 1 or any one of claims 2 to 3, wherein the absorption layer has a thickness less than or equal to 1×10 16 cm -3 The n-type carrier concentration.
5. The tandem photovoltaic device of claim 1 or any one of claims 2-4, wherein the absorber layer comprises oxygen in the grain boundaries.
6. The tandem photovoltaic device according to claim 1 or any one of claims 2 to 5, wherein the absorber layer has a 1×10 17 cm -3 Up to 1x10 19 cm -3 The average concentration in the range includes oxygen.
7. The tandem photovoltaic device of claim 1 or any one of claims 2-6, wherein the absorber layer comprises a dopant comprising rubidium (Rb).
8. The tandem photovoltaic device of claim 1 or any one of claims 2-7, wherein the absorber layer is a polycrystalline film having a thickness in the range of 0.25 μm to 2.0 μm and an average grain size in the range of 1.3 μm to 3.0 μm.
9. The tandem photovoltaic device according to claim 1 or any one of claims 2-8, wherein the absorber layer is a polycrystalline film, wherein the ratio of grains with (103) orientation to grains with (002) orientation is equal to or greater than 1:1000.
10. The tandem photovoltaic device of claim 1 or any one of claims 2-9, wherein the hole contact comprises a high work function layer having a work function greater than or equal to 5 eV.
11. The tandem photovoltaic device of claim 1 or any one of claims 2-10, wherein the hole contact comprises a layer having a p-mobility to n-mobility ratio of less than 2.
12. The tandem photovoltaic device according to claim 1 or any one of claims 2 to 11, wherein: The hole contact comprises a p+ layer of an n+ / p+ tunnel junction, The n+ / p+ tunnel junction has an n+ side and a p+ side, and The absorber layer forms the pn junction with the p+ side of the n+ / p+ tunnel junction.
13. The tandem photovoltaic device of claim 12, wherein the n+ side of the n+ / p+ tunnel junction comprises a metal oxide doped n+ layer.
14. The tandem photovoltaic device of claim 13, wherein the layer of metal oxide comprises SnO2:F.
15. The tandem photovoltaic device of claim 13, wherein the layer of metal oxide comprises ITO.
16. The tandem photovoltaic device of claim 13, wherein the layer of metal oxide comprises Cd2SnO4.
17. The tandem photovoltaic device of claim 13, wherein the layer of metal oxide comprises WO3.
18. The tandem photovoltaic device of claim 13, wherein the layer of metal oxide comprises MoO3.
19. The tandem photovoltaic device of claim 13, wherein the layer of metal oxide comprises CrO3.
20. The tandem photovoltaic device of claim 13, wherein the layer of metal oxide comprises V2O5.
21. The tandem photovoltaic device of claim 12, wherein the n+ side of the n+ / p+ tunnel junction is over an n-type transparent conductive oxide.
22. The tandem photovoltaic device of claim 12, wherein the n+ side of the n+ / p+ tunnel junction comprises GaP.
23. The tandem photovoltaic device of claim 12, wherein the n+ side of the n+ / p+ tunnel junction comprises BP.
24. The tandem photovoltaic device of claim 12, wherein the n+ side of the n+ / p+ tunnel junction comprises ZnSe.
25. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises a p-type transparent conductive oxide.
26. The tandem photovoltaic device of claim 25, wherein the p-type transparent conductive oxide comprises nickel oxide.
27. The tandem photovoltaic device of claim 25, wherein the p-type transparent conductive oxide comprises tin oxide.
28. The tandem photovoltaic device of claim 25, wherein the p-type transparent conductive oxide is doped with B, Mg, N, Sb, or any combination thereof.
29. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises a p-type alloy of Zn, S, Se, and Te.
30. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises PTAA.
31. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises PDI.
32. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises CBP.
33. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises TCTA.
34. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises TCP.
35. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises F8BT.
36. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises CuAlS2.
37. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises CuAlSe2.
38. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises CuGaO2.
39. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises GeMgP2.
40. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises BP.
41. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises GaP.
42. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises ZnSe.
43. A tandem photovoltaic device according to claim 1 or any one of claims 2-24, wherein the hole contact comprises TaO x N (1-x) .
44. A tandem photovoltaic device according to claim 1 or any one of claims 2-24, wherein the hole contact comprises a buffer layer comprising MoS2.
45. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises a buffer layer comprising WS2.
46. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises NbS2.
47. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises VS.
48. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises TaS2.
49. The tandem photovoltaic device of claim 1 or any one of claims 2-24, wherein the hole contact comprises TiS2.
50. A method of forming an absorber layer of a photovoltaic device, the method comprising: providing a layer stack including a p-type layer; depositing a polycrystalline film over the p-type layer, wherein the polycrystalline film consists essentially of CdSe; contacting the exposed surface of the polycrystalline film with a halogen compound and a promoter; heating the polycrystalline film in a controlled environment to form the absorber layer, wherein the controlled environment comprises oxygen, thereby: The absorption layer has a thickness less than 1x10 17 cm -3 The n-type carrier concentration; The absorber layer has a density of equal to or greater than 1×10 13 A level of chlorine is included in said grain boundaries; and The polycrystalline film has an average grain size that is larger than the thickness of the film.
51. The method of claim 46, wherein the p-type layer is a hole contact and forms a pn junction with the absorber layer.
52. The method of claim 46 or claim 47, wherein the controlled environment comprises selenium (Se), whereby heating in the controlled environment comprising Se reduces Se vacancies in the polycrystalline film.
53. The method of claim 46 or any one of claims 47-48, wherein the halogen compound comprises at least one of: CdCl2, NH4Cl, CdBr2, CdI2, MgCl2, or Ba(ClO3)2.
54. The method of claim 46 or any one of claims 47-49, wherein the promoter comprises at least one of: Li, Na, K, Rb, or Cs.
55. The method of claim 46 or any one of claims 47-50, wherein the promoter comprises rubidium chloride.
56. The method of claim 46 or any one of claims 47-51, wherein the step of depositing a polycrystalline film comprises depositing the film by vapor transport deposition (VTD).
57. The method of claim 46 or any one of claims 47-52, wherein the layer stack comprises an n+ / p+ tunnel junction and wherein the hole contact comprises a p+ layer of the n+ / p+ tunnel junction.
58. The method of claim 46 or any one of claims 47-53, wherein the average grain size of the polycrystalline film is greater than 1.2 μm.
59. A method of forming a photovoltaic device, the method comprising: annealing an absorber layer consisting essentially of CdSe in the presence of a halogen compound, whereby the grain size of the absorber layer grows and the halogen diffuses into the absorber layer; and The absorber layer is treated by heating in a controlled environment containing Se and O2, whereby the treatment reduces Se vacancies in the absorber layer.
60. The method of claim 55, wherein the annealing step and the treating step are performed sequentially, wherein the annealing step precedes the treating step.
61. The method of claim 55, wherein the annealing step and the treating step are performed simultaneously.
62. The method of claim 55 or any one of claims 56-57, wherein a hole contact forms a pn junction with the absorber layer.
63. A photovoltaic device, comprising: an absorber layer comprising CdSe, wherein the absorber layer is n-type; and A hole contact forms a pn junction with the absorption layer.
64. The method or photovoltaic device of any one of claims 46-59, wherein the absorber layer is disposed in an upper submodule of a tandem photovoltaic device.
65. The method or photovoltaic device of any one of claims 46-60, wherein the absorber layer has a carrier diffusion length greater than or equal to 50 nm.
66. The method or photovoltaic device of any one of claims 46-61, wherein the absorber layer has a carrier lifetime greater than or equal to 1 ns.
67. The method or photovoltaic device of any one of claims 46-62, wherein the absorber layer has a thickness less than or equal to 1 x 1016 cm -3 The p-type dopant concentration is .
68. The method or photovoltaic device of any one of claims 47-54 or 58-63, wherein the hole contact comprises a layer having a valence band offset greater than 0 eV relative to the absorber layer.
69. The method or photovoltaic device of any one of claims 47-54 or 58-64, wherein the hole contact comprises a high work function layer having a work function greater than or equal to 5 eV.
70. The method or photovoltaic device of any one of claims 47-54 or 58-65, wherein the hole contact comprises a layer having a p-mobility to n-mobility ratio of less than 2.
71. The method or photovoltaic device of any one of claims 47-54 or 58-66, wherein: The hole contact comprises a p+ layer of an n+ / p+ tunnel junction, The n+ / p+ tunnel junction has an n+ side and a p+ side, and The absorber layer forms the pn junction with the p+ side of the n+ / p+ tunnel junction.
72. The method or photovoltaic device of claim 67 wherein the n+ side of the n+ / p+ tunnel junction comprises a metal oxide doped n+ layer.
73. The method or photovoltaic device of claim 68, wherein the layer of metal oxide comprises at least one of: SnO2:F, ITO, Cd2SnO4, WO3, MoO3, CrO3, or V2O5.
74. The method or photovoltaic device of any one of claims 67-69, wherein the n+ side of the n+ / p+ tunnel junction is over an n-type transparent conductive oxide.
75. The method or photovoltaic device of any one of claims 67-70, wherein the n+ / p+ tunnel junction comprises at least one of: GaP, BP, or ZnSe.
76. The method or photovoltaic device of any one of claims 47-54 or 58-71, wherein the hole contact comprises a p-type transparent conductive oxide.
77. The method or photovoltaic device of claim 72, wherein the p-type transparent conductive oxide comprises nickel oxide.
78. The method or photovoltaic device of claim 72, wherein the p-type transparent conductive oxide comprises tin oxide.
79. The method or photovoltaic device of any one of claims 72-74, wherein the p-type transparent conductive oxide is doped with B, Mg, N, Sb, or any combination thereof.
80. The method or photovoltaic device of any one of claims 47-54 or 58-71, wherein the hole contact comprises a p-type alloy of Zn, S, Se, and Te.
81. The method or photovoltaic device of any one of claims 47-54 or 58-71, wherein the hole contact comprises at least one of PTAA, PDI, CBP, TCTA, TCP, F8BT, CuAlS2, CuAlSe2, CuGaO2, GeMgP2, BP, GaP, ZnSe, TaO x N (1-x) , MoS2, WS2, NbS2, VS, TaS2 or TiS2.
82. The method or photovoltaic device of claim 77, wherein the hole contact comprises a buffer layer comprising MoS2 or WS2.
83. The method or photovoltaic device of claim 77 or claim 78, wherein the hole contact comprises CuAlS2.
84. The method or photovoltaic device of claim 77 or claim 78, wherein the hole contact comprises CuAlSe2.
85. The method or photovoltaic device of claim 77 or claim 78, wherein the hole contact comprises CuGaO2.
86. The method or photovoltaic device of claim 77 or claim 78, wherein the hole contact comprises PTAA.