Microspherical TiO2-x / C / FeMn-LDO nano material as well as preparation method and application thereof

By preparing microspherical TiO2-x/C/FeMn-LDO nanomaterials, the problems of low catalytic efficiency and unstable structure of existing photocatalysts have been solved, and ammonia nitrogen and lipophilic antibiotics in water can be efficiently removed, and the material has magnetic properties. Characteristics of recycling.

CN118788320APending Publication Date: 2024-10-18CHINA THREE GORGES CORPORATION +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410899236.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing photocatalysts have low catalytic efficiency when removing ammonia nitrogen and organic pollutants in water bodies, and their structures are unstable and lack active sites, making it difficult to meet the needs for high-efficiency, low-cost, and no secondary pollution denitrification.

Method used

Using microspherical TiO2-x/C/FeMn-LDO nanomaterials, TiO2-x hollow microspheres were prepared through in-situ chemical reduction method, coated with sodium carboxymethyl cellulose to form a carbon layer, and deposited ferromanganese layers on the surface. Double hydroxide is calcined to prepare microspherical TiO2-x/C/FeMn-LDO nanomaterials with efficient catalytic performance.

Benefits of technology

It significantly improves the electron transfer efficiency and catalytic performance, provides more active sites and specific surface area, enhances the removal efficiency of ammonia nitrogen and lipophilic antibiotics, and achieves magnetic recovery of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788320A_ABST
    Figure CN118788320A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nano-materials, in particular to a microspheric TiO2-x / C / FeMn-LDO nano-material and a preparation method and application of the microspheric TiO2-x / C / FeMn-LDO nano-material. The preparation method is simple and controllable in process, the prepared microspherical TiO2-x / C / FeMn-LDO nano material has the advantages of combination of a spherical structure and a layered structure, carbon layer protection and oxygen vacancy stabilization on the basis of keeping the oxidation-reduction performance of TiO2, the conversion efficiency of photo-induced electrons is improved, the catalytic performance is high, the structure is stable, and the preparation method is suitable for industrial production. The photocatalyst has dual performances of adsorption and photocatalysis, and has important application in the field of efficient removal of ammonia nitrogen and lipophilic antibiotics in water when being used as a photo-Fenton catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nanomaterials, in particular to a microspherical TiO 2-x / C / FeMn-LDO nanomaterials and their preparation methods and applications. Background Art

[0002] With the rapid development of global agriculture and industrialization, the discharge of domestic sewage and industrial wastewater has increased, and the concentration of nitrogen-containing compounds in sewage and wastewater has continued to rise, especially the increase in ammonia nitrogen content, which has aggravated the eutrophication of water bodies and seriously damaged the water ecological environment. At present, the main methods of denitrification include physical stripping, physical adsorption, biodegradation, chemical precipitation, electrochemical oxidation, breakpoint chlorination, etc. These methods are either costly or inefficient. Breakpoint chlorination will also produce residual chlorine. Therefore, a new denitrification technology with high efficiency, low cost and no secondary pollution is urgently needed. Since ammonia nitrogen and organic pollutants often occur at the same time, their simultaneous removal has very important application value.

[0003] As research gradually deepens, advanced oxidation techniques (AOPs) have been continuously developed and applied. Advanced oxidation technology is a new type of oxidation treatment technology that is currently attracting much attention. It mainly works through the strong oxidizing substances (·OH, ·Cl, ·SO4, etc.) produced by the reaction. It is considered to be an ideal method for effectively removing difficult-to-degrade organic matter and ammonia nitrogen. Photocatalytic oxidation technology, as a type of advanced oxidation technology, is to add semiconductor photocatalysts to the reaction solution to produce ·OH with strong oxidizing ability under the condition of ultraviolet or visible light irradiation. ·OH undergoes redox reactions with pollutants to generate inorganic small molecules such as CO2. The photocatalytic oxidation technology treatment process not only has the characteristics of a wide range of applications, good removal effect, and no secondary pollution, but also has a good removal effect on certain special substances such as cyanide and bacteria.

[0004] Chinese patent document CN109675581A discloses an iron-manganese bimetallic oxide modified biochar photo-Fenton composite material and a preparation method thereof. The biochar is used as the main material and the iron-manganese bimetallic oxide is used as the modification material, combining the advantages of the two materials, and has the advantages of high catalytic performance, good recycling, low cost, and environmental friendliness. It has a good degradation effect on polycyclic aromatic hydrocarbons in water bodies, but there are still problems such as few active sites and the catalytic efficiency needs to be improved. Summary of the invention

[0005] In view of the shortcomings of existing photocatalysts, the purpose of the present invention is to provide a microspherical TiO2 photocatalyst with high catalytic performance, stable structure and significant improvement in electron transfer efficiency. 2-x / C / FeMn-LDO nanomaterials and their preparation methods and applications.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] The first aspect of the present invention provides a microspherical TiO 2-x / C / FeMn-LDO nanomaterial preparation method, the specific technical scheme is as follows:

[0008] A microspherical TiO 2-x The preparation method of / C / FeMn-LDO nanomaterial comprises the following steps:

[0009] (1) TiO2 hollow microspheres were used as raw materials and TiO 2-x Hollow microspheres, where 0.1≤x≤2;

[0010] (2) TiO 2-x The hollow microspheres were activated and sodium carboxymethyl cellulose was coated on the activated TiO 2-x The surface of hollow microspheres is pyrolyzed and carbonized to obtain microspherical TiO 2-x / C;

[0011] (3) Using co-precipitation method to deposit TiO 2-x / C surface to prepare manganese iron layered double hydroxide to obtain microspherical TiO 2-x / C / FeMn-LDH S ;

[0012] (4) TiO 2-x / C / FeMn-LDH S Calcination in an inert atmosphere to obtain microspherical TiO 2-x / C / FeMn-LDO nanomaterials.

[0013] The second aspect of the present invention provides microspherical TiO prepared by the above preparation method. 2-x / C / FeMn-LDO nanomaterials.

[0014] The third aspect of the present invention provides the microspherical TiO 2-x / C / FeMn-LDO nanomaterials are used as photo-Fenton catalysts in the catalytic degradation of ammonia nitrogen and lipophilic antibiotics in sewage or sludge tail water.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] 1. Microspherical TiO 2-x / C / FeMn-LDO nanomaterials, hollow TiO2 microspheres, have good permeability and light utilization; and the reduced TiO 2-x Microspheres make the material have a higher light response and light absorption range; TiO2-x The carbon layer on the surface can protect the Ti 3+ / O VS It is not oxidized, achieving high-efficiency transfer of photogenerated electrons, thereby improving its catalytic performance and efficiency;

[0017] 2. TiO 2-x The amorphous carbon formed by carbonization of the sodium carboxymethyl cellulose coated on the surface of the hollow sphere has a higher specific surface area, high porosity and good electron transfer ability compared with other carbon sources, providing more active sites for catalysis;

[0018] 3. Microspherical TiO 2-x / C / FeMn-LDO nanomaterial, bimetallic oxide (FeMn-LDO) is a bimetallic synergistic system with a large number of active centers on the surface, such as oxygen vacancies, surface acid-base centers, surface hydroxyls, etc. At the same time, the LDO precursor LDHs has a large specific surface area and "memory effect", which makes the derived LDO have good catalytic performance; in addition, during the calcination process of LDHs, the amorphous carbon of the material itself can be used as a reducing agent, so that the calcined LDO has more surface defects than general metal oxides, which can provide more oxygen vacancies (Vo), optimize the adsorption capacity of the material, and enhance the interface charge transfer and catalytic ability.

[0019] 4. Microspherical TiO 2-x / C / FeMn-LDO nanomaterials have a large number of active centers, forming Fenton-like materials that can produce a large number of hydroxyl radicals. They can fully utilize the catalytic activity of iron and manganese bimetallic oxides and combine with amorphous carbon to further enhance the photocatalyst's absorption of sunlight and visible light, effectively improving the catalytic performance of the catalyst. They can also use their own magnetism to achieve rapid recovery of the catalyst. They can be used as photo-Fenton catalysts, which have good effects in the efficient removal of ammonia nitrogen and lipophilic antibiotics in water. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is the TiO in Example 1 2-x Scanning electron micrographs of hollow microspheres at different magnifications.

[0021] Figure 2 For different TiO 2-x The mass ratio of hollow microspheres and sodium carboxymethyl cellulose is the product of microspherical TiO 2-x / C scanning electron microscope image; (a) TiO 2-x The mass ratio of hollow microspheres to sodium carboxymethyl cellulose is 1:2; (b) TiO 2-x The mass ratio of hollow microspheres to sodium carboxymethyl cellulose is 1:3; (c) TiO 2-xThe mass ratio of hollow microspheres to sodium carboxymethyl cellulose is 1:4; (d) TiO 2-x The mass ratio of hollow microspheres to sodium carboxymethyl cellulose is 1:5; (e) TiO 2-x The mass ratio of hollow microspheres to sodium carboxymethyl cellulose is 1:6.

[0022] Figure 3 For TiO in Example 2 2-x The product microspherical TiO when the mass ratio of hollow microspheres to sodium carboxymethyl cellulose is 1:4 2-x / Enlarged scanning electron microscope image of the C surface.

[0023] Figure 4 The microspherical TiO 2-x / SEM image of C.

[0024] Figure 5 The microspherical TiO 2-x / C / FeMn-LDH S Scanning electron microscopy images at different magnifications.

[0025] Figure 6 The microspherical TiO 2-x Scanning electron microscope image of / C / FeMn-LDO nanomaterials.

[0026] Figure 7 The microspherical TiO 2-x High magnification scanning electron microscope image of / C / FeMn-LDO nanomaterial.

[0027] Figure 8 The microspherical TiO 2-x Transmission electron microscopy image of / C / FeMn-LDO nanomaterials.

[0028] Fig. 9 The microspherical TiO 2-x X-ray diffraction pattern of / C / FeMn-LDO nanomaterials.

[0029] Fig.10 They are respectively the microspherical TiO 2-x Tauc plot of / C / FeMn-LDO nanomaterial used as photo-Fenton catalyst and microspherical TiO2 / C / FeMn-LDO nanomaterial used as photo-Fenton catalyst in Comparative Example 4.

[0030] Fig.11 Different TiO 2-x The mass ratio of hollow microspheres and sodium carboxymethyl cellulose in the microspherical TiO 2-xPL spectrum of / C / FeMn-LDO nanomaterial used as photo-Fenton catalyst. DETAILED DESCRIPTION

[0031] The present invention designs and synthesizes a microspherical TiO2 with simple and controllable preparation, magnetic recovery, high catalytic performance and stable structure. 2-x / C / FeMn-LDO nanomaterials were first synthesized by hydrothermal method to obtain TiO2 hollow microspheres, and then reduced with a reducing agent to obtain TiO 2-x Hollow microspheres are then activated with dilute acid solution to hydroxylate the surface of the hollow microspheres; TiO 2-x The activated hydroxyl groups on the surface of hollow microspheres and the hydroxyl groups on the surface of sodium carboxymethyl cellulose (CMC-Na) form hydrogen bonds, allowing CMC-Na to be adsorbed on TiO 2-x The surface of hollow microspheres, after pyrolysis carbonization, CMC-Na on TiO 2-x The surface of the hollow microspheres is carbonized to form an amorphous carbon layer of 5 to 10 nm, which can protect the Ti 3+ / O VS Without being oxidized, Fe / Mn salt was used as a precursor and co-precipitated on TiO 2-x FeMn-LDHs are generated on the surface of TiO2 / C microspheres, thus forming a spherical and layered composite material structure. Finally, a nanomaterial with excellent catalytic effect is prepared by high-temperature calcination, which combines the advantages of spherical structure and layered structure, carbon protective layer and stable oxygen vacancies. 2-x The carbon layer on the surface can protect the Ti 3+ / O VS It is not oxidized, achieving high-efficiency transfer of photogenerated electrons, and the appropriate band structure of the Fe-Mn layered bimetallic oxide is consistent with that of TiO 2-x The heterostructure constructed makes TiO 2-x The photoexcited electrons in the conduction band spontaneously transfer to the valence band of FeMn-LDO, consuming the residual holes in FeMn-LDO. Without affecting the redox activity of TiO2, the effective spatial separation of photogenerated electrons and holes is achieved, thereby improving its catalytic performance and efficiency.

[0032] The microspherical TiO 2-x / C / FeMn-LDO nanomaterials and their preparation methods and applications.

[0033] The first aspect of the present invention provides microspherical TiO 2-x The preparation method of / C / FeMn-LDO nanomaterial comprises the following steps:

[0034] (1) TiO2 hollow microspheres were used as raw materials and TiO 2-x Hollow microspheres, where 0.1≤x≤2;

[0035] (2) TiO 2-x The hollow microspheres were activated and sodium carboxymethyl cellulose was coated on the activated TiO 2-x The surface of hollow microspheres is pyrolyzed and carbonized to obtain microspherical TiO 2-x / C;

[0036] (3) Using co-precipitation method to prepare microspherical TiO 2-x / C surface to prepare manganese iron layered double hydroxide to obtain microspherical TiO 2-x / C / FeMn-LDH S ;

[0037] (4) Microspherical TiO 2-x / C / FeMn-LDH S Calcination in an inert atmosphere to obtain microspherical TiO 2-x / C / FeMn-LDO nanomaterials.

[0038] In some embodiments of the present invention, in step (1), the preparation method of the TiO2 hollow microspheres comprises: using Ti salt as a precursor, ethanol as a solvent, and urea as an organic additive, and performing a hydrothermal reaction to prepare TiO2 hollow microspheres. In some embodiments of the present invention, the Ti salt is selected from any one of Ti(SO4)2, TiCl4, and Ti(S2O7)2. In some embodiments of the present invention, the molar ratio of the Ti salt to urea is 1:1-2. In some embodiments of the present invention, the ratio of the mass of urea to the volume of ethanol in the urea-ethanol solution formed by the urea and ethanol is 0.02-0.05g / mL. Preferably, the concentration of the ethanol is 95wt%. In some embodiments of the present invention, the reaction temperature of the hydrothermal reaction is 120-140°C, and the reaction time is 12-14h.

[0039] In some embodiments of the present invention, in step (1), the in-situ chemical reduction method specifically comprises adding TiO2 hollow microspheres to a reducing agent solution, performing a reduction reaction at room temperature, washing, and drying to obtain TiO 2-x Hollow microspheres. In some embodiments of the present invention, the reducing agent is selected from any one or more of NaBH4, KBH4, and H2C2O4. Preferably, the solvent of the reducing agent solution is water, and the concentration of the reducing agent in the reducing agent solution is 0.1 to 0.5 mol / L. In some embodiments of the present invention, magnetic stirring is performed during the reduction reaction. In some embodiments of the present invention, the washing medium is water. In some embodiments of the present invention, the drying temperature of the drying is 60 to 80°C, and the drying time is 12 to 24 hours.

[0040] In some embodiments of the present invention, in step (2), the activation treatment comprises treating TiO 2-x The hollow microspheres are placed in a dilute acid solution for ultrasonic treatment. In some embodiments of the present invention, the dilute acid solution is selected from any one of dilute hydrochloric acid, dilute nitric acid, dilute sulfuric acid, hydrofluoric acid, etc. In some embodiments of the present invention, the concentration of the dilute acid solution is 0.0005-0.01 mol / L.

[0041] In some embodiments of the present invention, in step (2), the sodium carboxymethyl cellulose is coated on the activated TiO 2-x The surface of the hollow microspheres comprises: the activated TiO 2-x The hollow microspheres are dispersed in a sodium carboxymethyl cellulose solution, so that the sodium carboxymethyl cellulose is coated on the activated TiO 2-x In some embodiments of the present invention, the TiO 2-x The mass ratio of hollow microspheres to sodium carboxymethyl cellulose is 1:3-5. 2-x When the mass ratio of hollow microspheres to sodium carboxymethyl cellulose increases from 1:2 to 1:5, the TiO 2-x The carbon layer coverage on the surface of hollow microspheres gradually increased, but when the concentration of sodium carboxymethyl cellulose was too high (TiO 2-x When the mass ratio of hollow microspheres to sodium carboxymethyl cellulose was 1:6), it was not good. It was speculated that the excessive concentration of sodium carboxymethyl cellulose would cause it to self-assemble into a micellar structure and form a colloidal suspension, which would affect its adhesion to TiO 2-x The hollow microspheres are adsorbed on the surface, thus affecting the coating of the surface carbon layer; Figure 2 In figure e, we can see that a large number of cluster structures appear around the microspheres, which also confirms this point.

[0042] In some embodiments of the present invention, in step (2), the pyrolysis temperature is 400-600°C, and the pyrolysis time is 3-5h. In some embodiments of the present invention, the pyrolysis adopts programmed temperature increase, and the temperature increase rate is 5-10°C / min.

[0043] In some embodiments of the present invention, in step (2), the pyrolysis carbonization product needs to be washed, centrifuged, and dried to obtain microspherical TiO 2-x / C. In some embodiments of the present invention, the washing is washing with deionized water and ethanol in sequence. In some embodiments of the present invention, the drying temperature is 80-90°C and the drying time is 10-12h.

[0044] In some embodiments of the present invention, in step (3), the coprecipitation method comprises the following steps: ultrasonically treating a mixed salt solution of a trivalent iron salt and a divalent manganese salt, and dropping the solution into a mixed alkaline solution of NaOH and Na2CO3, maintaining the pH at 9.5 to 10.5; after the addition is complete, adding TiO 2-x / C, ultrasonic treatment, after precipitation is complete, washing and drying to obtain microspherical TiO 2-x / C / FeMn-LDH S In some embodiments of the present invention, the mixed salt solution contains Fe 3+ , Mn 2+ The molar ratio of Fe is 1-2:1-5. 3+ With Mn 2+ Fe in mixed salt solution 3+ The concentration of Mn is 0.1~1.0mol / L, 2+ The concentration of the mixed salt solution is 0.1-1.0 mol / L. In some embodiments of the present invention, the trivalent iron salt and the microspherical TiO 2-x / C has a mass ratio of 1 to 2:1. In some embodiments of the present invention, the temperature of the precipitation reaction is 150 to 170°C, and the reaction time is 3 to 5 hours. In some embodiments of the present invention, the ultrasonic treatment time is 10 to 20 minutes. In some embodiments of the present invention, the washing is sequentially washed with deionized water and ethanol; in some embodiments of the present invention, the drying method is vacuum drying, the drying temperature is 50 to 70°C, and the drying time is 2 to 4 hours.

[0045] In some embodiments of the present invention, in step (4), the calcination temperature is 400-600°C and the time is 1-2h. In some embodiments of the present invention, the calcination is performed by programmed temperature increase at a rate of 5-10°C / min. In some embodiments of the present invention, the inert atmosphere is one or a combination of nitrogen, argon and helium.

[0046] The second aspect of the present invention provides the microspherical TiO 2-x / C / FeMn-LDO nanomaterials prepared by the preparation method 2-x / C / FeMn-LDO nanomaterial. Figures 1-2 , Figures 5 to 8 It can be seen that the composite photo-Fenton catalyst of the present invention comprises a three-layer structure, which is TiO 2-x The hollow microsphere comprises an inner core layer, an amorphous carbon layer covering the outer portion of the inner core layer, and an iron-manganese bimetallic oxide layer deposited on the surface of the amorphous carbon layer.

[0047] The third aspect of the present invention provides the microspherical TiO 2-x / C / FeMn-LDO nanomaterials are used as photo-Fenton catalysts in the catalytic degradation of ammonia nitrogen and lipophilic antibiotics in sewage or sludge tail water.

[0048] In some embodiments of the present invention, the microspherical TiO 2-x / C / FeMn-LDO nanomaterials are used to catalyze the degradation of ammonia nitrogen and lipophilic antibiotics in sewage or sludge tail water, including the following steps: preparing microspherical TiO 2-x / C / FeMn-LDO nanomaterials are added to water containing ammonia nitrogen and lipophilic antibiotics, H2O2 solution is added, and the mixture is placed under visible light for photocatalytic degradation. Preferably, the ammonia nitrogen concentration in the water is 10-50 mg / L, the lipophilic antibiotic concentration is 10-100 mg / L, the H2O2 solution dosage is 1.5-5.0 mL / L, the catalyst dosage is 10-50 mg / L, and the degradation time is 30-120 min.

[0049] In some embodiments of the present invention, the antibiotics include quinolone antibiotics, macrolide antibiotics, tetracycline antibiotics, sulfonamide antibiotics, etc. The quinolone antibiotics include norfloxacin, ciprofloxacin, enrofloxacin, ofloxacin, etc.; the macrolide antibiotics include azithromycin, erythromycin, etc.; the tetracycline antibiotics include tetracycline, chlortetracycline, oxytetracycline, etc.; the sulfonamide antibiotics include sulfamethazine, sulfamethoxazole, etc.

[0050] The specific embodiments of the present invention are further described in detail below in conjunction with preferred embodiments. When the embodiments provide numerical ranges, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, as those skilled in the art grasp the prior art and record the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.

[0051] Example 1

[0052] A microspherical TiO 2-x The preparation method of / C / FeMn-LDO nanomaterial comprises the following steps:

[0053] (1) Weigh 10 g of Ti(SO4)2 and add it to a mixed solution of 2.5 g of urea and 50 mL of 95 wt% ethanol, mix well, then transfer the solution to a 150 mL polytetrafluoroethylene-lined reactor, react at 140°C for 12 h, cool naturally to room temperature, centrifuge, wash the product with deionized water and ethanol for several times, and vacuum dry at 80°C for 12 h to obtain the product TiO2 hollow microspheres; add the prepared TiO2 hollow microspheres to a 0.1 mol / L NaBH4 solution, stir magnetically at room temperature for 60 min, and finally wash with deionized water for several times and dry at room temperature to obtain TiO 2-x Hollow microspheres (0.1≤x≤2); the scanning electron microscopy characterization results of the product are as follows Figure 1 shown.

[0054] (2) Weigh 5g TiO 2-x The hollow microspheres were placed in 20 mL of 0.0015 mol / L dilute nitric acid solution, ultrasonicated for 10 min, and dispersed in 70 mL of 0.82 mol / L sodium carboxymethyl cellulose solution after centrifugation (TiO 2-x The mass ratio of hollow microspheres to sodium carboxymethyl cellulose was 1:3), ultrasonicated for 20 min, and vacuum filtered to remove the TiO 2-x The hollow microspheres were transferred to a muffle furnace, heated to 500°C at a heating rate of 5°C / min and kept warm for 5 h, and naturally cooled to room temperature. The product was washed several times with deionized water and ethanol, centrifuged, and vacuum dried at 85°C for 10 h to obtain the product microspherical TiO 2-x / C, microspherical TiO 2-x The scanning electron microscopy results of / C are shown in Figure 2 As shown in b.

[0055] (3) A mixed salt solution of 25 mL, 1.0 mol / L Fe(NO3)3·9H2O and 25 mL, 1.0 mol / L mn(NO3)2·4H2O was ultrasonicated for 20 min, and 7 g of microspherical TiO 2-x / C, stir evenly; dissolve 0.03 mol NaOH and 0.015 mol Na2CO3 in 100 mL water, stir for 30 min to form a mixed alkali solution; drop the mixed alkali solution into the mixed salt solution drop by drop, keep the pH stable at 10, ultrasonicate for 30 min after the addition is completed, react at 150 ° C for 3 h under oil bath conditions, cool naturally to room temperature, centrifuge, wash the product with deionized water and ethanol for several times, and vacuum dry at 70 ° C for 3 h to obtain the product microspherical TiO 2-x / C / FeMn-LDH S , microspherical TiO 2-x / C / FeMn-LDHS The SEM characterization results are as follows Figure 5 shown.

[0056] (4) Microspherical TiO 2-x / C / FeMn-LHD S Transfer to a muffle furnace and calcine in an inert atmosphere, heat to 550 °C at a heating rate of 5 °C / min and keep warm for 2 h, and cool naturally to room temperature to obtain the target product, microspherical TiO 2-x / C / FeMn-LDO nanomaterials, the SEM, TEM, and XRD characterization results of the target product are shown in Figures 6 to 9 shown.

[0057] Figure 1 , Figure 2 Middle b, Figure 5-7 The following are scanning electron microscope images of the products obtained in each step of Example 1. Figure 1 It can be seen that the TiO prepared in Example 1 2-x The hollow microsphere samples are in the shape of microspheres; Figure 2 Middle b, Figure 5-7 Compared to Figure 1 It can be seen that the surface of the microspheres coated with the carbon layer becomes rougher than that of the TiO2 microspheres, and the surface of the microspheres further coated with bimetallic oxides becomes even rougher. The intuitive morphology and structure preliminarily indicate that the material composite is successful.

[0058] Figure 8 The microspherical TiO 2-x Transmission electron microscope image of / C / FeMn-LDO nanomaterials. Figure 8 It can be seen that the sample presents an obvious core-shell structure.

[0059] Fig. 9 The microspherical TiO prepared in Example 1 2-x X-ray diffraction pattern of / C / FeMn-LDO nanomaterials. Fig. 9It can be seen that the material shows characteristic diffraction peaks of anatase TiO2 at 25.3o, 37.8, 48.0o, 55.1o and 68.8o at 2θ, corresponding to (101), (004), (200), (211) and (116) crystal planes, respectively. It can be seen that TiO2 still retains its original characteristic diffraction peaks after being reduced, indicating that the structural characteristics of TiO2 are not affected by the reducing agent; the broad and weak diffraction peak at 21.5° is the diffraction peak of carbon corresponding to (002) The decrease in the intensity of the characteristic diffraction peaks on the crystal plane may be attributed to the surface-coated LDO; the characteristic diffraction peaks of iron oxide 23.4o(111), 33.2o(220) and 40.8o(311) and the characteristic diffraction peaks of manganese oxide 24.6(002), 36.5(100) and 65.2(110) can also be observed in the sample; it can be seen that the characteristic peaks of TiO2, carbon and FeMn-LDO appear in the material at the same time, further indicating that the material is successfully composited.

[0060] Example 2

[0061] A microspherical TiO 2-x The preparation method of / C / FeMn-LDO nanomaterial comprises the following steps:

[0062] (1) Weigh 10 g of Ti(SO4)2 and add it to a mixed solution of 2.5 g of urea and 50 mL of 95 wt% ethanol, mix well, then transfer the solution to a 150 mL polytetrafluoroethylene-lined reactor, react at 140°C for 12 h, cool naturally to room temperature, centrifuge, wash the product with deionized water and ethanol for several times, and vacuum dry at 80°C for 12 h to obtain the product TiO2 hollow microspheres; add the prepared TiO2 hollow microspheres to a 0.1 mol / L NaBH4 solution, stir magnetically at room temperature for 60 min, and finally wash with deionized water and dry to obtain TiO 2-x Hollow microspheres (0.1≤x≤2).

[0063] (2) Weigh 5g TiO 2-x The hollow microspheres were placed in 20 mL of 0.0015 mol / L dilute nitric acid solution, ultrasonicated for 10 min, and dispersed in 70 mL of 1.09 mol / L sodium carboxymethyl cellulose solution after centrifugation (TiO 2-x The mass ratio of hollow microspheres to sodium carboxymethyl cellulose was 1:4), ultrasonic treatment was performed for 20 min, and vacuum filtration was performed to separate the TiO 2-x The hollow microspheres were transferred to a muffle furnace, heated to 600 °C at a heating rate of 5 °C / min and kept warm for 5 h, cooled naturally to room temperature, and centrifuged. The product was washed several times with deionized water and ethanol, and dried in vacuum at 85 °C for 10 h to obtain the product microspherical TiO2-x / C, microspherical TiO 2-x The scanning electron microscopy results of / C are shown in Figure 2 Medium c and Figure 3 shown.

[0064] (3) A mixed salt solution of 25 mL, 1.0 mol / L Fe(NO3)3·9H2O and 25 mL, 1.0 mol / L mn(NO3)2·4H2O was ultrasonicated for 20 min, and 7 g of microspherical TiO 2-x / C, stir evenly; dissolve 0.03 mol NaOH and 0.015 mol Na2CO3 in 100 mL water, stir for 30 min to form a mixed alkali solution; add the mixed alkali solution dropwise to the mixed salt solution, keep the pH stable at 9.5, ultrasonicate for 30 min after the addition is completed, react at 150 ° C for 5 h under oil bath conditions, cool naturally to room temperature, centrifuge, wash the product with deionized water and ethanol for several times, and vacuum dry at 70 ° C for 3 h to obtain the product microspherical TiO 2-x / C / FeMn-LDH S .

[0065] (4) Microspherical TiO 2-x / C / FeMn-LHD S Transfer to a muffle furnace and calcine in an inert atmosphere, heat to 550 °C at a heating rate of 5 °C / min and keep warm for 2 h, and cool naturally to room temperature to obtain the target product, microspherical TiO 2-x / C / FeMn-LDO nanomaterials.

[0066] Example 3

[0067] A microspherical TiO 2-x The preparation method of / C / FeMn-LDO nanomaterial comprises the following steps:

[0068] (1) Weigh 10 g of Ti(SO4)2 and add it to a mixed solution of 2.5 g of urea and 50 mL of 95 wt% ethanol, mix well, then transfer the solution to a 150 mL polytetrafluoroethylene-lined reactor, react at 130°C for 12 h, cool naturally to room temperature, centrifuge, wash the product with deionized water and ethanol for several times, and vacuum dry at 80°C for 12 h to obtain the product TiO2 hollow microspheres; add the prepared TiO2 hollow microspheres to a 0.1 mol / L NaBH4 solution, stir magnetically at room temperature for 60 min, and finally wash with deionized water and dry to obtain TiO 2-x Hollow microspheres (0.1≤x≤2).

[0069] (2) Weigh 5g TiO 2-xThe hollow microspheres were placed in 20 mL of 0.0015 mol / L dilute nitric acid solution, ultrasonicated for 10 min, and dispersed in 80 mL of 1.19 mol / L sodium carboxymethyl cellulose solution after centrifugation (TiO 2-x The mass ratio of hollow microspheres to sodium carboxymethyl cellulose was 1:5), ultrasonic treatment was performed for 20 min, and vacuum filtration was performed to separate the TiO 2-x The hollow microspheres were transferred to a muffle furnace, heated to 500°C at a heating rate of 5°C / min and kept warm for 5 h, and naturally cooled to room temperature. The product was washed several times with deionized water and ethanol, centrifuged, and vacuum dried at 85°C for 10 h to obtain the product TiO 2-x / C hollow microspheres, TiO 2-x The scanning electron microscopy characterization results of / C hollow microspheres are shown in Figure 2 As shown in middle d.

[0070] (3) A mixed salt solution of 25 mL, 1.0 mol / L Fe(NO3)3·9H2O and 50 mL, 2.0 mol / L Mn(NO3)2·4H2O was ultrasonicated for 20 min, and 7 g of microspherical TiO 2-x / C, stir evenly; dissolve 0.03 mol NaOH and 0.015 mol Na2CO3 in 100 mL water, stir for 30 min to form a mixed alkali solution; add the mixed alkali solution drop by drop to the mixed salt solution, keep the pH stable at 10, ultrasonicate for 20 min after the addition is completed, react at 150 ° C for 3 h under oil bath conditions, cool naturally to room temperature, centrifuge, wash the product with deionized water and ethanol for several times, and vacuum dry at 70 ° C for 3 h to obtain the product microspherical TiO 2-x / C / FeMn-LDH S .

[0071] (4) Microspherical TiO 2-x / C / FeMn-LDH S Transfer to a muffle furnace and calcine in an inert atmosphere, heating to 600 °C at a heating rate of 5 °C / min and keeping the temperature for 1.5 h, and naturally cooling to room temperature to obtain the target product, microspherical TiO 2-x / C / FeMn-LDO nanomaterials.

[0072] Comparative Example 1

[0073] Except for step (2), the carbon source is glucose, TiO 2-x The mass ratio of hollow microspheres to glucose is 1:3, in which TiO 2-xThe hollow microspheres were 5 g, the volume of the glucose aqueous solution was 40 mL, the concentration was 2.08 mol / L, the pyrolysis carbonization temperature was 150°C, the time was 5 h, and the rest was the same as in Example 1. The SEM characterization results of the product are shown in Figure 4 shown.

[0074] Comparative Example 2

[0075] Except for step (2), TiO 2-x The mass ratio of hollow microspheres to sodium carboxymethyl cellulose is 1:2, wherein the volume of sodium carboxymethyl cellulose solution is 70 mL, the concentration is 0.54 mol / L, and the rest is the same as in Example 1. The SEM characterization results of the product are shown in Figure 2 As shown in a.

[0076] Comparative Example 3

[0077] Except for step (2), TiO 2-x The mass ratio of hollow microspheres to sodium carboxymethyl cellulose is 1:6, wherein the volume of sodium carboxymethyl cellulose solution is 70 mL, and the concentration is 1.63 mol / L. The rest is the same as in Example 1. The SEM characterization results of the product are shown in Figure 2 As shown in figure e.

[0078] Comparative Example 4

[0079] The method does not include step (1), that is, directly using TiO2 hollow microspheres instead of TiO 2-x The hollow microspheres are subjected to the same operation as in Example 1 except that steps (2) to (4) are performed to obtain a microspherical TiO2 / C / FeMn-LDO composite nanomaterial.

[0080] Fig.10 The microspherical TiO prepared in Example 1 2-x Tauc plot of the microspherical TiO2 / C / FeMn-LDO4 nanomaterial and the microspherical TiO2 / C / FeMn-LDO nanomaterial prepared in Comparative Example 4 as a photo-Fenton catalyst. Fig.10 It can be seen that the microspherical TiO 2-x The absorption edge of / C / FeMn-LDO nanomaterials has a red shift, and the optical band gap is 2.68eV, which is significantly lower than 3.2eV of TiO2, indicating that the modified composite material has a wider light absorption range than single TiO2; at the same time, compared with the unreduced catalyst, the optical band gap is 2.89eV, which is still superior to single TiO2, indicating that the reduced TiO 2-x Microspheres can make the composite material have higher light response and light absorption range. The reduction of the band gap is related to the reduced Ti, which leads to the increase of the electronic state vacancy band, and the increase of the light absorption range may be due to the introduction of defects by Ti to improve the absorption of photon energy.

[0081] Fig.11 Different TiO 2-x The mass ratio of hollow microspheres and sodium carboxymethyl cellulose in the microspherical TiO 2-x PL spectrum of / C / FeMn-LDO composite photo-Fenton catalyst. Fig.11 It can be seen that within a certain range, as the concentration of sodium carboxymethyl cellulose increases, the PL intensity gradually decreases, indicating that the carbon layer can inhibit the recombination of photogenerated electron-hole pairs during the transfer process and achieve efficient transfer of photogenerated electrons, thereby improving its catalytic performance and efficiency.

[0082] The microspherical TiO 2-x / C / FeMn-LDO nanomaterials and the products prepared in Comparative Examples 1 to 4 are used to remove ammonia nitrogen and antibiotics in water. The specific operation is as follows: weigh the microspherical TiO prepared in Examples 1 to 3 respectively. 2-x / C / FeMn-LDO nanomaterials, microspherical TiO prepared in step (3) of Example 1 2-x / C / FeMn-LDHs, microspherical TiO prepared in step (2) of Example 1 2-x / C, TiO prepared in step (1) of Example 1 2-x Hollow microspheres, microspherical TiO prepared in Comparative Examples 1 to 3 2-x / C / FeMn-LDO, microspherical TiO prepared in Comparative Examples 1 to 3 2-x / C and comparative example 4 prepared microspherical TiO2 / C / FeMn-LDO 30mg each, the above thirteen groups of materials were placed in thirteen groups numbered 1 to 13, 50mL of ammonia nitrogen concentration 50mg / L, tetracycline 50mg / L solution, and stirred in the dark for 30min under the condition of shielding to achieve adsorption and desorption equilibrium; after the dark stirring, 1.5mL of H2O2 solution was added, and the reaction was carried out under light conditions for catalytic degradation for 30min. The results are shown in Table 1:

[0083] Table 1 Degradation rate of ammonia nitrogen and antibiotics by the nanomaterials prepared in the examples and comparative examples as photo-Fenton catalysts

[0084]

[0085]

[0086] From the results in Table 1, it can be seen that the microspherical TiO 2-x / C / FeMn-LDO photo-Fenton catalyst, with TiO 2-x Compared with the catalyst, it can greatly improve the removal efficiency of ammonia nitrogen and lipophilic antibiotics in water.2-x / C through TiO 2-x The hollow microspheres are coated with an amorphous carbon layer to improve the catalytic performance. 2-x / C / FeMn-LDHs further S Coated with TiO 2-x / C surface on the surface of the carbon layer, forming a spherical and layered composite material, which significantly increases the specific surface area of ​​the catalyst, improves the catalytic activity, and can also synergistically adsorb nitrogen and phosphorus with the carbon layer. Therefore, the removal efficiency of ammonia nitrogen and lipophilic antibiotics is greatly improved; microspherical TiO 2-x After calcination of / C / FeMn-LDHs, the calcined LDO has more surface defects than general metal oxides, which can provide more oxygen vacancies (Vo), optimize the adsorption capacity of the material, enhance the interfacial charge transfer and catalytic ability, and further improve the removal efficiency of ammonia nitrogen and lipophilic antibiotics in water.

[0087] Comparative Example 1 uses glucose with the same mass ratio as in Example 1 as the carbon source, and the obtained TiO 2-x / C and TiO 2-x The removal efficiency of / C / FeMn-LDO for ammonia nitrogen and lipophilic antibiotics in water is not as good as that of TiO 2-x / C and TiO 2-x / C / FeMn-LDO, indicating that the choice of carbon source has an important influence on the photocatalytic performance of the material. 2-x / C material scanning electron microscope image ( Figure 4 ) and the TiO obtained in Example 1 2-x / C material scanning electron microscope image ( Figure 2 (b) Microspherical TiO 2-x The surface morphology of the TiO / C materials is compared and it can be seen that the TiO 2-x The thinner carbon layer on the surface of the / C material may be attributed to the fact that glucose, as a monosaccharide, has a lower carbon content than sodium carboxymethyl cellulose. The concentration of sodium carboxymethyl cellulose solution in Comparative Example 2 is lower, resulting in the thinner surface of TiO 2-x The surface of the hollow microspheres is not completely covered with sodium carboxymethyl cellulose, and the obtained microspherical TiO 2-x / C The carbon layer on the surface of the material is unevenly distributed ( Figure 2 As shown in a), the photocatalytic performance is inferior to that of Examples 1 to 3. The concentration of sodium carboxymethyl cellulose solution in Comparative Example 3 is relatively high, resulting in the TiO 2-x Sodium carboxymethyl cellulose accumulates on the surface of hollow microspheres, and forms more cluster structures after carbonization ( Figure 2e), and hindered the subsequent bimetallic deposition, resulting in the photocatalytic efficiency of the material being lower than that of Examples 1 to 3. Comparative Example 4 obtained an unreduced TiO2 composite catalyst, whose light response and light absorption range were relatively weak, resulting in the photocatalytic efficiency of the material being lower than that of Examples 1 to 3.

[0088] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A microspherical TiO 2-x / C / FeMn-LDO nanomaterial preparation method, It is characterized in that The following steps are involved: (1) TiO 2 Hollow microspheres were used as raw materials and TiO 2-x Hollow microspheres, where 0.1≤x≤2; (2) TiO 2-x The hollow microspheres were activated and sodium carboxymethyl cellulose was coated on the activated TiO 2-x The surface of hollow microspheres is pyrolyzed and carbonized to obtain microspherical TiO 2-x / C; (3) Using co-precipitation method to prepare microspherical TiO 2-x / C surface to prepare manganese iron layered double hydroxide to obtain microspherical TiO 2-x / C / FeMn-LDH S ; (4) Microspherical TiO 2-x / C / FeMn-LDH S Calcination in an inert atmosphere to obtain microspherical TiO 2-x / C / FeMn-LDO nanomaterials.

2. The preparation method according to claim 1, It is characterized in that In step (1), one or more of the following features are included: (1a) TiO 2 The preparation method of hollow microspheres comprises: using Ti salt as a precursor, ethanol as a solvent, and urea as an organic additive, and performing a hydrothermal reaction to prepare TiO 2 Hollow microspheres; (1b) The in-situ chemical reduction method comprises: 2 The hollow microspheres were added into the reducing agent solution, and the reduction reaction was carried out at room temperature. After washing and drying, TiO 2-x Hollow microspheres.

3. The preparation method according to claim 2, It is characterized in that In step (1), one or more of the following features are included: (1a1) The Ti salt is selected from Ti(SO 4 ) 2 、TiCl 4 、Ti(S 2 O 7 ) 2 Any of; (1a2) The molar ratio of the Ti salt to urea is 1:1-2; (1a3) the ratio of the mass of urea to the volume of ethanol in the urea-ethanol solution formed by the urea and ethanol is 0.02-0.05 g / mL; (1a4) the concentration of the ethanol solution is 95 wt %; (1a5) The reaction temperature of the hydrothermal reaction is 120 to 140° C., and the reaction time is 12 to 14 hours; (1b1) The reducing agent is selected from NaBH 4 KBH 4 , H 2 C 2 O 4 Any one or more of; (1b2) performing magnetic stirring during the reduction reaction; (1b3) the reducing agent concentration in the reducing agent solution is 0.1 mol / L-0.5 mol / L; (1b4) the washing medium is deionized water; (1b5) The drying temperature of the drying is 60 to 80° C., and the drying time is 12 to 24 hours.

4. The preparation method according to claim 1, It is characterized in that In step (2), one or more of the following features are included: (2a) The activation treatment comprises: 2-x The hollow microspheres were placed in a dilute acid solution for ultrasonic treatment; (2b) The sodium carboxymethyl cellulose is coated on the activated TiO 2-x The surface of the hollow microspheres includes: activated TiO 2-x The hollow microspheres are dispersed in a sodium carboxymethyl cellulose solution, so that the sodium carboxymethyl cellulose is coated on the activated TiO 2-x Hollow microsphere surface; (2c) The pyrolysis temperature is 400-600° C. and the pyrolysis time is 3-5 h; (2d) The product after pyrolysis and carbonization needs to be washed, centrifuged, and dried to obtain microspherical TiO 2-x / C.

5. The preparation method according to claim 4, It is characterized in that In step (2), one or more of the following features are included: (2a1) the dilute acid solution is selected from any one of dilute hydrochloric acid, dilute nitric acid, dilute sulfuric acid, and hydrofluoric acid; (2a2) The concentration of the dilute acid solution is 0.0005-0.01 mol / L; (2b1) TiO 2-x The mass ratio of hollow microspheres to sodium carboxymethyl cellulose is 1:3-5; (2c1) The pyrolysis is performed by programmed heating at a rate of 5 to 10°C / min; (2d1) The washing is performed by sequentially washing with deionized water and ethanol; (2d2) The drying temperature is 80-90°C and the drying time is 10-12 hours.

6. The preparation method according to claim 1, It is characterized in that Includes one or more of the following characteristics: (3a) In step (3), the coprecipitation method comprises the following steps: ultrasonically treating a mixed salt solution of a trivalent iron salt and a divalent manganese salt, and adding dropwise to a mixture of NaOH and Na 2 CO 3 In the mixed alkali solution, keep the pH at 9.5-10.5; after the addition is complete, add TiO 2-x / C, ultrasonic treatment, after precipitation is complete, washing and drying to obtain microspherical TiO 2-x / C / FeMn-LDH S ; (4a) In step (4), the calcination temperature is 400-600°C and the time is 1-2h.

7. The preparation method according to claim 6, It is characterized in that Includes one or more of the following characteristics: (3a1) In step (3), the mixed salt solution contains Fe 3+ , Mn 2+ The molar ratio is 1-2:1-5; (3a2) In step (3), the trivalent iron salt and the microspherical TiO 2-x The mass ratio of / C is 1-2:1; (3a3) In step (3), the precipitation reaction temperature is 150-170°C and the reaction time is 3-5h. (3a4) In step (3), the ultrasonic treatment time is 10 to 20 minutes; (3a5) In step (3), the washing is performed by sequentially washing with deionized water and ethanol; (3a6) In step (3), the drying method is vacuum drying, the drying temperature is 50 to 70° C., and the drying time is 2 to 4 hours; (4a1) In step (4), the calcination is carried out by programmed heating at a heating rate of 5 to 10°C / min.

8. A microspherical TiO prepared by the preparation method according to any one of claims 1 to 7 2-x / C / FeMn-LDO nanomaterials.

9. The microspherical TiO as claimed in claim 8 2-x / C / FeMn-LDO nanomaterials are used as photo-Fenton catalysts in the catalytic degradation of ammonia nitrogen and lipophilic antibiotics in sewage or sludge tail water.

10. The use according to claim 9, It is characterized in that The antibiotics include quinolone antibiotics, macrolide antibiotics, tetracycline antibiotics or sulfonamide antibiotics.

Citation Information

Patent Citations

  • Composite optical anode of dye -sensitized solar cell

    CN102157273A

  • Porous carbon-coated reduced TiO2-n lithium-sulfur battery positive electrode material and preparation method thereof

    CN111509228A