Preparation method and application of bimetallic monatomic quantum dot nano-enzyme

Bimetallic single-atom quantum dot nanozymes were prepared through the solid-phase reaction of ethylenediaminetetraacetic acid metal chelates, which solved the problems of nanozyme catalytic activity and stability and achieved efficient antibacterial effects and low-cost industrial production.

CN118788349APending Publication Date: 2024-10-18SHANDONG ANALYSIS AND TEST CENTER
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410848523.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing nanozymes have low catalytic activity, poor specificity, complex synthesis methods, and high costs, which limit their application in clinical treatment and large-scale production.

Method used

A metal chelate of ethylenediaminetetraacetic acid is used for solid-phase reaction to prepare a bimetallic single-atom quantum dot nanozyme. High catalytic activity and stability can be obtained by regulating the ratio of different metals, which is suitable for antibacterial applications.

Benefits of technology

The bimetallic single-atom quantum dot nanozyme has achieved high catalytic activity and stability. The preparation process is simple and low-cost. It is suitable for large-scale production and industrial promotion and has strong antibacterial ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788349A_ABST
    Figure CN118788349A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of nano-materials, and particularly relates to a preparation method and application of bimetallic monatomic quantum dot nano-enzyme. Ethylenediamine tetraacetic acid chelated metal and ethylenediamine tetraacetic acid are adopted as raw materials, a bimetallic monatomic precursor is prepared through one-step low-temperature pyrolysis, formed metal nanoparticles are removed through soaking with hydrochloric acid, and the bimetallic monatomic quantum dot nano-enzyme can be obtained. The nano-enzyme has the advantages of efficient peroxidase-like activity, high stability, low environmental influence on performance and the like, the preparation method is rapid and simple, reactants are cheap and easy to obtain, and the nano-enzyme can be used for inactivating drug-resistant bacteria in environmental sewage, has good application potential in the fields of environmental monitoring, sewage treatment and the like, and has a wide market application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of nanomaterials, and specifically relates to a preparation method and application of a bimetallic single-atom quantum dot nanozyme. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] As a biocatalyst, natural enzymes play an important role in various biochemical reactions. Due to their inherent disadvantages, such as poor stability, high cost, and easy recognition and removal in the body, their applications are limited to a certain extent. Nanozymes are a type of simulated enzyme that has both the physical properties of nanomaterials and enzyme-like catalytic activity. At present, the application research developed based on the different properties of nanozymes has been very in-depth, and has been widely used in antimicrobial, disease diagnosis and treatment, while other application research is also constantly attracting attention. Nanozymes have efficient catalytic functions, and are heat-resistant, acid-resistant, stable, and easy to mass-produce. In addition, thanks to the progress of nanotechnology, biotechnology, and computational design in recent years, nanozymes can be modified by adding various types of molecules to keep their original properties while obtaining different capabilities. It is these characteristics that make nanozymes widely used as important functional molecules in analytical sensing, disease diagnosis and treatment, environmental protection, and antibacterial.

[0004] Although nanozymes have similar catalytic activity and enzymatic reaction kinetics as natural enzymes. However, compared with the high catalytic activity and high specificity of natural enzymes, the agglomeration of metal ions in their active centers leads to lower catalytic activity, and the lack of biological spatial structure leads to poor substrate selectivity, which cannot meet the requirements of some practical applications. At the same time, the catalytic mechanism of most nanozymes is still unclear, so the research focus is mainly on simulating oxidoreductase activity, but some nanozymes may have multiple types of enzyme activities, which sometimes even interfere with each other and affect their application. In terms of disease treatment, nanozymes are a small molecule nanomaterial, and their biosafety is an important issue. For nanozymes used for wound antibacterial or tumor treatment, safety to the human body is the first priority, so it is necessary to develop low-toxic and metabolizable nanozymes. The superposition of these factors makes the actual application of nanozymes in clinical treatment still have a long way to go.

[0005] Single-atom nanozymes (SAzymes) are a new generation of nanozymes that have developed rapidly in recent years. They have a wide range of applications in biosensing, disease diagnosis and treatment, and bioimaging. Single-atom nanozymes have dispersed single-atom structures and good coordination environments, which to a certain extent solve the problems of low catalytic activity and poor specificity of nanozymes. At present, inspired by the active metal site structure of natural enzymes, researchers have designed and simulated their metal active units at the atomic scale, and have successively developed manganese, cobalt, copper, and iron single-atom nanozymes. These single-atom nanozymes have designable geometric structures and electronic coordination, unique quantum size effects, maximum atomic utilization efficiency, and strong metal-loaded interactions, and have become new materials with catalytic activity and selectivity significantly higher than traditional nanozymes. The current synthesis methods of single-atom nanozymes are relatively complex, usually involving complex chemical reactions, strict condition control, and cumbersome steps. The position of individual atoms needs to be controlled by precise pre-design, which places high demands on synthesis technology. Moreover, the single-atom nanozymes currently synthesized are mainly concentrated in certain specific precious metals (such as Pt and Pd). These materials are expensive, so the synthesized single-atom nanozymes often have low yields, which limits their large-scale production and application.

[0006] In practical applications, due to different requirements for catalytic active centers, a single type of single-atom nanozymes may not be able to meet all application requirements, so more single-atom nanozymes with different active centers are needed. Summary of the invention

[0007] In order to make up for the shortcomings of the prior art, the present invention designs a new type of diatomic metal nanozyme with multiple metal active sites, and improves the enzyme-like activity of the nanozyme by regulating the coordination structure and mode. The dimetallic single-atom quantum dot nanozyme provided by the present invention has good catalytic activity, good stability, and strong antibacterial ability. The preparation method is fast and simple, and the reactants are cheap and easy to obtain. The technical solution provided by the present invention is as follows:

[0008] As a first aspect of the present invention, a method for preparing a bimetallic single-atom quantum dot nanozyme is provided, comprising the following steps: mixing a metal chelate of ethylenediaminetetraacetic acid with ethylenediaminetetraacetic acid, and heating to perform a solid phase reaction; the metal chelate of ethylenediaminetetraacetic acid has a general formula of: C 10 H 12 N2O8XNa2, wherein X is a divalent metal selected from iron, copper, nickel, cobalt and zinc; and the metal chelate of ethylenediaminetetraacetic acid comprises at least two substances.

[0009] Preferably, the metal chelate of EDTA is a salt or a hydrate.

[0010] Preferably, the metal chelate of EDTA comprises sodium iron EDTA and sodium zinc EDTA.

[0011] Preferably, ethylenediaminetetraacetic acid sodium iron, ethylenediaminetetraacetic acid sodium zinc, and ethylenediaminetetraacetic acid are uniformly mixed in a mass ratio of 0.25-1:0.25-1:1-1.5.

[0012] Preferably, ethylenediaminetetraacetic acid sodium iron, ethylenediaminetetraacetic acid sodium zinc, and ethylenediaminetetraacetic acid are uniformly mixed in a mass ratio of 0.25:0.25:1.5.

[0013] Preferably, the heating reaction temperature is 200-600° C., and the solid phase reaction time is 1-10 h.

[0014] Furthermore, after the solid phase reaction, the nanozyme is immersed in 1M to 6M hydrochloric acid for at least 10 hours to remove the formed metal nanoparticles, thereby obtaining the bimetallic single atom quantum dot nanozyme.

[0015] As a second aspect of the present invention, a bimetallic single-atom quantum dot nanozyme prepared by the preparation method is provided.

[0016] Preferably, the nanozyme is a spherical structure with a size of 2 to 5 nm.

[0017] As the third aspect of the present invention, it is to provide the application of the bimetallic single-atom quantum dot nanozyme in sterilization.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The present invention uses ethylenediaminetetraacetic acid sodium iron, ethylenediaminetetraacetic acid sodium zinc, and ethylenediaminetetraacetic acid to perform solid phase synthesis to obtain bimetallic nitrogen atom quantum dot nanozymes with higher performance. The preparation process is rapid, solvent-free, low in energy consumption, and low in pollution, solving the problems of long reaction time and complex preparation conditions of single-atom nanozyme materials. The synthesis method is simple to operate, low in cost, highly practical, does not require the participation of any solvent, and is free from dependence on reaction solvents, and is suitable for mass production and industrial promotion.

[0020] (2) Within the selection range of ethylenediaminetetraacetic acid chelated metal salts, the present invention can obtain single-atom quantum dot nanozyme materials with different bimetallic catalytic active centers by selecting different types of chelated metal salts, which have a bactericidal effect; thus, they can be used in antibacterial applications.

[0021] (3) The inventors unexpectedly discovered in their research that, at a specific ratio, the catalytic activity of the prepared nanozyme is much higher than that of other ratios, and the activity of the nanozyme containing iron atoms is higher than that of other elements; the results of the stability test found that the bimetallic single-atom quantum dot nanozyme provided by the present invention has good stability and can maintain high activity for a long time. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0023] Figure 1 This is a transmission electron microscopy image of the bimetallic single atom quantum dot nanozyme prepared in Example 3 of the present invention;

[0024] Figure 2 This is the X-ray powder diffraction pattern of the bimetallic single atom quantum dot nanozyme prepared in Example 3 of the present invention;

[0025] Figure 3 This is the infrared spectrum of the bimetallic single atom quantum dot nanozyme prepared in Example 3 of the present invention;

[0026] Figure 4 for Figure 3 Fe 0.25 Zn 0.25 EDTA 1.5 (marked as Fe / Zn dot in the figure) is an enlarged view of the infrared spectrum;

[0027] Figure 5 This is the Fe 2p X-ray photoelectron spectrum of the bimetallic single atom quantum dot nanozyme prepared in Example 3 of the present invention;

[0028] Figure 6 The UV-visible absorption spectra of TMB catalyzed by bimetallic single atom quantum dot nanozymes with different metal ratios in Experimental Example 1 of the present invention;

[0029] Figure 7 This is a diagram showing the stability evaluation results of the bimetallic single atom quantum dot nanozyme in Experimental Example 2 of the present invention;

[0030] Figure 8 This is a graph showing the evaluation results of the bactericidal effect of the bimetallic single atom quantum dot nanozyme in Experimental Example 3 of the present invention;

[0031] Fig. 9 This is the UV-visible absorption spectrum of TMB catalyzed by the nanozyme of EDTA obtained in Comparative Example 1 of the present invention;

[0032] Fig.10 This is a graph showing the evaluation results of the sterilization effect without adding any material in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0033] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0034] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0035] Embodiment 1:

[0036] Weigh 1g of sodium iron ethylenediaminetetraacetate and 1g of sodium zinc ethylenediaminetetraacetate, place in a sample bottle, vortex for 3-5 minutes, mix thoroughly, spread in a porcelain boat, place in a tube furnace, heat to 300℃ at a rate of 5℃ / min in a nitrogen atmosphere, and calcine at 300℃ for 2h. Collect the product after natural cooling. Record as Fe1Zn1. Then soak in 6M hydrochloric acid for at least 10h; if the hydrochloric acid concentration is lower, extend the soaking time or increase the number of soaking times.

[0037] Embodiment 2:

[0038] Weigh 0.5g of sodium iron ethylenediaminetetraacetate, 1g of sodium zinc ethylenediaminetetraacetate and 1g of ethylenediaminetetraacetic acid, place in a sample bottle, vortex for 3-5min, mix thoroughly, spread in a porcelain boat, place in a tube furnace, heat to 300℃ at a rate of 5℃ / min in a nitrogen atmosphere, and calcine at 300℃ for 2h. Collect the product after natural cooling. Recorded as Fe 0.5 Zn1EDTA1. Then soak in 6M hydrochloric acid for at least 10 hours.

[0039] Embodiment 3:

[0040] Weigh 0.25g of sodium iron ethylenediaminetetraacetate, 0.25g of sodium zinc ethylenediaminetetraacetate and 1.5g of ethylenediaminetetraacetic acid, place in a sample bottle, vortex for 3-5min, mix thoroughly, spread in a porcelain boat, place in a tube furnace, heat to 300℃ at a rate of 5℃ / min in a nitrogen atmosphere, and calcine at 300℃ for 2h. Collect the product after natural cooling. Recorded as Fe 0.25 Zn 0.25 EDTA 1.5 . Then soak in 6M hydrochloric acid for 10 hours.

[0041] from Figure 1 , 2 It can be seen from the scanning electron microscope image and powder diffraction spectrum that the material has uniform morphology, a particle size distribution of 2-5nm, and has a 002 crystal plane corresponding to the graphite structure.

[0042] Figure 3 The raw materials are sodium iron ethylenediaminetetraacetate (labeled as FeNaEDTA in the figure), 0.25g sodium zinc ethylenediaminetetraacetate (labeled as ZnNaEDTA in the figure), ethylenediaminetetraacetic acid (labeled as EDTA in the figure), and Fe 0.25 Zn 0.25 EDTA 1.5 The infrared spectrum of the Fe / Zn dot is shown in the figure. Figure 3 It can be seen from the infrared spectrum that the product material produces characteristic peaks that are different from the raw materials. The enlarged image is shown in Figure 4 As shown, it indicates the successful synthesis of the new material.

[0043] from Figure 5 From the X-ray photoelectron spectroscopy test results, there is an obvious Fe2p orbital peak, indicating that the Fe element has been successfully doped into the material.

[0044] Embodiment 4:

[0045] Weigh 1g of sodium copper ethylenediaminetetraacetate and 1g of sodium zinc ethylenediaminetetraacetate, place in a sample bottle, vortex for 3-5 minutes, mix thoroughly, spread in a porcelain boat, place in a tube furnace, heat to 300℃ at a rate of 5℃ / min in a nitrogen atmosphere, and calcine at 300℃ for 2h. Collect the product after natural cooling. Record as Cu1Zn1. Then soak in 6M hydrochloric acid for at least 10h.

[0046] Embodiment 5:

[0047] Weigh 0.5g of sodium copper ethylenediaminetetraacetate, 1g of sodium zinc ethylenediaminetetraacetate and 1g of ethylenediaminetetraacetic acid, place in a sample bottle, vortex for 3-5min, mix thoroughly, spread in a porcelain boat, place in a tube furnace, heat to 300℃ at a rate of 5℃ / min in a nitrogen atmosphere, and calcine at 300℃ for 2h. Collect the product after natural cooling. Record as Cu1Zn1EDTA1. Then soak in 6M hydrochloric acid for at least 10h.

[0048] Test Example 1

[0049] Among the methods for evaluating the catalytic activity of nanozymes, the most widely used method is colorimetry. Commonly used colorimetric substrates include 3,3,5,5-tetramethylbenzidine (TMB), o-phenylenediamine (OPD) and 2,2'-azido-bis-(3-ethylbenzothiazoline-6-sulfonic acid) (ABTS), etc., which produce corresponding color reactions under the catalysis of specific enzymes, thereby intuitively characterizing the enzyme activity and enzyme catalytic kinetic constants (based on the typical Michaelis–

[0050] Menten kinetic method). In this test example, TMB was used as the enzymatic substrate, and the oxidation of TMB in the presence of H2O2 was monitored to study the peroxidase-like activity of the bimetallic single-atom quantum dot nanozymes with different metal ratios prepared in each example.

[0051] The UV-visible absorption spectra of TMB catalyzed by the bimetallic single atom quantum dot nanozymes with different metal ratios prepared in Examples 1, 2, 3, 4, and 5 of the present invention are as follows: Figure 6 As shown, the curves include hydrogen peroxide + Fe1Zn1, hydrogen peroxide + Cu1Zn1, hydrogen peroxide + Fe 0.5 Zn1EDTA1, hydrogen peroxide + Fe 0.25 Zn 0.25 EDTA 1.5 , Hydrogen Peroxide

[0052] +Cu1Zn1EDTA1. The results show that adding Fe 0.25 Zn 0.25 EDTA 1.5 It showed the highest UV absorption intensity, that is, the highest peroxidase-like activity. This may be because the iron atom doping achieved the regulation of the diatomic d-band center, enhanced the affinity between the dimetallic atomic position and the substrate, and thus greatly improved the catalytic activity of the multi-enzyme.

[0053] Test Example 2

[0054] The stability of the bimetallic single-atom quantum dot nanozyme prepared in Example 3 was evaluated. After the prepared materials were stored at room temperature for 1 month, 3 months, and 6 months, TMB was used as the enzymatic substrate, and the changes in the peroxidase-like activity were evaluated by monitoring the UV-visible absorption spectra under the same material concentration, the same H2O2 and TMB concentrations. Figure 7 As shown, the results showed that the UV absorption intensity did not change significantly, indicating that the nanozyme can maintain high activity for a long time.

[0055] Experimental Example 3: Evaluation of the bactericidal effect of the bimetallic single atom quantum dot nanozyme prepared in Example 3

[0056] Prepare Fe with a concentration of 100 μg / mL using 0.1 M sodium acetate buffer as solvent. 0.25 Zn 0.25 EDTA 1.5 The mother solution is reserved. 100 μL of E. coli solution, 100 μL of Fe 0.25 Zn 0.25 EDTA 1.5The mother solution, 100 μL hydrogen peroxide solution, and 700 μL sodium acetate buffer were mixed and placed in a shaker at 180 rpm and incubated at 37°C for 1 hour. 100 μL of the mixture was then applied to a plate and placed in a 37°C oven for incubation for 24 hours. The plate was then observed and photographed. Figure 8 As shown, the results showed that no bacterial colonies were observed on the surface of the culture plate and bacterial growth was completely inhibited, indicating that the material has a good bactericidal effect.

[0057] Comparative Example 1:

[0058] The difference between this comparative example and Example 4 is that no ethylenediaminetetraacetic acid chelated metal salt is added during feeding.

[0059] Weigh 1.5g of ethylenediaminetetraacetic acid, place it in a sample bottle, vortex for 3-5 minutes, mix thoroughly, spread it in a porcelain boat, place it in a tube furnace, heat it to 300℃ at a rate of 5℃ / min in a nitrogen atmosphere, and calcine it at 300℃ for 2h. Collect the product after natural cooling. It is recorded as EDTA. The obtained material is a black powder. Under the same test conditions, in the peroxidase-like performance evaluation experiment, Fig. 9 As shown, the absorbance was lower than 0.2, indicating that the activity of EDTA-based peroxidase was extremely poor.

[0060] Comparative Example 2:

[0061] After mixing 100 μL of E. coli solution, 100 μL of hydrogen peroxide solution, and 800 μL of sodium acetate buffer, the mixture was placed in a shaker at 180 rpm and incubated at 37°C for 1 hour. Then 100 μL of the mixture was spread on a plate and placed in a 37°C oven for incubation for 24 hours. The mixture was observed and photographed. Fig.10 As shown, the results showed that when no material was added, the bacteria still grew normally and covered the entire culture plate.

[0062] Comparative Example 3:

[0063] Take the product EDTA prepared in Comparative Example 1 without ethylenediaminetetraacetic acid chelated metal salt, and prepare a 100 μg / mL EDTA stock solution with 0.1M sodium acetate buffer as solvent for use. Mix 100 μL of Escherichia coli solution, 100 μL of EDTA stock solution, 100 μL of hydrogen peroxide solution, and 700 μL of sodium acetate buffer, place them in a shaker, 180 rpm, incubate at 37°C for 1 hour, take 100 μL of the coated plate, place it in a 37°C oven for incubation for 24 hours, observe and take pictures. It was found that the results were the same as those in Comparative Example 2. The bacteria still grew normally when only the EDTA material was added, and the bactericidal effect could not be achieved.

[0064] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a bimetallic single-atom quantum dot nanozyme, It is characterized in that The method comprises the following steps: mixing a metal chelate of ethylenediaminetetraacetic acid with ethylenediaminetetraacetic acid, and heating the mixture to carry out a solid phase reaction; the metal chelate of ethylenediaminetetraacetic acid has the general formula: C 10 H 12 N 2 O 8 XOt 2 , wherein X is a divalent metal selected from iron, copper, nickel, cobalt, and zinc; and the metal chelate of ethylenediaminetetraacetic acid comprises at least two substances.

2. The preparation method according to claim 1, It is characterized in that The metal chelate of EDTA is a salt or a hydrate.

3. The preparation method according to claim 1, It is characterized in that Metal chelates of EDTA include sodium iron EDTA and sodium zinc EDTA.

4. The preparation method according to claim 1, It is characterized in that Ethylenediaminetetraacetic acid sodium iron, ethylenediaminetetraacetic acid sodium zinc, and ethylenediaminetetraacetic acid are uniformly mixed in a mass ratio of 0.25-1:0.25-1:1-1.

5.

5. The preparation method according to claim 1, It is characterized in that Sodium iron ethylenediaminetetraacetate, sodium zinc ethylenediaminetetraacetate, and ethylenediaminetetraacetic acid are evenly mixed in a mass ratio of 0.25:0.25:1.

5.

6. The preparation method according to claim 1, It is characterized in that The temperature of the heating reaction is 200-600° C., and the solid phase reaction time is 1-10 hours.

7. The preparation method according to claim 1, It is characterized in that After the solid phase reaction, the bimetallic single atom quantum dot nanozyme is obtained by soaking in 1M to 6M hydrochloric acid for at least 10 hours to remove the formed metal nanoparticles.

8. The bimetallic single atom quantum dot nanozyme prepared by the preparation method according to any one of claims 1 to 7.

9. The bimetallic single-atom quantum dot nanozyme according to claim 8, It is characterized in that It is a spherical structure with a size of 2 to 5 nm.

10. Application of the bimetallic single-atom quantum dot nanozyme according to claim 8 in sterilization.

Citation Information

Patent Citations

  • Application of metal doped carbon dots

    CN110327980A

  • Preparation and application of nickel-iron co-doped carbon dot nano enzyme

    CN117819529A