Environment-friendly catalytic hydrogenation olefin removal process and application thereof

By using aluminum nitride catalysts loaded with active metals and carbon powder in the catalytic reforming reaction, the problem of high olefin content in the catalytic reforming reaction is solved, efficient removal and long-life catalysts are achieved, the risk of environmental pollution is reduced, and the An environmentally friendly solution.

CN118788375AActive Publication Date: 2024-10-18NINGXIA BAOTING NEW ENERGY CO LTD +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410856320.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-18
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively reduce the olefin content in the reformed oil and raffinate oil during the catalytic reforming reaction, resulting in unqualified product quality and environmental pollution risks.

Method used

An environmentally friendly catalytic hydrogenation deolefinization process is adopted. The catalyst is prepared by loading active metal and carbon powder on the aluminum nitride carrier, and roasting it after electromagnetic coil pretreatment to form an aluminum oxide/aluminum nitride composite carrier to improve the catalyst's performance. activity and longevity.

Benefits of technology

It achieves efficient removal of olefins from the reformed oil and reduces the risk of environmental pollution. The catalyst has high activity and long life, with a single service life of more than 4 years. The process is environmentally friendly and avoids the depth difference and failure of the clay refining method. Happy question.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788375A_ABST
    Figure CN118788375A_ABST
Patent Text Reader

Abstract

The invention discloses an environment-friendly catalytic hydrogenation olefin removal process and application thereof, reformate is heated and then enters a hydrogenation reactor, PSA hydrogen is heated and then enters the bottom of the hydrogenation reactor, and the PSA hydrogen and the reformate are efficiently mixed to form a mixed material; enabling the mixed material to flow through a catalyst bed layer in the hydrogenation reactor from bottom to top, carrying out hydrogenation reaction under the action of a catalyst, extracting a reaction product from the top of the hydrogenation reactor, conveying the reaction product to a stabilization tower, and discharging a reaction excess gas phase extracted from the top of the stabilization tower into a gas phase recovery system through a reflux tank, part of refined oil extracted from the bottom of the stabilizing tower flows back to the stabilizing tower, and part of essential oil enters an aromatic hydrocarbon system after heat exchange. The unique hydrogenation catalyst is adopted to perform hydrogenation catalysis on the reformate to achieve the purpose of olefin removal, the defects of poor depth, high heavy component yield, quick clay inactivation and the like of clay refining treatment are overcome, and compared with an existing clay refining treatment method, the method has the advantages that the environmental pollution is small, and the method belongs to an environment-friendly olefin removal process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of petrochemical processes, and in particular to an environmentally friendly catalytic hydrogenation deolefination process and application thereof. Background Art

[0002] Aromatic hydrocarbons such as benzene, toluene, mixed xylene, and industrial carbon nine aromatics are important organic chemical raw materials. These aromatic hydrocarbon products are mainly derived from the catalytic reforming reaction of refined coal tar and naphtha. The reforming reaction product oil is rich in aromatic hydrocarbons and also contains a certain amount of olefin impurities. To produce qualified benzene, toluene, mixed xylene and other aromatic hydrocarbon products, the olefin impurities must be removed. Otherwise, the bromine index, pickling colorimetry, chromaticity and copper sheet corrosion of the aromatic hydrocarbon products are all unqualified, and the downstream equipment cannot meet the requirements of the quality of aromatic hydrocarbon products. At the same time, the olefins in the reforming reaction product oil will polymerize in the subsequent aromatic hydrocarbon extraction solvent and cause solvent pollution. The oxidation of olefins into organic acids can cause corrosion of the extraction system equipment. Olefins are also easy to cause scaling and coking, blocking pipelines. In the process of high-severity catalytic reforming reaction, the olefin content of the reaction product oil will exceed 1w%, and the olefin content of the raffinate oil will exceed 5w%. Therefore, how to reduce the olefin content in the reforming reaction product oil and the raffinate oil is a practical problem that needs to be solved in the industry.

[0003] At present, the industry generally adopts treatment processes such as bleached clay, modified bleached clay or molecular sieve refining agents. This process has problems such as poor refining depth, high yield of heavy components, and rapid deactivation of bleached clay. In particular, the disposal of deactivated bleached clay has serious environmental pollution risks, which puts refining companies under tremendous environmental pressure. In addition, the conventional dry point of the heavy components produced by the superposition and condensation of mixed aromatics and olefins reaches 350℃, which cannot be effectively utilized and has also become a problem for factory processing. Summary of the invention

[0004] The purpose of the present invention is to provide an environmentally friendly catalytic hydrogenation deolefination process and its application to solve the problem of using a clay refining method in the prior art.

[0005] In order to solve the above-mentioned technical problems, the present invention adopts the following technical solution: a hydrogenation catalyst is prepared by the following preparation method:

[0006] S1, taking aluminum nitride powder and calcining it at 150-230° C. under an inert atmosphere to obtain an aluminum nitride carrier;

[0007] S2, mixing the metal salt, polyvinyl alcohol and carbon powder aqueous solution and uniformly dispersing them by ultrasonication, placing the mixture in a freeze dryer for freeze drying to obtain active powder;

[0008] S3, mixing the active powder with deionized water to obtain an impregnation solution, and adding the aluminum nitride support obtained in step S1 into the impregnation solution for impregnation treatment;

[0009] S4, placing the aluminum nitride carrier after the impregnation treatment in a reaction container, winding an electromagnetic coil around the outside of the reaction container, and turning on the electromagnetic coil for pretreatment in an air or oxygen atmosphere to obtain a precursor;

[0010] S5. The precursor is transferred to a sintering furnace and calcined at 600-1000° C. in an inert gas atmosphere to obtain a catalyst.

[0011] Preferably, the metal salt is one or any mixture of nickel nitrate, nickel acetate, cobalt nitrate, cobalt acetate, molybdenum nitrate and molybdenum acetate.

[0012] Preferably, the active metal component in the catalyst accounts for 0.5 to 8% of the total mass of the catalyst.

[0013] Preferably, the amount of carbon powder added is 1-5% of the weight of the aluminum nitride carrier.

[0014] Preferably, the power of the electromagnetic coil during the pretreatment process is 2 to 4 kW.

[0015] The present invention also provides an environmentally friendly catalytic hydrogenation deolefination process, the specific process is as follows:

[0016] The reformed oil first enters the bottom of the hydrogenation reactor after being heated by heat exchange, and the PSA hydrogen enters the bottom of the hydrogenation reactor after being heated, and is efficiently mixed with the reformed oil at the bottom of the reactor to form a mixed material;

[0017] The mixed material flows from bottom to top through the catalyst bed in the hydrogenation reactor, the catalyst bed is filled with the above catalyst, and a hydrogenation reaction occurs under the action of the catalyst to obtain a reaction product;

[0018] The reaction product is extracted from the top of the hydrogenation reactor and transported to the stabilization tower. The excess reaction gas extracted from the top of the stabilization tower is discharged into the gas phase recovery system after passing through the reflux tank. Part of the refined oil extracted from the bottom of the stabilization tower is refluxed to the stabilization tower, and part of the refined oil enters the aromatic system after heat exchange.

[0019] Preferably, the preparation method of the catalyst is as follows:

[0020] Preferably, the reformed oil is heated to 130-170° C. in a first heat exchanger and then enters the bottom of the hydrogenation reactor.

[0021] Preferably, part of the refined oil produced from the bottom of the stabilization tower is refluxed to the stabilization tower via a condenser.

[0022] Preferably, part of the refined oil produced from the bottom of the stabilization tower is firstly heat exchanged with the reaction product produced from the top of the hydrogenation reactor through the second heat exchanger, and then heat exchanged with the reforming oil through the first heat exchanger before entering the aromatic system.

[0023] The present invention has the following beneficial effects:

[0024] 1. The present invention adopts a unique hydrogenation catalyst to hydrogenate the reformed oil to achieve the purpose of deolefination, which solves the defects of poor depth, high yield of heavy components, and rapid deactivation of clay through clay refining treatment. Compared with the existing clay refining treatment method, it has less environmental pollution and belongs to an environmentally friendly deolefination process;

[0025] 2. In the preparation process of the catalyst of the present invention, the active metal is loaded onto carbon powder, and then the carbon powder is loaded onto an aluminum nitride carrier by impregnation, which can avoid the aggregation of the active metal on the aluminum nitride carrier. In addition, a special pretreatment is performed before roasting. The aluminum nitride carrier after the impregnation treatment is loaded with carbon powder, and the carbon powder can be rapidly heated under the action of the electromagnetic coil. In this process, the aluminum nitride produces a carbon thermal reduction reaction, and part of the aluminum nitride is converted into aluminum. The aluminum further reacts with oxygen to form aluminum oxide, and an aluminum oxide / aluminum nitride composite carrier is formed after pretreatment. On the one hand, the carbon powder provides the heat required for the reaction under the action of the electromagnetic coil, and on the other hand, it participates in the conversion of aluminum nitride as a reducing agent. The catalyst finally obtained has the active metal loaded on the composite carrier of aluminum oxide and aluminum nitride. The aluminum nitride and aluminum oxide have a disordered, chaotic, polymorphic, mutually nested, hyperbolic composite porous structure, and the specific surface area and pore volume are improved. The catalyst has high activity, good reaction selection, and long service life. The single service life is expected to reach more than 4 years. And because the microporous structure of the carrier has higher strength and thermal conductivity, the structure will not collapse when the carbon is burned when the catalyst is revived. It also has fast thermal conductivity, controllable reaction, high revivification efficiency, and can be revived multiple times. New long-life, reusable catalysts can be developed to solve the industry's technical problems of short life and few revivals of existing catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The figure is a schematic diagram of the process flow of the catalytic hydrogenation deolefination process of the present invention. DETAILED DESCRIPTION

[0027] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with embodiments, but the content of the present invention is not limited to the following embodiments.

[0028] Hydrogenation reaction refers to the chemical reaction of a substance with hydrogen under hydrogenation conditions to produce the corresponding hydrogenation product. Hydrogenation reaction is an exothermic reaction, that is, the reaction is thermodynamically favorable. This is because during the hydrogenation process, the formation of carbon-hydrogen bonds and hydrogen-hydrogen bonds will release energy, thereby causing the reaction to proceed in the direction of producing more stable compounds. Since the rate of hydrogenation reaction is usually slow, a catalyst is needed to increase the reaction rate. The catalyst is usually a material that can adsorb hydrogen and reactant molecules and provide a suitable reaction surface to promote the reaction.

[0029] The impregnation method for preparing hydrogenation catalysts is to immerse the support material in the catalyst precursor solution to allow it to fully absorb the catalyst precursor, and then convert the precursor into an active component through steps such as drying and calcination. This method is suitable for the preparation of most catalysts and has the advantages of simple operation and stable production process.

[0030] The hydrogenation catalyst of the present invention is prepared based on an impregnation method, and the specific preparation process is as follows:

[0031] S1, taking aluminum nitride powder and calcining it at 150-230° C. for 1-3 h in an inert atmosphere to obtain an aluminum nitride carrier;

[0032] S2, mixing the metal salt, polyvinyl alcohol and carbon powder aqueous solution and uniformly dispersing them by ultrasonication, placing the mixture in a freeze dryer for freeze drying to obtain active powder;

[0033] The active powder is a powder obtained by loading the active metal onto the carbon powder. The freeze-drying method helps to disperse the active metal onto the carbon powder and avoid agglomeration of the active metal.

[0034] The metal salt is one of nickel nitrate, nickel acetate, cobalt nitrate, cobalt acetate, molybdenum nitrate and molybdenum acetate or any mixture thereof. The amount of carbon powder added is 1-5% of the weight of the aluminum nitride carrier.

[0035] S3, mixing the active powder with deionized water to obtain an impregnation solution, and adding the aluminum nitride support obtained in step S1 into the impregnation solution for impregnation treatment;

[0036] S4. Place the aluminum nitride carrier after the impregnation treatment in a reaction container, wind an electromagnetic coil around the outside of the reaction container, and turn on the electromagnetic coil for pretreatment in an air or oxygen atmosphere to obtain a precursor.

[0037] During the pretreatment process, the power of the electromagnetic coil is 2-4KW, and the treatment time is 5-15min.

[0038] After the impregnation treatment, the aluminum nitride carrier is loaded with carbon powder, which can be rapidly heated under the action of the electromagnetic coil. During this process, the aluminum nitride undergoes a carbon thermal reduction reaction, and part of the aluminum nitride is converted into aluminum. The aluminum further reacts with oxygen to form aluminum oxide, and after pretreatment, an aluminum oxide / aluminum nitride composite carrier is formed.

[0039] S5. The precursor is transferred to a sintering furnace and calcined for 4-8 hours at 600-1000° C. in an inert gas atmosphere to obtain a catalyst. The active metal component in the catalyst accounts for 0.5-8% of the total mass of the catalyst.

[0040] Example 1

[0041] S1, taking aluminum nitride powder and calcining it at 150° C. for 3 h in an inert atmosphere to obtain an aluminum nitride carrier;

[0042] S2, mixing nickel nitrate, polyvinyl alcohol and carbon powder aqueous solution, and evenly dispersing them by ultrasonication, placing the mixture in a freeze dryer for freeze drying to obtain active powder;

[0043] The carbon powder is XC-72, and the added amount of the carbon powder is 1% of the weight of the aluminum nitride carrier.

[0044] S3, taking the active powder and mixing it with deionized water to obtain an impregnation solution (one-time saturation impregnation method), adding the aluminum nitride support prepared in step S1 into the impregnation solution for impregnation treatment;

[0045] S4, placing the aluminum nitride carrier after the impregnation treatment in a reaction container, winding an electromagnetic coil on the outside of the reaction container, and turning on the electromagnetic coil for pretreatment in an air or oxygen atmosphere (power is 2KW, treatment time is 15min) to obtain a precursor;

[0046] S5. The precursor is transferred to a sintering furnace and calcined at 600° C. for 8 hours in an inert gas atmosphere to obtain a catalyst. The active metal component in the catalyst accounts for 1% of the total mass of the catalyst.

[0047] Example 2

[0048] S1, taking aluminum nitride powder and calcining it at 230° C. for 1 h in an inert atmosphere to obtain an aluminum nitride carrier;

[0049] S2, mixing cobalt acetate, polyvinyl alcohol and carbon powder aqueous solution, and evenly dispersing by ultrasonication, placing the mixture in a freeze dryer for freeze drying to obtain active powder;

[0050] The carbon powder is XC-72, and the added amount of the carbon powder is 5% of the weight of the aluminum nitride carrier.

[0051] S3, taking the active powder and mixing it with deionized water to obtain an impregnation solution (one-time saturation impregnation method), adding the aluminum nitride support prepared in step S1 into the impregnation solution for impregnation treatment;

[0052] S4, placing the aluminum nitride carrier after the impregnation treatment in a reaction container, winding an electromagnetic coil on the outside of the reaction container, and turning on the electromagnetic coil for pretreatment in an air or oxygen atmosphere (power is 4KW, treatment time is 5min) to obtain a precursor;

[0053] S5. The precursor is transferred to a sintering furnace and calcined at 1000° C. for 4 hours in an inert gas atmosphere to obtain a catalyst. The active metal component in the catalyst accounts for 8% of the total mass of the catalyst.

[0054] Example 3

[0055] S1, taking aluminum nitride powder and calcining it at 200° C. for 2 h in an inert atmosphere to obtain an aluminum nitride carrier;

[0056] S2, mixing molybdenum acetate, polyvinyl alcohol and carbon powder aqueous solution, and evenly dispersing by ultrasonication, placing the mixture in a freeze dryer for freeze drying to obtain active powder;

[0057] The carbon powder is XC-72, and the added amount of the carbon powder is 2% of the weight of the aluminum nitride carrier.

[0058] S3, taking the active powder and mixing it with deionized water to obtain an impregnation solution (one-time saturation impregnation method), adding the aluminum nitride support prepared in step S1 into the impregnation solution for impregnation treatment;

[0059] S4, placing the aluminum nitride carrier after the impregnation treatment in a reaction container, winding an electromagnetic coil around the outside of the reaction container, and turning on the electromagnetic coil for pretreatment in an air or oxygen atmosphere (power is 3KW, treatment time is 10min) to obtain a precursor;

[0060] S5. The precursor is transferred to a sintering furnace and calcined at 800° C. in an inert gas atmosphere to obtain a catalyst. The active metal component in the catalyst accounts for 2.5% of the total mass of the catalyst.

[0061] Example 4

[0062] S1, taking aluminum nitride powder and calcining it at 180° C. for 2.5 h in an inert atmosphere to obtain an aluminum nitride carrier;

[0063] S2, mixing nickel acetate, molybdenum nitrate, polyvinyl alcohol and carbon powder aqueous solution, and evenly dispersing by ultrasonication, placing the mixture in a freeze dryer for freeze drying to obtain active powder;

[0064] The carbon powder is XC-72, and the added amount of the carbon powder is 1.5% of the weight of the aluminum nitride carrier.

[0065] S3, taking the active powder and mixing it with deionized water to obtain an impregnation solution (one-time saturation impregnation method), adding the aluminum nitride support prepared in step S1 into the impregnation solution for impregnation treatment;

[0066] S4, placing the aluminum nitride carrier after the impregnation treatment in a reaction container, winding an electromagnetic coil on the outside of the reaction container, and turning on the electromagnetic coil for pretreatment in an air or oxygen atmosphere (power is 2.5KW, and the treatment time is 12min) to obtain a precursor;

[0067] S5. The precursor is transferred to a sintering furnace and calcined at 700° C. for 8 hours in an inert gas atmosphere to obtain a catalyst. The active metal component in the catalyst accounts for 0.6% of the total mass of the catalyst.

[0068] Example 5

[0069] S1, taking aluminum nitride powder and calcining it at 150° C. for 3 h in an inert atmosphere to obtain an aluminum nitride carrier;

[0070] S2, mixing nickel nitrate, cobalt nitrate, molybdenum acetate, polyvinyl alcohol and carbon powder aqueous solution, and evenly dispersing by ultrasonication, placing the mixture in a freeze dryer for freeze drying to obtain active powder;

[0071] The carbon powder is XC-72, and the added amount of the carbon powder is 2.2% of the weight of the aluminum nitride carrier.

[0072] S3, taking the active powder and mixing it with deionized water to obtain an impregnation solution (one-time saturation impregnation method), adding the aluminum nitride support prepared in step S1 into the impregnation solution for impregnation treatment;

[0073] S4, placing the aluminum nitride carrier after the impregnation treatment in a reaction container, winding an electromagnetic coil around the outside of the reaction container, and turning on the electromagnetic coil for pretreatment in an air or oxygen atmosphere (power is 1.8KW, and the treatment time is 14min) to obtain a precursor;

[0074] S5. The precursor is transferred to a sintering furnace and calcined at 7500° C. for 8 hours in an inert gas atmosphere to obtain a catalyst. The active metal component in the catalyst accounts for 1.2% of the total mass of the catalyst.

[0075] Example 6

[0076] An environmentally friendly catalytic hydrodeolefination process, as follows:

[0077] The reformed oil first enters the bottom of the hydrogenation reactor after being heated by heat exchange, and the PSA hydrogen enters the bottom of the hydrogenation reactor after being heated, and is efficiently mixed with the reformed oil at the bottom of the reactor to form a mixed material;

[0078] The mixed material flows from bottom to top through the catalyst bed in the hydrogenation reactor, and the catalyst bed is filled with the catalyst of Example 1 (the packing density of the catalyst in the hydrogenation reactor is 0.55 t / m 3 ; The upper and lower parts of the hydrogenation reactor are filled with porcelain balls, and the middle part is filled with catalysts), and hydrogenation reaction occurs under the action of the catalyst to obtain reaction products;

[0079] The reaction product is extracted from the top of the hydrogenation reactor and transported to the stabilization tower. The excess reaction gas extracted from the top of the stabilization tower is discharged into the gas phase recovery system after passing through the reflux tank. Part of the refined oil extracted from the bottom of the stabilization tower is refluxed to the stabilization tower, and part of the refined oil enters the aromatic system after heat exchange.

[0080] The reformed oil is heated to 130-170°C in the first heat exchanger and then enters the bottom of the hydrogenation reactor.

[0081] Part of the refined oil produced from the bottom of the stabilization tower is refluxed to the stabilization tower through the condenser.

[0082] Part of the refined oil produced from the bottom of the stabilization tower first passes through the second heat exchanger to exchange heat with the reaction product produced from the top of the hydrogenation reactor, and then passes through the first heat exchanger to exchange heat with the reforming oil before entering the aromatic system.

[0083] The hydrogen-to-oil ratio of the hydrogenation reactor is 2 to 6:1.

[0084] The process flow diagram is shown in Figure 1 In the catalytic hydrodeolefination process, the olefins in the reformed oil mainly undergo the following chemical reactions:

[0085] (1) Monoolefin hydrogenation reaction

[0086] R1-CH=CH-R2+H2→R1-CH2-CH2-R2

[0087] (2) Diolefin hydrogenation reaction

[0088] R1-CH=CH-CH=CH-R2+H2→R1-(CH2)4-R2

[0089] (3) Hydrocracking reaction

[0090] R1-CH2-CH2-R2+H2→R1-CH3+R2-CH3

[0091] (4) Aromatic Hydrogenation Saturation Reaction

[0092] C n H 2n-6 +3H2→C n H 2n

[0093] Catalytic hydrogenation catalysts can accelerate reactions (1) and (2) and inhibit reactions (3) and (4).

[0094] After re-contact and dechlorination, the reformed oil is heat-exchanged to the reaction temperature (130-170°C) through the stabilizer feed / tower bottom heat exchanger and enters the bottom of the deolefination reactor. The hydrogen from PSA also enters the bottom of the reactor after removing iron filings and other particulate impurities through the filter, and is efficiently mixed with the raw oil in the mixing section at the bottom of the reactor. The mixed material flows from bottom to top through the catalyst bed in the tubular reactor, and a hydrogenation reaction occurs under the action of the catalyst. The reaction product is controlled by the reactor outlet regulating valve, and then further heat-exchanged with the stabilizer bottom oil and enters the stabilizer. The excess gas phase of the reaction is discharged from the top of the stabilizer reflux tank into the gas phase recovery system, and the refined oil at the bottom of the tower enters the aromatics unit to produce aromatic products. A bypass is set at the reactor outlet heat exchanger to adjust the distribution of the heat exchange load to meet the reactor inlet temperature adjustment needs. The amount of hydrogen supplemented by the reaction is controlled at a ratio of 2-6:1 to the raw material volume, and the reaction pressure comes from the self-pressure pressure of the re-contact tank.

[0095] The decolorization effect of the reforming oil is obvious. The bromine index of the reaction product can be reduced from 5000mgBr / 100g to below 200mgBr / 100g. The olefin removal rate of the reaction product is greater than 98%, and the aromatic loss is less than 0.2%. No heavy aromatics are generated during the reaction process, and PX-grade xylene (bromine index less than 50mgBr / 100g) can be produced.

[0096] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A hydrogenation catalyst, characterized in that Prepared by the following preparation method: S1, taking aluminum nitride powder and calcining it at 150-230° C. under an inert atmosphere to obtain an aluminum nitride carrier; S2, mixing the metal salt, polyvinyl alcohol and carbon powder aqueous solution and uniformly dispersing them by ultrasonication, placing the mixture in a freeze dryer for freeze drying to obtain active powder; S3, mixing the active powder with deionized water to obtain an impregnation solution, and adding the aluminum nitride support obtained in step S1 into the impregnation solution for impregnation treatment; S4, placing the aluminum nitride carrier after the impregnation treatment in a reaction container, winding an electromagnetic coil around the outside of the reaction container, and turning on the electromagnetic coil for pretreatment in an air or oxygen atmosphere to obtain a precursor; S5. The precursor is transferred to a sintering furnace and calcined at 600-1000° C. in an inert gas atmosphere to obtain a catalyst.

2. A hydrogenation catalyst as claimed in claim 1, characterized in that The metal salt is one of nickel nitrate, nickel acetate, cobalt nitrate, cobalt acetate, molybdenum nitrate and molybdenum acetate, or any mixture thereof.

3. A hydrogenation catalyst as claimed in claim 1, characterized in that The active metal component in the catalyst accounts for 0.5 to 8% of the total mass of the catalyst.

4. A hydrogenation catalyst as claimed in claim 1, characterized in that The added amount of carbon powder is 1-5% of the weight of the aluminum nitride carrier.

5. A hydrogenation catalyst as claimed in claim 1, characterized in that: The power of the electromagnetic coil during the pretreatment process is 2 to 4KW.

6. An environmentally friendly catalytic hydrodeolefination process, characterized in that: The specific process is as follows: The reformed oil first enters the bottom of the hydrogenation reactor after being heated by heat exchange, and the PSA hydrogen enters the bottom of the hydrogenation reactor after being heated, and is efficiently mixed with the reformed oil at the bottom of the reactor to form a mixed material; The mixed material flows from bottom to top through the catalyst bed in the hydrogenation reactor, the catalyst bed is filled with the catalyst described in any one of claims 1 to 5, and a hydrogenation reaction occurs under the action of the catalyst to obtain a reaction product; The reaction product is extracted from the top of the hydrogenation reactor and transported to the stabilization tower. The excess reaction gas extracted from the top of the stabilization tower is discharged into the gas phase recovery system after passing through the reflux tank. Part of the refined oil extracted from the bottom of the stabilization tower is refluxed to the stabilization tower, and part of the refined oil enters the aromatic system after heat exchange.

7. An environmentally friendly catalytic hydrodeolefination process as claimed in claim 6, characterized in that: The reformed oil is heated to 130-170° C. in the first heat exchanger and then enters the bottom of the hydrogenation reactor. The hydrogen-to-oil ratio of the hydrogenation reactor is 2-6:

1.

8. An environmentally friendly catalytic hydrodeolefination process as claimed in claim 6, characterized in that: Part of the refined oil produced from the bottom of the stabilization tower is refluxed to the stabilization tower through a condenser.

9. An environmentally friendly catalytic hydrodeolefination process as claimed in claim 6, characterized in that: Part of the refined oil produced from the bottom of the stabilization tower first passes through the second heat exchanger to exchange heat with the reaction product produced from the top of the hydrogenation reactor, and then passes through the first heat exchanger to exchange heat with the reforming oil before entering the aromatic system.

10. Use of the hydrogenation catalyst as claimed in claim 1 in a catalytic hydrogenation deolefination process.

Citation Information

Patent Citations

  • Environment-friendly aromatic oil two-stage hydrogenation method

    CN115181587A

  • Reforming hydrogen production device

    CN117861586A

  • Method of modifying zeolite catalyst

    CN1704167A

  • Hydrodealkylation processes

    US5849969A