Large-deformation combined extrusion method for high-toughness magnesium alloy
By adopting the large deformation composite extrusion method in magnesium alloys, changing the shape and size of the extruded billet, and combining differential temperature asymmetric extrusion and stepped solid solution heat treatment, the problem of grain growth and poor mechanical properties during the large deformation process of magnesium alloys has been solved. Solve the problem and realize the short-process and low-cost production of high-strength and high-plasticity magnesium alloys.
Patent Information
- Application Number
- CN202410926819.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The existing technology has the problems of grain growth and poor mechanical properties during the large deformation process of magnesium alloys, and efficient and low-cost production methods have not been fully explored. In particular, it is difficult to achieve high strength and plasticity synergy in magnesium alloys with medium and low alloy content. effect.
The high-strength magnesium alloy large deformation composite extrusion method is adopted. By changing the shape and size of the extruded blank, combined with differential temperature asymmetric upsetting extrusion and stepped solid solution heat treatment, a single pass upsetting extrusion composite deformation and grain can be achieved. Refinement, reducing temperature rise and improving mechanical properties.
It realizes the short-process, low-cost and efficient production of high-strength and high-plasticity magnesium alloys, shortens the process flow, improves the mechanical properties, has a wide range of applications, and is suitable for the actual industrial production of magnesium alloys with medium and low alloy content.
Smart Images

Figure CN118788907A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of magnesium alloy materials and deformation processing thereof, and in particular to a large deformation composite extrusion method for high-strength and toughness magnesium alloys. Background Art
[0002] With the continuous advancement of the "dual carbon" goal and the urgent need to reduce the weight of major equipment, lightweighting has become a prominent research direction in the field of metal structural materials. Magnesium alloys have many excellent properties, such as low relative density and good strength and toughness. Effective weight reduction and good plasticity and toughness make magnesium alloys have broad application prospects in the fields of automobiles, electronic communications, aerospace, etc.
[0003] The high cost and scarcity of heavy rare earth elements (Gd, Ho, etc.) limit their large-scale use in industrial production. Among a series of rare earth-free magnesium alloys, Mg-Al-Sn-Ca alloys provide a low-cost approach to developing new deformable magnesium alloys with high strength and plasticity. Mg-Al-based alloys are the most widely used magnesium alloy system with good strength and ductility. The addition of Sn can reduce the stacking fault energy of magnesium, form a Mg2Sn high-temperature melting point phase, inhibit the growth of dynamic recrystallized grains, and improve the plasticity of Mg-Al alloys. Ca is an abundant and inexpensive element with an atomic size similar to that of rare earths. Adding Ca to magnesium alloys can reduce the stacking fault energy, form CaMgSn intermetallic compounds, and randomize the texture, thereby improving the strength and plasticity of magnesium alloys.
[0004] Asymmetric extrusion technology makes full use of the fact that magnesium alloys are prone to dynamic recrystallization. By introducing shear deformation, dynamic recrystallization is promoted, the base surface texture is weakened or the base surface is tilted, and the mechanical properties of magnesium alloys can be improved through single-pass extrusion. Invention patent CN112570480B discloses a method for weakening the texture of ATX magnesium alloy sheets by asymmetric extrusion, which improves the forming performance of magnesium alloy extruded sheets.
[0005] By changing the shape of the billet to achieve upsetting-extrusion composite deformation, a large number of dislocations and twins can be formed in the extruded billet at the beginning of extrusion, resulting in a large number of nucleation sites, promoting recrystallization, and refining the grains. However, a large amount of deformation often generates a large amount of deformation heat and friction heat, which will cause the fine grains that have already undergone recrystallization to grow in the later stage of extrusion, which is not conducive to mechanical properties. By controlling the temperature difference between the mold and the extruded billet, differential temperature extrusion can alleviate the temperature increase caused by the large deformation process. Invention patent CN115478199B discloses a high-strength and toughness magnesium alloy deformed material and its preparation method, which achieves a better balance of strength and plasticity through differential temperature extrusion processing. However, the total alloy element mass percentage of the magnesium alloy used in the patent is above 7%, and the extrusion speed is slow, which is not conducive to low-cost and efficient production.
[0006] Therefore, it is necessary to develop a short-process and efficient preparation method for magnesium alloys that can be used in actual industrial production to achieve high-strength and high-plasticity synergy in magnesium alloys with medium and low alloy contents. Summary of the invention
[0007] The purpose of the present invention is to provide a high-strength and toughness magnesium alloy large deformation composite extrusion method, optimize the existing extrusion method, and achieve different matching relationships between the billet and the mold cavity by changing the shape and size of the extruded billet, thereby introducing additional upsetting strain in the extrusion process, realizing single-pass upsetting extrusion composite deformation, refining the grains, and improving the mechanical properties. At the same time, in conjunction with the differential temperature extrusion method, the grain growth caused by the increase in temperature during the large deformation process is alleviated, thereby realizing short-process, low-cost and efficient production of high-strength and toughness magnesium alloys.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] A high-strength and tough magnesium alloy large deformation composite extrusion method includes three steps: casting billet preparation, step-by-step solution heat treatment, and differential temperature asymmetric upsetting extrusion. The specific operation is as follows:
[0010] Step 1: high-purity Mg ingot, high-purity Al block, high-purity Sn block and Mg-20Ca master alloy are used as raw materials, and the above raw materials are weighed according to the ratio of aluminum: 1.0-6.0wt%, tin: 0.2-1.2wt%, calcium: 0.1-0.6wt%, and the balance is magnesium, and then the above raw materials are alloyed, and the obtained alloy melt is gravity cast into an ingot, and the casting riser is removed and the oxide scale is polished for the next step of processing;
[0011] Step 2: placing the ingot obtained in step 1 in a heat treatment furnace, performing a step-by-step solution treatment on the ingot, and immediately water quenching the ingot after the heat treatment procedure to obtain a better solution effect;
[0012] The step-by-step solution treatment is set to three stages. The first stage is heated from room temperature to 320°C-380°C and kept at the corresponding temperature for 2-3 hours. The purpose of this stage is to prevent the ingot from cracking due to sudden heating; the second stage is heated from 320°C-380°C to 420°C-430°C and kept at the corresponding temperature for 2-4 hours. The purpose of this stage is to melt the intermetallic compounds with lower melting points in the ingot into the Mg matrix, improve the element segregation in the cast alloy, and prevent defects such as extrusion hot cracks caused by segregation. At the same time, the melted alloy elements can produce fine dynamic precipitation phases during large deformation composite extrusion, which is beneficial to the improvement of mechanical properties; the third stage is heated from 420°C-430°C to 470°C-490°C and kept at the corresponding temperature for 2-3 hours. The purpose of this stage is to melt the coarse and refractory phase as much as possible without growing up, so as to prevent it from having an adverse effect on the subsequent extrusion process and mechanical properties.
[0013] Step 3: Performing shape processing on the heat-treated billet obtained in step 2 to obtain an extruded billet, and then applying lubricant to the extruded billet and the extrusion die respectively and preheating them, the extruded billet is preheated at 380°C-400°C for 20-60 minutes, and the extrusion die is preheated at 100°C-380°C for 10-80 minutes; the extrusion die uses an asymmetric large shear extrusion die, and the shape of the extruded billet is selected from a truncated cone, a trapezoidal shape, or a rectangular cylinder with an outline size smaller than the extrusion cavity size according to the shape of the extrusion die cavity and different upsetting requirements, so that the extruded billet can be upsetting deformed synchronously during the extrusion process; after the preheating is completed, the preheated extruded billet is placed in the extrusion die cavity, and the mold temperature is different from the billet temperature to achieve differential temperature asymmetric upsetting extrusion; then the extruded magnesium alloy is immediately water quenched to obtain an extruded magnesium alloy.
[0014] The present invention adopts the above method to prepare a high-strength and tough magnesium alloy, the main components of which are recorded in mass percentage as follows: aluminum:
[0015] 1.0~6.0wt%, tin: 0.2~1.2wt%, calcium: 0.1~0.6wt%, inevitable impurity content ≤0.05%, and the balance is magnesium.
[0016] Preferably, the alloy smelting process in step 1 is as follows:
[0017] 1) Melt the high-purity Mg ingot, and introduce a mixed protective gas of 1% SF6 and 99% CO2 into the furnace at a melting furnace temperature of 690°C-710°C to reduce oxidation and burning;
[0018] 2) After the Mg ingot is fully melted, high-purity Al block, high-purity Sn block and Mg-20Ca master alloy are added to the melt in sequence;
[0019] 3) After the alloy raw materials are fully melted, the melt is stirred, refined with argon blowing, and slag is removed in sequence, and the alloy melt is kept at 680° C.-700° C. for 10 minutes to obtain the alloy melt.
[0020] Preferably, the casting mold in step one is a sub-rapid water-cooled copper mold, a Y-shaped iron mold or a cylindrical ingot iron mold.
[0021] Preferably, the heating rate of the heating process in step 2 does not exceed 5°C / min.
[0022] Preferably, a small amount of high-purity Ar gas is introduced into the heat treatment furnace in step 2 during the step-by-step solution treatment process to protect the ingot and prevent it from oxidation and burning.
[0023] Preferably, the specific operation of the shape processing in step three mainly includes cutting the heat-treated blank using an electric spark wire cutting device to obtain the required shape size, grinding the cut blank with sandpaper, and removing the surface oxide layer to obtain an extruded blank.
[0024] Preferably, the mold cavity of the asymmetric large shear extrusion mold in step three is rectangular or cylindrical, the extrusion ratio is 10-50, and the ratio of the length from the center line of the extrusion outlet to the two sides of the cavity is 1.1-4.
[0025] Preferably, the extrusion speed of the differential temperature asymmetric upsetting extrusion in step three is 8-18 mm / s.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The present invention achieves upsetting and extrusion composite deformation in a single extrusion process by designing a matching relationship between extrusion billets with different shapes or sizes and the extrusion die cavity, thereby shortening the process flow. The large deformation upsetting extrusion process promotes grain refinement. At the same time, there is no need to change the die shape. Different structures and properties can be obtained by simply controlling the upsetting amount of the billet, thereby realizing the preparation of high-performance magnesium alloys with a short process and high degree of freedom.
[0028] (2) The present invention realizes differential temperature extrusion by controlling the temperature of the extrusion die and the extrusion billet to be different, so that the magnesium alloy extrusion billet can be deformed at a lower temperature, reducing the production cost. At the same time, it alleviates the temperature increase caused by the large deformation process, prevents the grain growth caused by excessively high extrusion temperature, and is beneficial to stabilizing the mechanical properties of the product.
[0029] (3) The present invention achieves high strength and high plasticity by using a magnesium alloy with medium and low alloy element mass percentages. The total alloy mass fraction does not exceed 6%, and the mechanical properties reach the high alloy level, breaking the strengthening and toughening barrier of magnesium alloys, so that the strength and plasticity are improved synergistically.
[0030] (4) The present invention proposes a large deformation process coupled with differential temperature extrusion. The upsetting process before extrusion can activate the metal flow inside the blank to ensure smooth subsequent deformation process. The deformation heat and friction heat generated in the large deformation process can dynamically compensate for the temperature difference between the blank and the die to maintain the extrusion temperature at a certain level. Under the combined effect, conventional magnesium alloys, difficult-to-deform rare earth magnesium alloys or some light alloys can achieve high-speed extrusion with a large extrusion ratio at a relatively low extrusion temperature, and have a wide range of applications.
[0031] (5) The present invention can produce deformed magnesium alloy at a relatively high extrusion speed and obtain excellent mechanical properties. The extrusion outlet speed can be as fast as 20 m / min, thus achieving efficient production.
[0032] (6) The asymmetric extrusion die used in the present invention can introduce additional shear strain to randomize the grain orientation, which helps to improve the uniformity of mechanical properties in all directions of the extruded magnesium alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 A schematic diagram of the trapezoidal extrusion billet shape and its placement in the die;
[0034] Figure 2 It is a statistical diagram of mechanical properties of the embodiment. DETAILED DESCRIPTION
[0035] The technical scheme of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Example 1: Mg-3.8Al-1.1Sn-0.4Ca
[0037] A high-strength and tough magnesium alloy large deformation composite extrusion method mainly includes three steps: casting billet preparation, step-by-step solution heat treatment, and differential temperature asymmetric upsetting extrusion. The specific operation is as follows:
[0038] (1) Casting billet preparation:
[0039] High-purity Mg ingot, high-purity Al block, high-purity Sn block and Mg-20Ca master alloy are used as raw materials, and the above raw materials are weighed according to the ratio of aluminum: 3.8wt%, tin: 1.1wt%, calcium: 0.4wt%, and the balance is magnesium, and alloy smelting is performed;
[0040] The alloy smelting process includes: melting high-purity Mg ingots, introducing a mixed protective gas with a volume fraction of 1% SF6 and 99% CO2 into the furnace body at a smelting furnace temperature of 710°C to reduce oxidation and burning, and after the Mg ingots are fully melted, adding high-purity Al blocks, high-purity Sn blocks, and Mg-20Ca master alloys to the melt in sequence, stirring the melt in sequence after the alloy raw materials are fully melted, blowing argon to refine, and removing slag operations, and after the alloy melt is kept at 690°C for 10 minutes, casting it into a sub-rapid water-cooled copper mold to obtain an ingot, removing the casting riser, and grinding the oxide scale to prepare for the next step of step-by-step solution heat treatment.
[0041] (2) Step solution heat treatment: The ingot obtained in the previous step is placed in a heat treatment furnace and subjected to step solution treatment. The step solution treatment process can be specifically set to three stages. The first stage is heated from room temperature to 375°C and kept warm for 3 hours. The purpose of this stage is to prevent the ingot from cracking due to sudden heating. The second stage is heated from 375°C to 430°C and kept warm for 2 hours. The purpose of this stage is to melt the intermetallic compounds with lower melting points in the ingot into the Mg matrix, improve the element segregation in the cast alloy, and prevent defects such as extrusion hot cracks caused by segregation. At the same time, the melted alloy elements can produce fine dynamic precipitation phases in the large deformation composite extrusion process, which is beneficial to the improvement of mechanical properties. The third stage is heated from 430°C to 490°C and kept warm for 3 hours. The purpose of this stage is to melt the coarse and insoluble phase as much as possible without growing up, so as to prevent it from having an adverse effect on the subsequent extrusion process and mechanical properties. The heating rate during the heating process does not exceed 5°C / min, and a small amount of high-purity Ar gas is introduced into the heat treatment furnace during the step-by-step solution treatment to protect the ingot and prevent it from oxidation and burning. After the heat treatment process is completed, the ingot is immediately water quenched to obtain a better solution effect.
[0042] (3) Differential temperature asymmetric upsetting extrusion: Use electric spark wire cutting equipment to cut the heat-treated billet obtained in the previous step to obtain a trapezoidal billet with an upper bottom width of 10 mm, a lower bottom width of 70 mm, a height of 45 mm, and a thickness of 10 mm. Use sandpaper to grind the cut billet, remove the surface oxide layer, and obtain a trapezoidal extrusion billet. Apply graphite lubricant to the surface of the extruded billet and the surface of the asymmetric extrusion die cavity. The die cavity is rectangular, with a cavity size of 70 mm wide × 12 mm thick × 80 mm high, an extrusion ratio of 21, and a ratio of the length from the center line of the extrusion outlet to both sides of the cavity of 1.5. Place the extruded billet in a heating furnace preheated to 400°C for 60 minutes, preheat the die to 200°C with a heating sleeve and keep it warm for 20 minutes. The die temperature is different from the billet temperature to achieve differential temperature extrusion. After the extrusion billet and the extrusion die are preheated, the preheated extrusion billet is placed in the extrusion die, with the 70mm lower bottom edge in contact with the bottom of the die cavity, and the 10mm upper bottom edge located on the side with a shorter distance between the center line of the die and the side wall. Subsequently, forward extrusion is performed at an extrusion speed of 16mm / s. The extruded magnesium alloy is immediately water quenched to obtain an extruded magnesium alloy with a width of 20mm and a thickness of 2mm.
[0043] The main components of the magnesium alloy are recorded in mass percentage as follows: aluminum: 3.8wt%, tin: 1.1wt%, calcium: 0.4wt%, the content of inevitable impurities is ≤0.05%, and the balance is magnesium.
[0044] Example 2: Mg-2.0Al-0.8Sn-0.5Ca
[0045] A high-strength and tough magnesium alloy large deformation composite extrusion method mainly includes three steps: casting billet preparation, step-by-step solution heat treatment, and differential temperature asymmetric upsetting extrusion. The specific operation is as follows:
[0046] (1) Casting billet preparation:
[0047] High-purity Mg ingot, high-purity Al block, high-purity Sn block and Mg-20Ca master alloy are used as raw materials, and the above raw materials are weighed according to the ratio of aluminum: 2.0wt%, tin: 0.8wt%, calcium: 0.5wt%, and the balance is magnesium, and alloy smelting is performed;
[0048] The alloy smelting process comprises: melting a high-purity Mg ingot, introducing a mixed protective gas with a volume fraction of 1% SF6 and 99% CO2 into a furnace body at a smelting furnace temperature of 710°C to reduce oxidation and burning, and after the Mg ingot is fully melted, sequentially adding a high-purity Al block, a high-purity Sn block, and a Mg-20Ca master alloy into the melt, and after the alloy raw materials are fully melted, sequentially stirring the melt, refining with argon gas, and removing slag operations, and after the alloy melt is kept at 690°C for 10 minutes, casting it into a sub-rapid water-cooled copper mold to obtain an ingot, removing the casting riser, and grinding the oxide scale to prepare for the next step of step-by-step solution heat treatment.
[0049] (2) Step solution heat treatment: The ingot obtained in the previous step is placed in a heat treatment furnace and subjected to step solution treatment. The step solution treatment process can be specifically set to three stages. The first stage is heated from room temperature to 320°C and kept warm for 2 hours. The purpose of this stage is to prevent the ingot from cracking due to sudden heating. The second stage is heated from 320°C to 430°C and kept warm for 2 hours. The purpose of this stage is to melt the intermetallic compounds with lower melting points in the ingot into the Mg matrix, improve the element segregation in the cast alloy, and prevent defects such as extrusion hot cracks caused by segregation. At the same time, the melted alloy elements can produce fine dynamic precipitation phases in the large deformation composite extrusion process, which is beneficial to the improvement of mechanical properties. The third stage is heated from 430°C to 490°C and kept warm for 2 hours. The purpose of this stage is to melt the coarse and insoluble phase as much as possible without growing up, so as to prevent it from having an adverse effect on the subsequent extrusion process and mechanical properties. The heating rate during the heating process does not exceed 5°C / min, and a small amount of high-purity Ar gas is introduced into the heat treatment furnace during the step-by-step solution treatment to protect the ingot and prevent it from oxidation and burning. After the heat treatment process is completed, the ingot is immediately water quenched to obtain a better solution effect.
[0050] (3) Differential temperature asymmetric upsetting extrusion: Use electric spark wire cutting equipment to cut the heat-treated billet obtained in the previous step to obtain a rectangular billet with a height of 50 mm, a width of 55 mm and a thickness of 12 mm. Use sandpaper to grind the cut billet to remove the surface oxide layer to obtain a rectangular extruded billet. Apply graphite lubricant to the surface of the extruded billet and the surface of the asymmetric extrusion die cavity. The die cavity is rectangular, with a cavity size of 70 mm wide × 12 mm thick × 80 mm high, an extrusion ratio of 21, and a length ratio of 1.5 from the center line of the extrusion outlet to both sides of the cavity. Place the extruded billet in a heating furnace preheated to 400°C for 40 minutes, preheat the die to 220°C with a heating sleeve and keep it warm for 20 minutes. The die temperature is different from the billet temperature to achieve differential temperature extrusion. After the extrusion billet and the extrusion die are preheated, the preheated extrusion billet is placed in the extrusion die, with the 55mm wide side in contact with the bottom of the die cavity, and the billet is located on the side with a shorter distance between the center line of the die and the side wall. Then forward extrusion is performed at an extrusion speed of 15mm / s. The extruded magnesium alloy is immediately water quenched to obtain an extruded magnesium alloy with a width of 20mm and a thickness of 2mm.
[0051] The main components of the magnesium alloy are recorded in mass percentage as follows: aluminum: 2.0wt%, tin: 0.8wt%, calcium: 0.5wt%, the content of inevitable impurities is ≤0.05%, and the balance is magnesium.
[0052] Example 3: Mg-2.2Al-0.8Sn-0.5Ca
[0053] A high-strength and tough magnesium alloy large deformation composite extrusion method mainly includes three steps: casting billet preparation, step-by-step solution heat treatment, and differential temperature asymmetric upsetting extrusion. The specific operation is as follows:
[0054] (1) Casting billet preparation:
[0055] High-purity Mg ingot, high-purity Al block, high-purity Sn block and Mg-20Ca master alloy are used as raw materials, and the above raw materials are weighed according to the ratio of aluminum: 2.2wt%, tin: 0.8wt%, calcium: 0.5wt%, and the balance is magnesium, and alloy smelting is performed;
[0056] The alloy smelting process comprises: melting a high-purity Mg ingot, introducing a mixed protective gas with a volume fraction of 1% SF6 and 99% CO2 into a furnace body at a smelting furnace temperature of 710°C to reduce oxidation and burning, and after the Mg ingot is fully melted, sequentially adding a high-purity Al block, a high-purity Sn block, and a Mg-20Ca master alloy into the melt, and after the alloy raw materials are fully melted, sequentially stirring the melt, refining with argon gas, and removing slag operations, and after the alloy melt is kept at 700°C for 10 minutes, casting it into a sub-rapid water-cooled copper mold to obtain an ingot, removing the casting riser, and grinding the oxide scale to prepare for the next step of step-by-step solution heat treatment.
[0057] (2) Step solution heat treatment: The ingot obtained in the previous step is placed in a heat treatment furnace and subjected to step solution treatment. The step solution treatment process can be specifically set to three stages. The first stage is heated from room temperature to 320°C and kept warm for 2 hours. The purpose of this stage is to prevent the ingot from cracking due to sudden heating. The second stage is heated from 320°C to 430°C and kept warm for 2 hours. The purpose of this stage is to melt the intermetallic compounds with lower melting points in the ingot into the Mg matrix, improve the element segregation in the cast alloy, and prevent defects such as extrusion hot cracks caused by segregation. At the same time, the melted alloy elements can produce fine dynamic precipitation phases in the large deformation composite extrusion process, which is beneficial to the improvement of mechanical properties. The third stage is heated from 430°C to 490°C and kept warm for 2 hours. The purpose of this stage is to melt the coarse and insoluble phase as much as possible without growing up, so as to prevent it from having an adverse effect on the subsequent extrusion process and mechanical properties. The heating rate during the heating process does not exceed 5°C / min, and a small amount of high-purity Ar gas is introduced into the heat treatment furnace during the step-by-step solution treatment to protect the ingot and prevent it from oxidation and burning. After the heat treatment process is completed, the ingot is immediately water quenched to obtain a better solution effect.
[0058] (3) Differential temperature asymmetric upsetting extrusion: Use electric spark wire cutting equipment to cut the heat-treated billet obtained in the previous step to obtain a rectangular billet with a height of 55 mm, a width of 50 mm and a thickness of 12 mm. Use sandpaper to grind the cut billet to remove the surface oxide layer to obtain a rectangular extruded billet. Apply graphite lubricant to the surface of the extruded billet and the surface of the asymmetric extrusion die cavity. The die cavity is rectangular, with a cavity size of 70 mm wide × 12 mm thick × 80 mm high, an extrusion ratio of 21, and a length ratio of 1.5 from the center line of the extrusion outlet to both sides of the cavity. Place the extruded billet in a heating furnace preheated to 390°C for 40 minutes, preheat the die to 210°C with a heating sleeve and keep it warm for 20 minutes. The die temperature is different from the billet temperature to achieve differential temperature extrusion. After the extrusion billet and the extrusion die are preheated, the preheated extrusion billet is placed in the extrusion die, with the 50mm wide side in contact with the bottom of the die cavity, and the billet is located on the side with a shorter distance between the center line of the die and the side wall. Then forward extrusion is performed at an extrusion speed of 15mm / s. The extruded magnesium alloy is immediately water quenched to obtain an extruded magnesium alloy with a width of 20mm and a thickness of 2mm.
[0059] The main components of the magnesium alloy are recorded in mass percentage as follows: aluminum: 2.2wt%, tin: 0.8wt%, calcium: 0.5wt%, the content of inevitable impurities is ≤0.05%, and the balance is magnesium.
[0060] Comparative Example 1:
[0061] Paper title: Influence of Al Addition on the Microstructure and Mechanical Properties of Mg-Zn-Sn-Mn-Ca Alloys. Journal name: Materials. Author: Shujuan Yan, Caihong Hou, Angui Zhang, Fugang Qi. Page 14, Mg-6Sn-4Zn-1Mn-0.2Ca-2Al ingot was subjected to conventional forward extrusion at 350℃, extrusion ratio 25, and exit speed 2m / min. After two-step aging heat treatment at 90℃-24h and 180℃-8h, the extruded magnesium alloy obtained the best mechanical properties of tensile strength 350MPa and elongation 14%, and the total alloy element mass percentage was 13.2%.
[0062] Comparative Example 2:
[0063] Paper title: Effect of extrusion speed on microstructure and mechanical properties of Mg-Al-Ca-Sn alloy. Journal name: Materials Research Express. Author: Maochao Zhang, Chao Yang, Zhenshuai Li, Shuai Bao, Peiran Ye, Yungui Chen. Page 7, Mg-2.5Al-2Ca-1Sn ingot was subjected to conventional forward extrusion at 260°C, extrusion ratio 25, extrusion speed 6mm / min, and the best mechanical properties of tensile strength 302MPa, elongation 11.4% were obtained, and the total alloy element mass percentage was 5.5%.
[0064] The mechanical properties of high-strength and high-toughness large-deformation extruded magnesium alloys obtained in Examples 1 to 3 and the mechanical property parameters of Comparative Examples 1 and 2 are shown in Table 1:
[0065] Table 1
[0066]
[0067] As shown in Table 1, when the mass percentage of the total alloying elements in Example 1 is less than that in Comparative Example 1, only one extrusion can obtain better tensile strength and elongation than that in Comparative Example 1 after extrusion combined with two-step aging heat treatment. When the mass percentage of the total alloying elements in Example 2 and Example 3 is less than that in Comparative Example 2, only one extrusion can obtain elongation much higher than that in Comparative Example 2, and at the same time, they also have great advantages in high strength and toughness.
Claims
1. A high-strength and high-toughness magnesium alloy large deformation composite extrusion method, characterized in that: The specific operation of this method is: Step 1: high-purity Mg ingot, high-purity Al block, high-purity Sn block and Mg-20Ca master alloy are used as raw materials, and the above raw materials are weighed according to the ratio of aluminum: 1.0-6.0wt%, tin: 0.2-1.2wt%, calcium: 0.1-0.6wt%, and the balance is magnesium, and then the above raw materials are alloyed, and the obtained alloy melt is gravity cast into an ingot, and the casting riser is removed and the oxide scale is polished for the next step of processing; Step 2: placing the ingot obtained in step 1 in a heat treatment furnace, performing a step-by-step solution treatment on the ingot, and immediately water quenching the ingot after the heat treatment procedure is completed; The step-by-step solution treatment is set to three stages. In the first stage, the temperature is heated from room temperature to 320°C-380°C and kept at the corresponding temperature for 2-3 hours; in the second stage, the temperature is heated from 320°C-380°C to 420°C-430°C and kept at the corresponding temperature for 2-4 hours; in the third stage, the temperature is heated from 420°C-430°C to 470°C-490°C and kept at the corresponding temperature for 2-3 hours. Step 3: Performing shape processing on the heat-treated billet obtained in step 2 to obtain an extruded billet, and then applying lubricant to the extruded billet and the extrusion die respectively and preheating them, the extruded billet is preheated at 380°C-400°C for 20-60 minutes, and the extrusion die is preheated at 100°C-400°C for 10-80 minutes; the extrusion die is an asymmetric large shear extrusion die, and the shape of the extruded billet is a truncated cone, a trapezoid, or a rectangular cylindrical shape whose outline size is smaller than the extrusion cavity size of the die according to the shape of the extrusion die cavity and different upsetting requirements, so that the extruded billet can be upsetting deformed synchronously during the extrusion process; After preheating, the preheated extrusion blank is placed in the extrusion die cavity for positive extrusion to achieve differential temperature asymmetric upsetting extrusion; then the extruded magnesium alloy is immediately water quenched to obtain an extruded magnesium alloy, i.e., a high-strength and toughness magnesium alloy.
2. The high-strength and toughness magnesium alloy large deformation composite extrusion method according to claim 1, characterized in that: The process of alloy smelting in step 1 is as follows: 1) Melt the high-purity Mg ingot, and introduce a mixed protective gas of 1% SF6 and 99% CO2 into the furnace at a melting furnace temperature of 690°C-710°C to reduce oxidation and burning; 2) After the Mg ingot is fully melted, high-purity Al block, high-purity Sn block and Mg-20Ca master alloy are added to the melt in sequence; 3) After the alloy raw materials are fully melted, the melt is stirred, refined with argon blowing, and slag is removed in sequence, and the alloy melt is kept at 680° C.-700° C. for 10 minutes to obtain the alloy melt.
3. The high-strength and toughness magnesium alloy large deformation composite extrusion method according to claim 1, characterized in that: The casting mold described in step 1 adopts a sub-rapid water-cooled copper mold, a Y-shaped iron mold or a cylindrical ingot iron mold.
4. The high-strength and toughness magnesium alloy large deformation composite extrusion method according to claim 1, characterized in that: The heating rate in the heating process in step 2 does not exceed 5°C / min.
5. The high-strength and toughness magnesium alloy large deformation composite extrusion method according to claim 1, characterized in that: In step 2, high-purity Ar gas is introduced into the heat treatment furnace during the step-by-step solution treatment process to protect the ingot.
6. The high-strength and toughness magnesium alloy large deformation composite extrusion method according to claim 1, characterized in that: The specific operation of the shape processing described in step three mainly includes cutting the heat-treated blank with an electric spark wire cutting device to obtain the required shape size, grinding the cut blank with sandpaper, and removing the surface oxide layer to obtain the extruded blank.
7. The high-strength and toughness magnesium alloy large deformation composite extrusion method according to claim 1, characterized in that: The extrusion speed of the forward extrusion in step 3 is 8-18 mm / s.
8. The high-strength and toughness magnesium alloy large deformation composite extrusion method according to claim 1, characterized in that: The mold cavity of the asymmetric large shear extrusion mold is rectangular or cylindrical, the extrusion ratio is 10-50, and the length ratio from the center line of the extrusion outlet to both sides of the cavity is 1.1-4.
9. A high-strength and tough magnesium alloy prepared according to the method according to any one of claims 1 to 8, characterized in that: The main components are recorded in percentage by mass as follows: aluminum: 1.0-6.0wt%, tin: 0.2-1.2wt%, calcium: 0.1-0.6wt%, the content of inevitable impurities is ≤0.05%, and the balance is magnesium.
Citation Information
Patent Citations
Differential temperature extrusion method for preparing bimetal composite sectional materials
CN108466468A
Method for achieving ATX series magnesium alloy plate texture weakening through asymmetric extrusion
CN112570480A
One-step light alloy preparation method combining upsetting and asymmetric extrusion
CN113953343A
Ultrahigh-plasticity rare earth wrought magnesium alloy and preparation method of extruded plate thereof
CN114293079A
Magnesium alloy asymmetric extrusion die and extrusion method
CN117732904A