Preparation method of boulder

Through the mixing and hydraulic molding of ore powder, inorganic binders and additives, combined with steam drying treatment, the high production cost and environmental protection problems of hydrocarbon stone are solved, and the preparation of hydrocarbon stone with low cost and high yield is realized, adapting to Different usage requirements.

CN118789652APending Publication Date: 2024-10-18NANJING MEIKETENG TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040598.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The existing hydrophilic stone production method has high costs, serious environmental problems and low yield, making it difficult to popularize it for mass consumption.

Method used

Ore powder, inorganic binders and additives are mixed in proportion, then hydraulically molded and dried in a steam room. The molding pressure and thickness are controlled to provide a variety of thickness options.

Benefits of technology

It has achieved low-cost, high-yield production of hydrocarbon stone, and solved environmental problems through steam drying to adapt to different use needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972272120000041
    Figure BDA0004972272120000041
Patent Text Reader

Abstract

The invention provides a water boulder preparation method, and relates to the field of water boulder production, and the water boulder preparation method comprises the following production processes: 1, uniformly mixing mineral powder, an inorganic binder and an additive according to a ratio; 2, conveying the mixture into a mold cavity of an oil press, pressing at the pressure of 50-80 tons / cavity, maintaining the pressure for 5 seconds, and demolding from the mold cavity after molding; thirdly, the demolded primary products are transferred into a stacking disc, during the period, each primary product is kept in a vertical state, and automatic stacking is conducted after the stacking disc is full; and 4, transferring the stacked primary products into a steam room, and steaming for 4 hours by using steam at 100 DEG C. The invention provides a novel preparation method of the water boulder, which can be used for industrially producing the water boulder firstly, and is limited to manufacturing the water boulder by drying the pre-formed primary products by using the steam, so that the method is green and environment-friendly, is low in defective rate, and in addition, has the advantages of low production cost and high production efficiency. And the thickness of the boulder can be adjusted by controlling the mold pressing pressure, various thickness selection schemes are provided, and different users are catered.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of water-bleached stone production, in particular to a water-bleached stone preparation method. Background Art

[0002] Water-skipping stone is a kind of game prop used in the game of skipping stones. In the early period, water-skipping stones were mostly flat, stone pieces or stone tiles of different shapes, and their functions were limited to leisure and entertainment. In recent years, skipping stones have evolved into a trend of competitive sports. For this trend, it is necessary to add unified standards to game props such as water-skipping stones. At present, there are methods of mass production of water-skipping stones by selecting natural stones through cutting, etc., but due to the material cost and equipment labor cost, the price of water-skipping stones produced by this method is often high, and it is difficult to popularize it to the mass consumption level. In addition, there are environmental protection problems such as sewage and particulate pollution in the production. In addition, there is also a method of pressing ore powder and producing water-skipping stones by sintering, but due to factors such as process, the yield rate is not high. Therefore, it is necessary to propose a method for preparing water-skipping stones with low manufacturing cost and high yield rate based on the above description. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing water-blasted stone to solve the above technical problems.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The method for preparing water-bleached stone includes the following production process:

[0006] First, the ore powder, inorganic binder and additives are mixed in proportion;

[0007] Second, the mixed material is transported to the mold cavity of the hydraulic press, pressed at a pressure of 50-80 tons / cavity, and the pressure is maintained for 5 seconds. After molding, it is ejected from the mold cavity;

[0008] Third, the demoulding primary products are transferred to the pallet. During this period, each piece of primary product is kept in an upright state. When the pallet is full, it will be automatically stacked.

[0009] Fourth, the palletized primary products are transferred to the steam room, steamed with 100°C steam for 4 hours, and then cooled at room temperature. After 24 hours, they are steamed again with 100°C steam for 4 hours, and then cooled and dried at room temperature.

[0010] Preferably, the proportion of ore powder in the mixture is controlled at 60%-70%, the proportion of inorganic binder in the mixture is controlled at 20%-30%, and the proportion of additives in the mixture is controlled at 5%-10%.

[0011] Preferably, the humidity of the mixed material after mixing is controlled at 2%-6%.

[0012] Preferably, the additives include lubricants and mold release agents.

[0013] The beneficial effects of the present invention are:

[0014] The present invention provides a new method for preparing riprap. The method can firstly be used for industrialized production of riprap. Secondly, the method is limited to steam drying preformed primary products to produce riprap, which is not only green and environmentally friendly, but also has a low defective rate. In addition, the thickness of the riprap can be adjusted by controlling the molding pressure, providing a variety of thickness options to cater to different user groups. DETAILED DESCRIPTION

[0015] In order to make the technical means, creative features, objectives and effects of the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments, but the following embodiments are only preferred embodiments of the present invention, not all. Based on the embodiments in the implementation mode, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0016] Specific embodiments of the present invention are described below.

[0017] Example 1

[0018] In this embodiment, a method for preparing water-bleached stone is proposed, including the following production process:

[0019] First, the ore powder, inorganic binder and additives are mixed in proportion;

[0020] Among them, the proportion of ore powder in the mixture is 60%, the proportion of inorganic binder in the mixture is 30%, the proportion of additives in the mixture is 10%, and the humidity of the mixed mixture is 7%;

[0021] Second, the mixed material is transported to the mold cavity of the hydraulic press, pressed at a pressure of 60 tons / cavity, and the pressure is maintained for 5 seconds. After molding, it is ejected from the mold cavity;

[0022] Third, the demoulding primary products are transferred to the pallet. During this period, each piece of primary product is kept in an upright state. When the pallet is full, it will be automatically stacked.

[0023] Fourth, the palletized primary products are transferred to the steam room, steamed with 100°C steam for 4 hours, and then cooled at room temperature. After 24 hours, they are steamed again with 100°C steam for 4 hours, and then cooled and dried at room temperature.

[0024] Example 2

[0025] In this embodiment, a method for preparing water-bleached stone is proposed, including the following production process:

[0026] First, the ore powder, inorganic binder and additives are mixed in proportion;

[0027] Among them, the proportion of ore powder in the mixture is 65%, the proportion of inorganic binder in the mixture is 25%, the proportion of additives in the mixture is 10%, and the humidity of the mixed mixture is 6%;

[0028] Second, the mixed material is transported to the mold cavity of the hydraulic press, pressed at a pressure of 60 tons / cavity, and the pressure is maintained for 5 seconds. After molding, it is ejected from the mold cavity;

[0029] Third, the demoulding primary products are transferred to the pallet. During this period, each piece of primary product is kept in an upright state. When the pallet is full, it will be automatically stacked.

[0030] Fourth, the palletized primary products are transferred to the steam room, steamed with 100°C steam for 4 hours, and then cooled at room temperature. After 24 hours, they are steamed again with 100°C steam for 4 hours, and then cooled and dried at room temperature.

[0031] Example 3

[0032] In this embodiment, a method for preparing water-bleached stone is proposed, including the following production process:

[0033] First, the ore powder, inorganic binder and additives are mixed in proportion;

[0034] Among them, the proportion of ore powder in the mixture is 70%, the proportion of inorganic binder in the mixture is 20%, the proportion of additives in the mixture is 10%, and the humidity of the mixed mixture is 4%;

[0035] Second, the mixed material is transported to the mold cavity of the hydraulic press, pressed at a pressure of 60 tons / cavity, and the pressure is maintained for 5 seconds. After molding, it is ejected from the mold cavity;

[0036] Third, the demoulding primary products are transferred to the pallet. During this period, each piece of primary product is kept in an upright state. When the pallet is full, it will be automatically stacked.

[0037] Fourth, the palletized primary products are transferred to the steam room, steamed with 100°C steam for 4 hours, and then cooled at room temperature. After 24 hours, they are steamed again with 100°C steam for 4 hours, and then cooled and dried at room temperature.

[0038] Example 4

[0039] In this embodiment, a method for preparing water-bleached stone is proposed, including the following production process:

[0040] First, the ore powder, inorganic binder and additives are mixed in proportion;

[0041] Among them, the proportion of ore powder in the mixture is 70%, the proportion of inorganic binder in the mixture is 20%, the proportion of additives in the mixture is 10%, and the humidity of the mixed mixture is 4%;

[0042] Second, the mixed material is transported to the mold cavity of the hydraulic press, pressed at a pressure of 70 tons / cavity, and the pressure is maintained for 5 seconds. After molding, it is ejected from the mold cavity;

[0043] Third, the demoulding primary products are transferred to the pallet. During this period, each piece of primary product is kept in an upright state. When the pallet is full, it will be automatically stacked.

[0044] Fourth, the palletized primary products are transferred to the steam room, steamed with 100°C steam for 4 hours, and then cooled at room temperature. After 24 hours, they are steamed again with 100°C steam for 4 hours, and then cooled and dried at room temperature.

[0045] Example 5

[0046] In this embodiment, a method for preparing water-bleached stone is proposed, including the following production process:

[0047] First, the ore powder, inorganic binder and additives are mixed in proportion;

[0048] Among them, the proportion of ore powder in the mixture is 70%, the proportion of inorganic binder in the mixture is 20%, the proportion of additives in the mixture is 10%, and the humidity of the mixed mixture is 4%;

[0049] Second, the mixed material is transported to the mold cavity of the hydraulic press, pressed at a pressure of 80 tons / cavity, and the pressure is maintained for 5 seconds. After molding, it is ejected from the mold cavity;

[0050] Third, the demoulding primary products are transferred to the pallet. During this period, each piece of primary product is kept in an upright state. When the pallet is full, it will be automatically stacked.

[0051] Fourth, the palletized primary products are transferred to the steam room, steamed with 100°C steam for 4 hours, and then cooled at room temperature. After 24 hours, they are steamed again with 100°C steam for 4 hours, and then cooled and dried at room temperature.

[0052] The proportion of each component in the mixed material, the mixed material humidity and the molding pressure in Examples 1 to 5 are shown in Table 1:

[0053]

[0054] Table 1

[0055] Embodiments 1 to 3 provide three groups of preparation methods for water-pebbled stones. Embodiments 3 to 4 adjust the molding pressure. After the adjustment, the thickness of the water-pebbled stones changes without significant changes in weight, and the feel can be adjusted based on the thickness change.

[0056] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing water-bleached stone, characterized in that: The production process includes the following: First, the ore powder, inorganic binder and additives are mixed in proportion; Second, the mixed material is transported to the mold cavity of the hydraulic press, pressed at a pressure of 50-80 tons / cavity, and the pressure is maintained for 5 seconds. After molding, it is ejected from the mold cavity; Third, the demoulding primary products are transferred to the pallet. During this period, each piece of primary product is kept in an upright state. When the pallet is full, it will be automatically stacked. Fourth, the palletized primary products are transferred to the steam room, steamed with 100°C steam for 4 hours, and then cooled at room temperature. After 24 hours, they are steamed again with 100°C steam for 4 hours, and then cooled and dried at room temperature.

2. The method for preparing water-drifted stone according to claim 1, characterized in that: The proportion of ore powder in the mixture is controlled at 60%-70%, the proportion of inorganic adhesive in the mixture is controlled at 20%-30%, and the proportion of additives in the mixture is controlled at 5%-10%.

3. The method for preparing water-drifted stone according to claim 1, characterized in that: The humidity of the mixed material after mixing is controlled at 2%-6%.

4. The method for preparing water-drifted stone according to claim 1, characterized in that: Additives include lubricants and release agents.