Preparation method of anti-caking potassium perchlorate
By adding polyvinyl alcohol and polyionic liquid to the saturated solution of potassium perchlorate, and using cross-linking agents to form a three-dimensional network structure, the problem of potassium perchlorate agglomeration is solved, the agglomeration rate and friction sensitivity are significantly reduced, and its performance in storage and transportation is improved. security in.
Patent Information
- Application Number
- CN202411260531.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-09-10
AI Technical Summary
Potassium perchlorate is prone to caking during storage and use, mainly due to its strong hygroscopicity, which leads to surface dissolution, recrystallization and the formation of crystal bridges. Existing anti-caking methods have limited effects or make it difficult to control product purity.
Add polyvinyl alcohol and polyionic liquid to the saturated solution of potassium perchlorate, adjust the pH to 3-5, then add a cross-linking agent, and form a three-dimensional network structure film layer through stirring and ultrasonic oscillation to enhance the anti-caking performance of the particles. .
Significantly reduces the caking rate and friction sensitivity of potassium perchlorate, making it safer during transportation and storage and avoiding adhesion between particles.
Smart Images

Figure QLYQS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of inorganic materials, specifically to a method for preparing anti-caking potassium perchlorate. Background Technology
[0002] Potassium perchlorate is an inorganic salt crystal that may clump during storage and use. This is mainly due to its strong hygroscopicity, which makes it easy to absorb moisture from the air, causing the surface to dissolve and recrystallize to form crystal bridges, thus leading to clumping.
[0003] Currently, there are roughly two methods for selecting anti-caking additives for inorganic salt crystals both domestically and internationally. One method is to use some inert powders to separate the particle surfaces and prevent excessive contact between particles from causing bridging. However, if the additive dosage is too small, the anti-caking effect is poor; if the additive dosage is too large, it is difficult to control the purity of the finished product within the product quality standard, i.e., the impurity content exceeds the standard. The other method is to add polymers or surfactants to prevent agglomeration by changing the surface properties of inorganic salt crystals or forming a polymer film. Currently, there is relatively little research on this method. Summary of the Invention
[0004] Purpose of the invention: To address the above-mentioned technical problems, this invention proposes a method for preparing anti-caking potassium perchlorate.
[0005] The technical solution adopted is as follows: A method for preparing anti-caking potassium perchlorate: Add the potassium perchlorate to be modified, polyvinyl alcohol, and polyionic liquid to a saturated potassium perchlorate solution, mix well, adjust the pH of the system to 3-5, add the crosslinking agent and stir to react. After the reaction is complete, filter and dry.
[0006] Furthermore, the preparation method of the polyionic liquid is as follows: Ionic liquids undergo free radical polymerization under the action of free radical initiators. The resulting polymer product is then filtered out and dried.
[0007] Furthermore, the anion of the ionic liquid is any one of halide ions, tetrafluoroborate ions, hexafluorophosphate ions, bis(trifluoromethanesulfonyl)imide ions, and p-toluenesulfonate ions.
[0008] Furthermore, the cationic structure of the ionic liquid is shown below: , where n is a positive integer, n≥5.
[0009] Furthermore, the free radical initiator is azobisisobutyronitrile and / or azobisisoheptanenitrile.
[0010] Furthermore, the crosslinking agent is glutaraldehyde.
[0011] Furthermore, the mass ratio of the polyvinyl alcohol, polyionic liquid, and crosslinking agent is 70-100:10-50:1-5.
[0012] Furthermore, ultrasonic oscillation is applied simultaneously with the stirring reaction.
[0013] Furthermore, the temperature during the stirring reaction is 30-60℃.
[0014] Furthermore, the drying temperature is ≤100℃.
[0015] The beneficial effects of this invention are: This invention provides a method for preparing anti-caking potassium perchlorate. Polyvinyl alcohol can be coated onto the surface of potassium perchlorate to form a film, which is then cross-linked with a cross-linking agent to form a three-dimensional network structure, enhancing the strength of the film layer. This prevents the potassium perchlorate particles from damaging the film layer under conditions such as temperature changes, compression, and humidity, thereby avoiding particle adhesion and exhibiting excellent anti-caking effects. Polyionic liquids possess both surfactant and self-lubricating properties, and the amino groups in their structure can undergo cross-linking reactions with the cross-linking agent. Under the combined effect of these factors, existing potassium perchlorate can be modified to have better anti-caking performance. Compared with commercially available potassium perchlorate, the potassium perchlorate prepared by this invention has an extremely low agglomeration rate and a significantly reduced friction sensitivity, making it safer during transportation and storage. Detailed Implementation
[0016] Unless otherwise specified in the examples, the conditions were performed under standard conditions or as recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available products. Techniques not mentioned in this invention refer to existing technologies. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.
[0017] Example 1: A method for preparing anti-caking potassium perchlorate: Add 200g of commercially available potassium perchlorate (particle size 50-100μm) to 5000ml of saturated potassium perchlorate aqueous solution. First, add 80g of polyvinyl alcohol and mix well. Then, dissolve 20g of polyionic liquid in 500ml of DMF and add it to the mixture. After mixing well, adjust the pH of the system to 4 with hydrochloric acid. Then, dissolve 4g of crosslinking agent glutaraldehyde in 100ml of DMF and slowly add it dropwise to the mixture. Stir the reaction solution under ultrasonic vibration and 35℃ water bath conditions for 60min. After the reaction is completed, return to room temperature and filter. Place the obtained product in a 60℃ oven and dry for 24h. The preparation method of polyionic liquid is as follows: ; Dissolve 50g of 3-aminooctyl-1-vinylimidazolium chloride and 1g of azobisisobutyronitrile in an appropriate amount of chloroform to obtain solution A and solution B. Under nitrogen protection, slowly add solution B to solution A while stirring continuously. Heat to reflux for 6 hours and then restore to room temperature. Filter out the resulting precipitate and dry it.
[0018] Example 2: A method for preparing anti-caking potassium perchlorate: Add 200g of commercially available potassium perchlorate (particle size 50-100μm) to 5000ml of saturated potassium perchlorate aqueous solution. First, add 80g of polyvinyl alcohol and mix well. Then, dissolve 20g of polyionic liquid in 500ml of DMF and add it to the mixture. After mixing well, adjust the pH of the system to 4 with hydrochloric acid. Then, dissolve 4g of crosslinking agent glutaraldehyde in 100ml of DMF and slowly add it dropwise to the mixture. Stir the reaction solution under ultrasonic vibration and 35℃ water bath conditions for 60min. After the reaction is completed, return to room temperature and filter. Place the obtained product in a 60℃ oven and dry for 24h. The preparation method of polyionic liquid is as follows: ; Dissolve 50g of 3-aminooctyl-1-vinylimidazolium tetrafluoroborate and 1g of azobisisobutyronitrile in an appropriate amount of chloroform to obtain solution A and solution B. Under nitrogen protection, slowly add solution B to solution A while stirring continuously. Heat to reflux for 6 hours and then restore to room temperature. Filter out the resulting precipitate and dry it.
[0019] Example 3: A method for preparing anti-caking potassium perchlorate: Add 200g of commercially available potassium perchlorate (particle size 50-100μm) to 5000ml of saturated potassium perchlorate aqueous solution. First, add 80g of polyvinyl alcohol and mix well. Then, dissolve 20g of polyionic liquid in 500ml of DMF and add it to the mixture. After mixing well, adjust the pH of the system to 4 with hydrochloric acid. Then, dissolve 4g of crosslinking agent glutaraldehyde in 100ml of DMF and slowly add it dropwise to the mixture. Stir the reaction solution under ultrasonic vibration and 35℃ water bath conditions for 60min. After the reaction is completed, return to room temperature and filter. Place the obtained product in a 60℃ oven and dry for 24h. The preparation method of polyionic liquid is as follows: ; Dissolve 50g of 3-aminooctyl-1-vinylimidazolium hexafluorophosphate and 1g of azobisisobutyronitrile in an appropriate amount of chloroform to obtain solution A and solution B. Under nitrogen protection, slowly add solution B to solution A while stirring continuously. Heat to reflux for 6 hours and then restore to room temperature. Filter out the resulting precipitate and dry it.
[0020] Example 4: A method for preparing anti-caking potassium perchlorate: Add 200g of commercially available potassium perchlorate (particle size 50-100μm) to 5000ml of saturated potassium perchlorate aqueous solution. First, add 90g of polyvinyl alcohol and mix well. Then, dissolve 10g of polyionic liquid in 500ml of DMF and add it to the mixture. After mixing well, adjust the pH of the system to 4 with hydrochloric acid. Then, dissolve 4g of crosslinking agent glutaraldehyde in 100ml of DMF and slowly add it dropwise to the mixture. Stir the reaction solution under ultrasonic vibration and 35℃ water bath conditions for 60min. After the reaction is completed, return to room temperature and filter. Place the obtained product in a 60℃ oven and dry for 24h. The preparation method of polyionic liquid is as follows: ; Dissolve 50g of 3-aminooctyl-1-vinylimidazolium chloride and 1g of azobisisobutyronitrile in an appropriate amount of chloroform to obtain solution A and solution B. Under nitrogen protection, slowly add solution B to solution A while stirring continuously. Heat to reflux for 6 hours and then restore to room temperature. Filter out the resulting precipitate and dry it.
[0021] Example 5: A method for preparing anti-caking potassium perchlorate: Add 200g of commercially available potassium perchlorate (particle size 50-100μm) to 5000ml of saturated potassium perchlorate aqueous solution. First, add 70g of polyvinyl alcohol and mix well. Then, dissolve 30g of polyionic liquid in 500ml of DMF and add it to the mixture. After mixing well, adjust the pH of the system to 4 with hydrochloric acid. Then, dissolve 4g of crosslinking agent glutaraldehyde in 100ml of DMF and slowly add it dropwise to the mixture. Stir the reaction solution under ultrasonic vibration and 35℃ water bath conditions for 60min. After the reaction is completed, return to room temperature and filter. Place the obtained product in a 60℃ oven and dry for 24h. The preparation method of polyionic liquid is as follows: ; Dissolve 50g of 3-aminooctyl-1-vinylimidazolium chloride and 1g of azobisisobutyronitrile in an appropriate amount of chloroform to obtain solution A and solution B. Under nitrogen protection, slowly add solution B to solution A while stirring continuously. Heat to reflux for 6 hours and then restore to room temperature. Filter out the resulting precipitate and dry it.
[0022] Comparative Example 1: Basically the same as Example 1, except that no polyionic liquid was added.
[0023] A method for preparing anti-caking potassium perchlorate: Add 200g of commercially available potassium perchlorate (particle size 50-100μm) to 5000ml of saturated potassium perchlorate aqueous solution. First, add 80g of polyvinyl alcohol and mix well. Then add 500ml of DMF and mix well. Adjust the pH of the system to 4 with hydrochloric acid. Dissolve 4g of crosslinking agent glutaraldehyde in 100ml of DMF and slowly add it dropwise to the mixture. Stir the reaction solution under ultrasonic vibration and 35℃ water bath conditions for 60min. After the reaction is completed, return to room temperature and filter. Place the obtained product in a 60℃ oven and dry for 24h.
[0024] Comparative Example 2: Basically the same as Example 1, except that no polyionic liquid and crosslinking agent glutaraldehyde were added.
[0025] A method for preparing anti-caking potassium perchlorate: Add 200g of commercially available potassium perchlorate (particle size 50-100μm) to 5000ml of saturated potassium perchlorate aqueous solution. First, add 80g of polyvinyl alcohol and mix well. Then add 500ml of DMF and mix well. Adjust the pH of the system to 4 with hydrochloric acid. Then slowly add 100ml of DMF dropwise to the mixture. Stir the reaction solution under ultrasonic vibration and 35℃ water bath conditions for 60min. After the reaction is completed, return to room temperature and filter. Place the obtained product in a 60℃ oven and dry for 24h.
[0026] Performance testing: ①The potassium perchlorate prepared in Examples 1-5 and Comparative Examples 1-2 and commercially available potassium perchlorate were pressed into cylindrical samples with a diameter of φ100mm×100mm under 3MPa. After absorbing moisture for 30 days in an environment with 75% humidity and 25℃, the cylindrical sample was allowed to fall freely from 10m above the ground and then passed through a 40-mesh sieve. The agglomeration rate η was calculated. m1 is the sieve residue mass, and m0 is the sample mass.
[0027] ② The potassium perchlorate from Examples 1-5 and Comparative Examples 1-2, and commercially available potassium perchlorate were used as test samples. Friction sensitivity tests were conducted using a friction sensitivity meter according to the method in GJB770B-2005. The test pressure was 3.92 MPa and the swing angle was 90°. During the test, any sample that showed one of the following phenomena was judged as exploding: discoloration, odor, smoke, explosive sound, or ablation marks on the impact surface. Otherwise, it was judged as not exploding. Each group of samples was measured in parallel 25 times, and the test results were expressed as the percentage of explosion.
[0028] The test results are shown in Table 1 below: Table 1: ; As shown in Table 1 above, the potassium perchlorate prepared by this invention has an extremely low agglomeration rate compared to commercially available potassium perchlorate, and the friction sensitivity is significantly reduced.
[0029] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing anti-caking potassium perchlorate, characterized in that: Add the potassium perchlorate to be modified, polyvinyl alcohol and polyionic liquid to the saturated potassium perchlorate solution, mix well and adjust the pH of the system to 3-5, then add the crosslinking agent and stir to react, filter and dry after the reaction is completed; The preparation method of the polyionic liquid is as follows: The ionic liquid undergoes free radical polymerization under the action of a free radical initiator, and the obtained polymerization product is filtered out and then dried; The anion of the ionic liquid is any one of a halogen ion, a tetrafluoroborate ion, a hexafluorophosphate ion, a bis(trifluoromethanesulfonyl)imide ion, and a p-toluenesulfonate ion; The cation structure of the ionic liquid is shown below: ; Wherein, n is a positive integer, n=8; The free radical initiator is azobisisobutyronitrile and / or azobisisoheptanenitrile; The cross-linking agent is glutaraldehyde.
2. The method for preparing the anti-caking potassium perchlorate according to claim 1, characterized in that: The mass ratio of the polyvinyl alcohol, the polyionic liquid and the cross-linking agent is 70-100:10-50:1-5.
3. The method for preparing the anti-caking potassium perchlorate according to claim 1, characterized in that: The reaction was stirred while ultrasonic vibration was applied.
4. The method for preparing the anti-caking potassium perchlorate according to claim 1, characterized in that: The temperature during the stirring reaction is 30-60°C.
5. The method for preparing the anti-caking potassium perchlorate according to claim 1, characterized in that: Drying temperature ≤100℃.
Citation Information
Patent Citations
Method for treating potash with anticaking agent
CA1211318A
New nanoscale ammonium perchlorate cladding technology
CN103708423A
Method for preparing yttrium perchlorate from rare earth yttrium oxide
CN117466251A
Method of producing fine particle ammonium perchlorate
US3685163A
Method of making ultra-fine ammonium perchlorate particles
US3819336A
Cited By
Preparation method and application of ultrafine potassium perchlorate
CN119263215A
Preparation method of fine-particle potassium perchlorate
CN119370803A
A method for preparing fine-particle potassium perchlorate
CN119370803B