Preparation method of lithium difluorophosphate

By using lithium fluoride and phosphoric acid cyclic anhydride to react with hydrogen fluoride in an organic solvent under an inert gas environment, the problems of low product quality and complicated processes in the preparation method of lithium difluorophosphate in the existing technology are solved, and high purity and high yield are achieved. The preparation is efficient, suitable for industrial production, and improves the dispersion performance and commercial value of the product.

CN118790971AActive Publication Date: 2024-10-18HUBEI BAIJIERUI ADVANCED MATERIALS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411130056.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-10-18
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The existing preparation method of lithium difluorophosphate has problems such as low product quality, complex process, high reaction energy consumption and low element utilization rate, making it difficult to be suitable for industrial production.

Method used

In a closed inert gas environment, use lithium fluoride and phosphoric acid cyclic anhydride to react in an organic solvent, slowly add the fluorination reagent, control the temperature and reaction time, and obtain high-purity lithium difluorophosphate through concentration, cooling, filtration and drying. , the preferred lithium fluoride and 1-propylphosphoric acid cyclic anhydride are reacted with hydrogen fluoride to achieve efficient preparation.

Benefits of technology

It achieves the preparation of high purity (more than 99.5%) and high yield (more than 95%) lithium difluorophosphate, simplifies the process, reduces reaction energy consumption, is suitable for industrial production, and improves the dispersion performance and commercial value of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure FDA0004997554560000011
    Figure FDA0004997554560000011
  • Figure HDA0004997554580000011
    Figure HDA0004997554580000011
Patent Text Reader

Abstract

The invention relates to the technical field of synthesis of lithium battery additives, and particularly discloses a preparation method of lithium difluorophosphate. The method comprises the following steps: (1) in a closed inert gas environment, adding a lithium fluoride solid and phosphoric acid cyclic anhydride into an organic solvent, uniformly dispersing, controlling the temperature of a system to be-10 DEG C to 60 DEG C, then slowly adding a fluorinating reagent into the system, and after the fluorinating reagent is added, continuing to preserve heat for the total reaction time of 3-4 hours; (2) concentrating the reaction material in the step (1), cooling and crystallizing, filtering and drying to obtain lithium difluorophosphate with the purity of more than 99.5%; wherein the lithium fluoride in the step (1) is replaced by sodium fluoride or potassium fluoride, the sodium difluorophosphate or the potassium difluorophosphate is finally obtained in the step (2), and the purity of the sodium difluorophosphate or the potassium difluorophosphate reaches 99.5% or above. The method is low in reaction energy consumption, high in element utilization rate and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium battery additive synthesis, and in particular to a method for preparing lithium difluorophosphate. Background Art

[0002] Lithium-ion batteries have higher specific capacity and discharge voltage than traditional lead-acid batteries and alkaline batteries, and they are less polluting to the environment. In the development of lithium salt additive products, the traditional lithium hexafluorophosphate as an electrolyte can no longer meet the needs of lithium-ion batteries under special environmental conditions. However, lithium difluorophosphate as an electrolyte additive can effectively improve the high cycle performance and high and low temperature storage performance of lithium-ion batteries, significantly improving their cycle stability at minus 15°C, and forming a more stable SEI film under high temperature conditions. The formed SEI film can effectively prevent the electrolyte from corroding the electrodes and current collectors, making lithium-ion batteries have better high and low temperature performance. Therefore, lithium difluorophosphate, as a new type of lithium salt additive, is not only of great significance to the use and development of lithium batteries, but also has great commercial value as an industrial product.

[0003] At present, there are many methods for producing lithium difluorophosphate. For example, lithium difluorophosphate is prepared by reacting lithium hexafluorophosphate with siloxane. This method is difficult to produce, and the by-product is a fluorosilane product, which is highly toxic. The production process is dangerous and very unfavorable to production.

[0004] For example, CN113148971A discloses a method of using POCl 3 and anhydrous triphosphate in an organic solvent. This method has a low yield of the product, low product purity, and the phosphate used (such as Na 3 PO 4 , K 3 PO 4 etc.) will cause other metal ions (sodium, potassium) in the product to exceed the standard, making it impossible to apply it to lithium battery electrolyte, which is not conducive to industrial production.

[0005] For example, CN106882782A discloses a method using POF 3 With P 2 O 5 And lithium-containing inorganic salts (LiF, LiOH, Li 2 CO 3 ) in an organic solvent, the POF used in this reaction 3 It is a gas with high activity, which makes it inconvenient to store and transport. The reaction is a pressurized reaction, which requires high equipment. The moisture content of the reaction system needs to be less than 1ppm. The reaction conditions are harsh and it is difficult to achieve industrialization.

[0006] For example, CN112897494A discloses a synthesis process of lithium difluorophosphate, which uses phosphorus oxide, lithium fluoride, and phosphorus pentafluoride to react in anhydrous hydrogen fluoride to synthesize lithium difluorophosphate, wherein P 2 O 5 It is very easy to react with water to form phosphate, and when the phosphorus oxide compound is polyphosphoric acid or metaphosphoric acid (see Examples 6 and 7), the reaction by-product is phosphoric acid, and the element utilization rate is not high; at the same time, the phosphate is difficult to handle in subsequent treatments, and the residual phosphate will corrode the lithium battery diaphragm material and the aluminum coating material, thereby causing a battery short circuit and a fire, and is not suitable for use in lithium battery electrolytes.

[0007] In summary, the existing preparation methods of lithium difluorophosphate have low product quality, complex processes, high reaction energy consumption, and low element utilization, which are very unfavorable for the industrialization and promotion of lithium difluorophosphate. Summary of the invention

[0008] Based on the problems existing in the prior art, the present invention aims to provide a method for preparing lithium difluorophosphate which has excellent product purity, simple process, low reaction energy consumption, high element utilization rate and is suitable for industrial production.

[0009] In order to achieve the above object, the present invention provides the following technical solutions:

[0010] A method for preparing difluorophosphate comprises the following steps:

[0011] (1) In a closed inert gas environment, solid lithium fluoride and cyclic phosphoric acid anhydride are added to an organic solvent and dispersed uniformly, the system temperature is controlled to be -10°C to 60°C, and then a fluorination reagent is slowly added to the system. After the addition is completed, the system is kept warm for a total reaction time of 3 to 4 hours; the total reaction time includes the addition time of the fluorination reagent and the heat preservation time;

[0012] (2) The reaction material of step (1) is concentrated, cooled and crystallized, filtered and dried to obtain lithium difluorophosphate, wherein the purity of the lithium difluorophosphate reaches more than 99.5%.

[0013] Further, in step (1):

[0014] The lithium fluoride can be replaced by sodium fluoride or potassium fluoride, and the final step (2) obtains sodium difluorophosphate or potassium difluorophosphate, respectively, and the purity of both reaches more than 99.5%.

[0015] The structural formula of the phosphoric acid cyclic anhydride is as follows:

[0016] Among them, R 1 It is an alkyl group having 1 to 4 carbon atoms.

[0017] The phosphoric acid cyclic anhydride is preferably 1-propyl phosphoric acid cyclic anhydride.

[0018] The organic solvent is any one of benzene, pyridine, ether and carbonate, preferably any one of toluene, o-xylene, tetrahydrofuran, ethylene glycol dimethyl ether, ethyl methyl carbonate, diethyl carbonate, pyridine, ethylene glycol diethyl ether and dimethyl carbonate, and most preferably pyridine.

[0019] The molar ratio of the lithium fluoride to the phosphoric acid cyclic anhydride is 3: 1. The concentration of the phosphoric acid cyclic anhydride in the system is 0.5-1.2 mol / L, preferably 0.7-1.0 mol / L.

[0020] The fluorination agent is hydrogen fluoride gas or hydrogen fluoride pyridine complex (preferably 70 wt % hydrogen fluoride pyridine solution).

[0021] The ratio of the amount of hydrogen fluoride to the amount of phosphoric acid cyclic anhydride in the fluorination reagent is 3:1.

[0022] Preferably, the system temperature is controlled at 20-40°C; more preferably, the system temperature is controlled at 20-30°C, and most preferably, the system temperature is controlled at 25±2°C; then the fluorination reagent is slowly added to the system, the addition is completed within 2.5-3 hours, and then the temperature is kept warm for 0.5-1 hour.

[0023] Further, in step (2): the reaction material of step (1) is concentrated, the concentration temperature is not more than 60°C, and the mass of the residue is concentrated to 2.5-2.7 times the mass of the theoretical product, and the temperature is reduced to 5-10°C for crystallization, and then filtered and dried to obtain lithium difluorophosphate.

[0024] In the present invention, preferably, lithium fluoride is used as the fluoride salt, 1-propyl phosphoric acid cyclic anhydride is used as the phosphoric acid cyclic anhydride, and hydrogen fluoride gas is used as the fluorination agent for the reaction. The reaction principle is:

[0025]

[0026] During the entire process of the above-mentioned preparation method, the water content of the solution is less than 100 ppm and the solution is protected by an inert gas.

[0027] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0028] (1) The raw materials for the reaction are easily available, the market supply and demand of the product is stable, and the solvent required for the reaction is also a relatively common solvent. Therefore, the process can be simple, the reaction does not produce toxic and harmful gases, the reaction has low requirements on the reaction equipment, and the production of lithium difluorophosphate with high product quality can be achieved.

[0029] (2) The purity of lithium difluorophosphate prepared by the present invention can reach more than 99.5%, which can fully meet the requirements of electrolyte preparation. In addition, the reaction yield is high, and the obtained solid particles have good dispersibility, which is conducive to the promotion of lithium difluorophosphate as a new type of lithium salt high and low temperature performance additive. It has very large commercial value, social value and economic value.

[0030] (3) The present invention uses relatively easy-to-obtain 1-propylphosphoric acid cyclic anhydride and lithium fluoride as raw materials, performs fluorination reaction with hydrogen fluoride at room temperature, and adopts a solvent thermal method to quickly and efficiently prepare lithium difluorophosphate with high purity (more than 99.5%) and yield (more than 95%). The reaction time and reaction efficiency are greatly improved, which is very helpful for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the ion chromatogram of lithium difluorophosphate prepared in Example 3. DETAILED DESCRIPTION

[0032] The applicant further describes the technical solution of the present invention in conjunction with specific embodiments below, but the scope of protection requested by the claims of the present invention is not limited to these embodiments.

[0033] The inert gas environment described in the following embodiments and comparative examples is a nitrogen environment.

[0034] Embodiment 1 A method for preparing lithium difluorophosphate comprises the following steps:

[0035] (1) At room temperature (25° C.), under an inert gas environment, add 988 ml of pyridine to a 2 L 316 stainless steel reaction bottle (hereinafter referred to as the “reaction bottle”), and then add 77.82 g (3.00 mol) of lithium fluoride (electronic grade, the same below) and 318.8 g (1.00 mol) of 1-propylphosphoric acid cyclic anhydride, and use magnetic stirring to evenly disperse the reaction raw materials;

[0036] (2) Seal the reaction bottle containing the reaction raw materials and place it in a low-temperature coolant circulation pump;

[0037] (3) Cool the reaction bottle in step (2) to -10°C with cold ethanol, then introduce 60.03 g of hydrogen fluoride gas for 2.5-3 h;

[0038] (4) After ventilation, the reaction was kept at -10°C for 1 h;

[0039] (5) placing the reaction bottle containing the reaction material of step (4) in an oil bath, slowly heating to 35-40° C. for concentration, and concentrating until the mass of the residue is 2.5 times the mass of the theoretical product, then cooling to 10° C. for crystallization, filtering the material, and drying the wet solid of the filter cake at a drying temperature of 105° C. for 24 h, finally obtaining 291.4 g of lithium difluorophosphate solid, with a yield of 90.02% and a product purity of 99.53%.

[0040] The lithium difluorophosphate solid product obtained in step (5) is placed in a container, and then the container is shaken. The product has good fluidity in the container, indicating that the product has good dispersibility.

[0041] Embodiment 2 A method for preparing lithium difluorophosphate comprises the following steps:

[0042] (1) At room temperature (25° C.), under an inert gas environment, add 988 ml of pyridine to a 2 L 316 stainless steel reaction bottle, then add 77.82 g of lithium fluoride and 318.8 g of 1-propylphosphoric acid cyclic anhydride, and use magnetic stirring to evenly disperse the reaction materials;

[0043] (2) Seal the reaction bottle containing the reaction raw materials;

[0044] (3) introducing 60.03 g of hydrogen fluoride gas into the reaction bottle in step (2) for 2.5-3 h;

[0045] (4) After ventilation, continue the reaction at room temperature for 1 h;

[0046] (5) placing the reaction bottle containing the reaction material of step (4) in an oil bath, heating to 35-40° C. for concentration, concentrating until the mass of the residue is 2.5 times the mass of the theoretical product, then cooling to 10° C. for crystallization, filtering the material, and drying the wet solid of the filter cake at a drying temperature of 105° C. for 24 h, finally obtaining 307.5 g of lithium difluorophosphate solid, with a yield of 95% and a product purity of 99.73%.

[0047] The lithium difluorophosphate solid product obtained in step (5) is placed in a container, and then the container is shaken. The product has good fluidity in the container, indicating that the product has good dispersibility.

[0048] Embodiment 3 A method for preparing lithium difluorophosphate comprises the following steps:

[0049] (1) At room temperature (25° C.), under an inert gas environment, add 988 ml of pyridine to a 2 L 316 stainless steel reaction bottle, then add 77.82 g of lithium fluoride and 318.8 g of 1-propylphosphoric acid cyclic anhydride, and use magnetic stirring to evenly disperse the reaction materials;

[0050] (2) Seal the reaction bottle containing the reaction raw materials and place it in an oil bath;

[0051] (3) The reaction flask in step (2) was heated to 40° C. in an oil bath, and then 60.03 g of hydrogen fluoride gas was introduced for 2.5-3 h;

[0052] (4) After ventilation, keep the reaction at 40°C for 1 hour;

[0053] (5) The reaction bottle containing the reaction material of step (4) was concentrated at 35-40° C. until the mass of the residue was 2.5 times the mass of the theoretical product, and then the temperature was cooled to 10° C. for crystallization. The material was filtered and the wet solid of the filter cake was dried at a drying temperature of 105° C. for 24 h to finally obtain 297.8 g of lithium difluorophosphate solid with a yield of 92% and a product purity of 99.60%.

[0054] The lithium difluorophosphate solid product obtained in step (5) is placed in a container, and then the container is shaken. The product has good fluidity in the container, indicating that the product has good dispersibility.

[0055] Embodiment 4 A method for preparing lithium difluorophosphate comprises the following steps:

[0056] (1) At room temperature (25° C.), under an inert gas environment, add 1115.6 ml of pyridine to a 2 L 316 stainless steel reaction bottle, then add 125.96 g (3.00 mol) of sodium fluoride and 318.8 g (1.00 mol) of 1-propylphosphoric acid cyclic anhydride, and use magnetic stirring to evenly disperse the reaction materials;

[0057] (2) Seal the reaction bottle containing the reaction raw materials;

[0058] (3) introducing 60.03 g of hydrogen fluoride gas into the reaction bottle in step (2) for 2.5-3 h;

[0059] (4) After ventilation, continue the reaction at room temperature for 1 h;

[0060] (5) The reaction bottle containing the reaction material of step (4) was placed in an oil bath, heated to 35-40° C. for concentration, and concentrated until the mass of the residue was 2.5 times the mass of the theoretical product, then cooled to 10° C. for crystallization, the material was filtered, and the wet solid of the filter cake was dried at a drying temperature of 105° C. for 24 h, and finally 355.1 g of sodium difluorophosphate solid was obtained, with a yield of 95.5% and a product purity of 99.69%.

[0061] The solid sodium difluorophosphate product obtained in step (5) is placed in a container, and then the container is shaken. The product has good fluidity in the container, indicating that the product has good dispersibility.

[0062] Embodiment 5 A method for preparing lithium difluorophosphate comprises the following steps:

[0063] (1) At room temperature (25° C.), under an inert gas environment, add 1260.5 ml of pyridine to a 2 L 316 stainless steel reaction bottle, then add 174.3 g (3.00 mol) of potassium fluoride and 318.8 g (1.00 mol) of 1-propylphosphoric acid cyclic anhydride, and use magnetic stirring to evenly disperse the reaction materials;

[0064] (2) Seal the reaction bottle containing the reaction raw materials;

[0065] (3) introducing 60.03 g of hydrogen fluoride gas into the reaction bottle in step (2) for 2.5-3 h;

[0066] (4) After ventilation, continue the reaction at room temperature for 1 h;

[0067] (5) The reaction bottle containing the reaction material of step (4) was placed in an oil bath, the temperature was raised to 35-40° C. for concentration, and the residue was concentrated to 2.5 times the mass of the theoretical product, and then the temperature was lowered to 10° C. for crystallization. The material was filtered, and the wet solid of the filter cake was dried at a drying temperature of 105° C. for 24 h, and finally 403.4 g of potassium difluorophosphate solid was obtained, with a yield of 96.0% and a product purity of 99.65%.

[0068] The potassium difluorophosphate solid product obtained in step (5) is placed in a container, and then the container is shaken. The product has good fluidity in the container, indicating that the product has good dispersibility.

[0069] Embodiment 6 A method for preparing lithium difluorophosphate comprises the following steps:

[0070] (1) At room temperature (25° C.), under an inert gas environment, add 988 ml of pyridine to a 2 L 316 stainless steel reaction bottle, then add 77.82 g of lithium fluoride and 318.8 g of 1-propylphosphoric acid cyclic anhydride, and use magnetic stirring to evenly disperse the reaction materials;

[0071] (2) Seal the reaction bottle containing the reaction raw materials and put it into a hot oil pan;

[0072] (3) The reaction flask in step (2) was heated to 60° C. in an oil bath, and then 60.03 g of hydrogen fluoride gas was introduced for 2.5-3 h;

[0073] (4) After the ventilation is completed, the reaction is kept at 60°C for 1 hour;

[0074] (5) The reaction bottle containing the reaction material of step (4) was concentrated at 55-60° C. until the mass of the residue was 2.5 times the mass of the theoretical product, and then the temperature was cooled to 10° C. for crystallization. The material was filtered and the wet solid of the filter cake was dried at a drying temperature of 105° C. for 24 h to finally obtain 296.1 g of lithium difluorophosphate solid with a yield of 91.5% and a product purity of 99.59%.

[0075] The lithium difluorophosphate solid product obtained in step (5) is placed in a container, and then the container is shaken. The product has good fluidity in the container, indicating that the product has good dispersibility.

[0076] Embodiment 7 A method for preparing lithium difluorophosphate comprises the following steps:

[0077] (1) At room temperature (25° C.), under an inert gas environment, add 988 ml of pyridine to a 2 L 316 stainless steel reaction bottle, then add 77.82 g of lithium fluoride and 318.8 g of 1-propylphosphoric acid cyclic anhydride, and use magnetic stirring to evenly disperse the reaction materials;

[0078] (2) Seal the reaction bottle containing the reaction raw materials;

[0079] (3) adding 85.75 g of 70 wt % hydrogen fluoride pyridine solution to the reaction bottle in step (2) dropwise for 2.5-3 h;

[0080] (4) After the addition was completed, the reaction was continued at room temperature for 1 h;

[0081] (5) placing the reaction bottle containing the reaction material of step (4) in an oil bath, heating to 35-40° C. for concentration, concentrating until the mass of the residue is 2.5 times the mass of the theoretical product, then cooling to 10° C. for crystallization, filtering the material, and drying the wet solid of the filter cake at a drying temperature of 105° C. for 24 h, finally obtaining 294.9 g of lithium difluorophosphate solid, with a yield of 91.1% and a product purity of 99.53%.

[0082] The lithium difluorophosphate solid product obtained in step (5) is placed in a container, and then the container is shaken. The product has good fluidity in the container, indicating that the product has good dispersibility.

[0083] Comparative Example 1 A method for preparing lithium difluorophosphate comprises the following steps:

[0084] (1) At room temperature (25° C.), under an inert gas environment, add 988 ml of pyridine to a 2 L 316 stainless steel reaction bottle, then add 76.5 g (2.95 mol) of lithium fluoride and 318.8 g (1.00 mol) of 1-propylphosphoric acid cyclic anhydride, and stir the reaction materials uniformly using a magnetic stirrer;

[0085] (2) Seal the reaction bottle containing the reaction raw materials;

[0086] (3) introducing 60.03 g of hydrogen fluoride gas into the reaction bottle in step (2) for 2.5-3 h;

[0087] (4) After ventilation, continue the reaction at room temperature for 1 h;

[0088] (5) placing the reaction bottle containing the reaction material of step (4) in an oil bath, heating to 35-40° C. for concentration, concentrating until the mass of the residue is 2.5 times the mass of the theoretical product, then cooling to 10° C. for crystallization, filtering the material, and drying the wet solid of the filter cake at a drying temperature of 105° C. for 24 h, finally obtaining 294.6 g of lithium difluorophosphate solid, with a yield of 92.5% and a product purity of 98.9%.

[0089] It can be seen from the comparison between Example 2 and Comparative Example 1 that when the molar ratio of lithium fluoride to 1-propyl phosphoric acid cyclic anhydride is less than 3, the raw material 1-propyl phosphoric acid cyclic anhydride cannot react completely, thereby affecting the purity of the product.

[0090] Comparative Example 2 A method for preparing lithium difluorophosphate comprises the following steps:

[0091] (1) At room temperature (25° C.), under an inert gas environment, add 988 ml of pyridine to a 2 L 316 stainless steel reaction bottle, then add 103.76 g (4 mol) of lithium fluoride and 318.8 g of 1-propylphosphoric acid cyclic anhydride, and use magnetic stirring to evenly disperse the reaction materials;

[0092] (2) Seal the reaction bottle containing the reaction raw materials;

[0093] (3) introducing 60.03 g of hydrogen fluoride gas into the reaction bottle in step (2) for 2.5-3 h;

[0094] (4) After ventilation, continue the reaction at room temperature for 1 h;

[0095] (5) The reaction bottle containing the reaction material of step (4) was placed in an oil bath, heated to 35-40°C for concentration, and concentrated until the mass of the residue was 2.5 times the mass of the theoretical product, then cooled to 10°C for crystallization, the material was filtered, and the wet solid of the filter cake was dried at a drying temperature of 105°C for 24 hours to finally obtain 324.1 g of lithium difluorophosphate solid with a product purity of 92%.

[0096] (6) At room temperature (25° C.), the 92% pure product obtained in step (5) was added to 971 g of ethylene glycol dimethyl ether. After slowly dissolving, the material was filtered. The filtrate was heated to 35-40° C. and concentrated. After concentrating until the mass of the residue was 2.1 times the mass of the theoretical product, the temperature was lowered to 10° C. for crystallization. The material was filtered and the wet solid of the filter cake was dried at 105° C. for 24 h to obtain 277.33 g of a solid product with a yield of 85.67% and a product purity of 99.78%.

[0097] It can be seen from Example 2 compared with Comparative Example 1 that when the molar ratio of lithium fluoride to 1-propylphosphoric acid cyclic anhydride is greater than 3, the raw material lithium fluoride is excessive, the purity of the obtained product does not meet the standard, and further impurity removal is required to obtain a high-purity product. However, the purification and impurity removal step affects the yield of the product.

Claims

1. A method for preparing a difluorophosphate, characterized in that: The steps include: (1) In a closed inert gas environment, lithium fluoride solid and phosphoric acid cyclic anhydride are added to an organic solvent and dispersed evenly, the system temperature is controlled at -10°C to 60°C, and then the fluorination reagent is slowly added to the system. After the addition is completed, the system is kept warm. The total reaction time is 3 to 4 hours; (2) concentrating the reaction material of step (1), cooling and crystallizing, filtering and drying to obtain lithium difluorophosphate, wherein the purity of the lithium difluorophosphate reaches more than 99.5%; The structural formula of the phosphoric acid cyclic anhydride is as follows: Wherein, R1 is an alkyl group having 1 to 4 carbon atoms; The fluorination agent is hydrogen fluoride gas or hydrogen fluoride pyridine complex; The molar ratio of the lithium fluoride to the phosphoric acid cyclic anhydride is 3:1, and the molar ratio of the hydrogen fluoride to the phosphoric acid cyclic anhydride in the fluorination reagent is 3:1; Alternatively, the lithium fluoride in step (1) is replaced by sodium fluoride or potassium fluoride, and finally in step (2) sodium difluorophosphate or potassium difluorophosphate is obtained, respectively, and the purity of both reaches above 99.5%.

2. The preparation method according to claim 1, characterized in that: The phosphoric acid cyclic anhydride is 1-propyl phosphoric acid cyclic anhydride.

3. The preparation method according to claim 1 or 2, characterized in that: The organic solvent is any one of benzene, pyridine, ether and carbonate.

4. The preparation method according to claim 3, characterized in that: The organic solvent is any one of toluene, o-xylene, tetrahydrofuran, ethylene glycol dimethyl ether, ethyl methyl carbonate, diethyl carbonate, pyridine, ethylene glycol diethyl ether and dimethyl carbonate.

5. The preparation method according to claim 1, characterized in that: The concentration of phosphoric acid cyclic anhydride in the system is 0.5-1.2 mol / L.

6. The preparation method according to claim 5, characterized in that: The concentration of phosphoric acid cyclic anhydride in the system is 0.7-1.0 mol / L.

7. The preparation method according to claim 1, characterized in that: The hydrogen fluoride pyridine complex is a 70 wt % hydrogen fluoride pyridine solution.

8. The preparation method according to claim 1, characterized in that: In step (1), the system temperature is controlled at 20-40°C.

9. The preparation method according to claim 8, characterized in that: In step (1), the system temperature is controlled at 20-30° C., preferably, the system temperature is controlled at 25±2° C. Then, the fluorination reagent is slowly added to the system, the addition is completed over 2.5-3 hours, and the temperature is kept warm for 0.5-1 hour.

10. The preparation method according to claim 1, characterized in that: In step (2), the temperature is raised to no more than 60° C. during concentration, and the residue is concentrated until its mass is 2.5-2.7 times the mass of the theoretical product, and then the temperature is lowered to 5-10° C. for crystallization.

Citation Information

Patent Citations

  • Preparation method of difluoro lithium phosphate

    CN108033435A

  • Preparation method of lithium difluorophosphate

    CN113336214A

  • Method for producing difluorophosphate

    US20150064091A1

  • Preparation method for lithium difluorophosphate and product obtained therefrom

    WO2024002386A1