Carboxylic acid copolymer assisted synthesized large-wall-thickness mesoporous molecular sieve and preparation method thereof
By using the composite technology of carboxylic acid copolymer and nonionic surfactant to increase the pore wall thickness of mesoporous molecular sieves, the problem of insufficient stability of mesoporous molecular sieves is solved, and higher stability and application potential are achieved.
Patent Information
- Application Number
- CN202310378771.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-11
AI Technical Summary
The existing mesoporous molecular sieves have low pore wall thickness, resulting in poor stability and limiting their application in harsh chemical processes.
The precursor of the Y-type molecular sieve is assembled using a combination of carboxylic acid copolymer and nonionic surfactant. The electrostatic repulsion and steric hindrance effect of the carboxylic acid copolymer are used to improve the unit cell parameters of the mesoporous molecular sieve, thereby increasing the pore wall. thickness.
The pore wall thickness and stability of the mesoporous molecular sieve are significantly improved, enhancing its application potential in harsh chemical processes.
Smart Images

Figure CN118791009A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of mesoporous molecular sieve synthesis, and particularly relates to a carboxylic acid copolymer-assisted synthesis of a thick-walled mesoporous molecular sieve and a preparation method thereof. Background Art
[0002] Mesoporous molecular sieves are considered to have broad prospects in the field of heavy oil macromolecule conversion due to their large specific surface area, regular and adjustable pore structure and other excellent properties. However, the amorphous pore wall leads to poor hydrothermal stability, which greatly limits its application in harsh chemical processes. Therefore, it is of great significance to increase the pore wall thickness of mesoporous molecular sieves and thus improve their stability.
[0003] Kresge (Nature, 1992, 359 (6397): 710-712) reported a method for synthesizing high-wall-thick mesoporous molecular sieves by calcining a liquid crystal structure formed by a template and a silicate. The synthesized sample has mesoporous order, and its pore size can be adjusted by adding different templates or changing the reaction conditions. This method uses the liquid crystal structure formed by the template micelle as a template, and the silicate species polymerizes around the block copolymer micelle to form a pore wall, thereby forming a mesoporous molecular sieve.
[0004] Sangchoom (Journal of Materials Chemistry, 2012, 22(36): 18872-18878) synthesized pure silica MCM-41 samples using fumed silica, CTAB, tetramethylammonium hydroxide (TMAOH) and water as raw materials. The effect of high temperature synthesis on the stability of structural order was studied. The increase in crystallization temperature leads to an increase in pore size and a decrease in long-range order, but at the same time can produce thicker pore walls. The molecular sieve samples synthesized at 190°C showed thicker pore walls, and The hole wall thickness at 150℃ Compared with the This is significantly higher than previously reported.
[0005] Cyril (Microporous and Mesoporous Materials, 2018, 271: 196-202) synthesized SBA-15 by sol-gel method. The effect of chloride ions on the structure and surface properties of SBA-15 was explored by changing the HCl concentration, with the aim of adjusting the surface density of active hydroxyl groups that can be used for subsequent derivatization. The results showed that during the sol-gel preparation of SBA-15, the surface silanol coverage increased by two times as the HCl concentration increased from 0 to 2.0 M, while the mesoporous pore size also slightly widened from 4.2 nm to 4.9 nm. However, the smaller unit cell parameters are not conducive to the large-scale transport of macromolecules or macromolecules.
[0006] Yuan et al. (Langmuir, 2008, 24(9):5038-5043) studied mesoporous silica by using P123 and perfluorooctanoic acid (PFOA) as co-templates in an acid-catalyzed sol-gel process. The results showed that by increasing the molar ratio of PFOA / P123 as the co-template, a structural transition from a rod-like two-dimensional hexagonal mesostructure to a sharp-edged structure can be achieved, and the wall thickness of silica can be greatly increased.
[0007] Jomekian (Journal of Porous Materials, 2012, 19: 979-988) used tetraethyl orthosilicate as a silica source, 1-hexadecylamine as a template, and 1,3,5-trimethylbenzene as an organic auxiliary reagent to synthesize a new type of mesoporous MCM-41. Compared with the maximum wall thickness of 1.8 nm of mesoporous MCM-41 prepared by traditional methods, the wall thickness of the molecular sieve sample obtained by removing the template by solvent extraction in this study is The hole diameter is
[0008] An et al. (Journal of the Chinese Ceramic Society, 2019, 47(04): 473-479) used F127 as a template and methyl cellulose (MC) as a template co-agent. They added MC to the F127 solution using a conventional method to synthesize MC-SBA-16 mesoporous molecular sieve, and used it as a carrier to prepare a Ni-based catalyst. The prepared catalyst was applied to the hydrogenation reaction for catalytic testing and compared with Ni-containing SBA-16. The results showed that with the addition of MC, MC can play a good dispersing role, thereby changing some structural properties of the product, such as increasing the specific surface area and pore size. However, the molecular weight of the block copolymer F127 is small, and it is impossible to ensure that the micelles formed can be evenly arranged and dispersed during the assembly process, resulting in a small unit cell parameter of the synthesized SBA-16.
[0009] The precursor assembly technology introduces the primary and secondary structural units of the microporous molecular sieve into the pore wall of the mesoporous molecular sieve, increases the wall thickness of the molecular sieve and improves the hydrothermal stability of the mesoporous molecular sieve.
[0010] Luo et al. (Journal of Chemistry in Universities, 2007(05):801-805) prepared highly ordered mesoporous silica-alumina molecular sieve MSAMS-4 by placing the calcined SBA-15 in a dilute solution of β molecular sieve precursor and glycerol for two high temperature crystallization processes. The results showed that the microstructure units of the microporous molecular sieve were introduced into the pore wall of the mesoporous molecular sieve, and the pore wall thickness of the obtained silica-alumina molecular sieve MSAMS-4 increased by 1.0 nm.
[0011] Laha et al. (Microporous and mesoporous materials, 2010, 133 (1-3): 82-90) used tetraethylammonium hydroxide (TEAOH) as a template agent, and under alkaline conditions, used HS-40 silica sol and aluminum hydroxide nonahydrate as silicon and aluminum sources, and obtained a sol precursor containing β molecular sieve structural units after stirring and mixing crystallization; then, under the action of mesoporous template agents lauric acid alcohol polyoxyethylene ether and CTAB, Al-MCM-48-BEA molecular sieve was self-assembled and synthesized. XRD results show that Al-MCM-48-BEA still maintains good mesoporous order after being treated in boiling water for 120h and in 700℃ steam for 4h. Due to the presence of β molecular sieve structure in Al-MCM-48-BEA, the mesoporous pore wall of the sample becomes thicker.
[0012] Li (Spectrochimica Acta Part A: Molecular and Biomolecular Spectroscopy, 2013, 107: 218-226) studied the introduction of Y-type molecular sieve as a precursor into the formation process of MCM-41 molecular sieve. The study found that when the Y-type precursor was mixed with hexadecyltrimethylammonium bromide (CTAB), the precursor containing the secondary building unit of the Y-type molecular sieve would promote the formation of a metastable mesoporous structure. On the contrary, low-polymerization aluminosilicates and well-crystallized molecular sieve crystals could not be assembled with CTAB in the secondary stage. The results show that the high anionic charge density and the appropriate multi-coordination number of the secondary structural unit of the molecular sieve promote the formation of mesoporous walls. Its unit cell parameter a0 is 4.4nm and the wall thickness is 1.9nm.
[0013] Mi et al. (Industrial & Engineering Chemistry Research, 2017, 56, 25, 7224–7228) synthesized mesoporous molecular sieves by introducing the ionic surfactant sodium dodecyl sulfate (SDS) into extremely low concentration copolymers. The unit cell parameter a0 of the molecular sieve sample is 11.47 nm, and the pore wall thickness is 5.27 nm. The study found that even at low concentrations of P123, the strong interaction between the hydrophobic chains of sodium dodecyl sulfate (SDS) and the polypropylene oxide (PPO) units of P123 can lead to the formation of mixed micelles. The self-aggregation of SDS molecules can induce the formation of mixed micelles, the core of which is composed of SDS micelles with PPO units and poly (ethylene oxide PEO) units. The introduction of ionic surfactants can improve the wall thickness and stability of mesoporous molecular sieves.
[0014] Although the precursor assembly method has greatly improved the wall thickness and stability of mesoporous molecular sieves, the stability of this process still needs to be improved. The reason is that the pore wall thickness of mesoporous molecular sieves is relatively low. Therefore, improving the pore wall thickness of mesoporous molecular sieves synthesized by the precursor assembly method has important theoretical significance and application value.
[0015] The Chinese patent application document with publication number CN104591200A discloses a preparation method for significantly increasing the lattice spacing and pore wall thickness of SBA-15 mesoporous molecular sieve, which belongs to the field of inorganic porous material preparation technology. The polymer P123 is used as the main template agent, and another enol polymer is used as the auxiliary template agent. Under hydrothermal conditions, a co-condensation-hydrolysis reaction is performed to prepare an SBA-15 mesoporous molecular sieve with significantly increased molecular lattice spacing and pore wall thickness, improve thermal and hydrothermal stability, and greatly increase its application potential as a large pore size, large specific surface area, especially as a thick pore wall carrier material in many fields such as energy chemical industry, environmental protection and biotechnology. However, the patent does not disclose the use of a carboxylic acid copolymer to prepare a mesoporous molecular sieve. Summary of the invention
[0016] The technical problem to be solved by the present invention is how to solve the problem that the pore wall thickness of the existing mesoporous molecular sieve is relatively low, thereby resulting in poor stability of the mesoporous molecular sieve.
[0017] The present invention solves the above technical problems through the following technical means:
[0018] The first aspect of the present invention provides a method for synthesizing a high-stability mesoporous molecular sieve assisted by a carboxylic acid copolymer, comprising the following steps:
[0019] (1) Preparation of Y-type precursor:
[0020] Aluminum source, Na2O, silicon source and water are stirred and mixed to obtain a Y-type precursor solution;
[0021] (2) Carboxylic acid copolymers assisted by block nonionic surfactants to synthesize mesoporous molecular sieves:
[0022] The nonionic surfactant is dissolved in water, and then the carboxylic acid copolymer is added and stirred. After the solution is dissolved, the Y-type precursor solution is added dropwise. After the addition is completed, the mixture is assembled and then transferred to a polytetrafluoroethylene reactor for crystallization. The mesoporous molecular sieve product is obtained through filtration, washing, drying and calcination.
[0023] Beneficial effects: The present invention uses a composite of a carboxylic acid copolymer and a nonionic surfactant to assemble a Y-type molecular sieve precursor, and utilizes the electrostatic repulsion and steric hindrance effect of the carboxylic acid copolymer to greatly improve the unit cell parameters of the mesoporous molecular sieve, thereby obtaining a mesoporous molecular sieve with a larger pore wall thickness.
[0024] Preferably, the stirring in step (1) is specifically: stirring at 40-100° C. for 5-15 hours.
[0025] Preferably, in step (1), the molar ratio of the aluminum source, Na2O, silicon source and water is 1:10-20:10-20:200-400.
[0026] Preferably, the aluminum source in step (1) is selected from one or more of aluminum sulfate 18hydrate (Al2(SO4)3·18H2O), aluminum nitrate (Al(NO3)3), sodium aluminate (NaAlO2), aluminum chloride (AlCl3), and aluminum isopropoxide (AIP).
[0027] Preferably, in step (1), the silicon source is selected from one or more of tetraethyl orthosilicate (TEOS), sodium orthosilicate (Na4SiO4), water glass, silicon powder, and silica sol.
[0028] Preferably, the nonionic surfactant in step (2) is selected from polyethylene oxide-polypropylene oxide-polyethylene oxide PEO 20 PPO 70 PEO 20 (P123), Polyethylene oxide-Polypropylene oxide-Polyethylene oxide PEO 80 PPO 30 PEO 80 (F68), Polyethylene oxide-polypropylene oxide-polyethylene oxide PEO 106 PPO 70 PEO 106 (F127), Polyethylene oxide-Polypropylene oxide-Polyethylene oxide PEO 43 PPO 14 PEO 43(F38) one or more block copolymers.
[0029] Preferably, in step (2), the carboxylic acid copolymer is selected from one of methyl methacrylate copolymer (AMPS), phosphoryl carboxylic acid copolymer (POCA), maleic acid-acrylic acid copolymer (AAMA), and acrylic acid-itaconic acid copolymer (IA-Co-AA).
[0030] Preferably, in step (2), the mass ratio of the carboxylic acid copolymer to the non-ionic surfactant is 1:50-300.
[0031] Preferably, in step (2), the mass ratio of the carboxylic acid copolymer to water is 1:10-100.
[0032] Preferably, the crystallization temperature in step (2) is 80-150° C., and the crystallization time is 1-4 days.
[0033] Preferably, the calcination conditions in step (2) are: temperature 400-800° C., 4-8 h.
[0034] The second aspect of the present invention provides a mesoporous molecular sieve prepared by the above method.
[0035] The advantages of the present invention are:
[0036] 1. The present invention uses a carboxylic acid copolymer and a nonionic surfactant to assemble the precursor of the Y-type molecular sieve, and utilizes the electrostatic repulsion and steric hindrance effect of the carboxylic acid copolymer to greatly improve the unit cell parameters of the mesoporous molecular sieve, thereby obtaining a mesoporous molecular sieve with a larger pore wall thickness.
[0037] 2. The present invention uses carboxylic acid copolymers as auxiliary templates to synthesize mesoporous molecular sieves. For example, AAMA contains multiple -COOH bonds, which interact with the PEO segment in the block copolymer F68 to form composite micelles. The presence of multiple carboxyl groups increases the electrostatic repulsion of the micelles; and there is a large steric hindrance, which increases the unit cell parameters of the micelle sample. When the pore diameters are close, the increase in the unit cell parameters will greatly increase the pore wall thickness of the molecular sieve. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is the XRD characterization result diagram of the mesoporous molecular sieve prepared in Example 1. It can be seen that the product has a typical ordered two-dimensional mesoporous structure.
[0039] Figure 2 This is a diagram showing the BET characterization results of the mesoporous molecular sieve prepared in Example 1. It can be seen that the product has a hysteresis loop that is unique to mesoporous materials.
[0040] Figure 3This is a pore size distribution curve of the mesoporous molecular sieve prepared in Example 1. It can be seen that the product has a mesoporous structure. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] The experimental methods in the following examples are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified.
[0043] Source of raw materials: Aluminum sulfate and other raw materials are from PetroChina Lanzhou Petrochemical Company, all of which are industrial products; the template agent is purchased from Jiangsu Hai'an Petrochemical Chemical Co., Ltd., which is an industrial product; tetraethyl orthosilicate and maleic acid-acrylic acid copolymer are both commercially available reagents, industrial grade.
[0044] Analysis method: Phase detection and confirmation were performed using the XRD-7000 X-ray crystal powder diffractometer from Shimadzu Corporation of Japan. Instrument parameters: Cu-Ka ray, wavelength 0.1543nm, tube voltage 40kV, tube current 50mA. Sample test conditions: scanning angle 0.5°-5°, scanning speed 1° / min.
[0045] The ASAP2020M fully automatic adsorption instrument produced by Micromeritics Corporation of the United States was used to measure the adsorption-desorption isotherms of the samples at liquid nitrogen temperature. Nitrogen was used as the adsorbate. The Brunauer-Emmett-Teller (BET) equation was used to calculate the specific surface area of the samples according to the adsorption equilibrium isotherm between the relative pressure of 0.05 and 0.25. The t-plot model was used to distinguish the internal surface area and the external surface area of the samples. The static capacity method was used to determine the pore volume and pore size distribution, thereby calculating the pore structure parameters.
[0046] Embodiment 1:
[0047] A method for synthesizing a high-stability mesoporous molecular sieve assisted by a carboxylic acid copolymer comprises the following steps:
[0048] (1) Preparation of Y-type precursor 1:
[0049] Prepared with a molar ratio of Al2(SO4)3·18H2O:Na2O:SiO2:H2O=1:18:15:320, stirred at 98°C for 8h;
[0050] (2) Synthesis of mesoporous molecular sieves:
[0051] At 35°C, 40g of nonionic surfactant F68 was dissolved in 600mL of deionized water, and then 0.6g of AAMA was added and stirred for 0.5h. After it was dissolved, 350g of Y-type precursor 1 solution was added dropwise, and the pH value of the solution was adjusted with sulfuric acid. After the addition was completed, the mixture was assembled for 20h, and then transferred to a polytetrafluoroethylene reactor for crystallization for 1d. The mesoporous molecular sieve product was obtained after filtration, washing, drying, and calcination at 550°C for 6h.
[0052] Embodiment 2:
[0053] A method for synthesizing a high-stability mesoporous molecular sieve assisted by a carboxylic acid copolymer comprises the following steps:
[0054] (1) Preparation of Y-type precursor 1:
[0055] Prepared with a molar ratio of Al2(SO4)3·18H2O:Na2O:SiO2:H2O=1:18:15:320, stirred at 98°C for 8h;
[0056] (2) Synthesis of mesoporous molecular sieves:
[0057] At 20°C, 20g of nonionic surfactant F38 was dissolved in 100mL of deionized water, and then 0.2g of POCA was added and stirred for 0.5h. After it was dissolved, 50g of Y-type precursor 1 solution was added dropwise, and the pH value of the solution was adjusted with sulfuric acid. After the addition was completed, the mixture was assembled for 10h, and then transferred to a polytetrafluoroethylene reactor for crystallization for 1d. The mesoporous molecular sieve product was obtained after filtration, washing, drying, and calcination at 400°C for 4h.
[0058] Embodiment 3:
[0059] A method for synthesizing a high-stability mesoporous molecular sieve assisted by a carboxylic acid copolymer comprises the following steps:
[0060] (1) Preparation of Y-type precursor 2:
[0061] Prepare with a molar ratio of Al(NO3)3:Na2O:SiO2:H2O=1:20:20:400 and stir at 40°C for 15h;
[0062] (2) Synthesis of mesoporous molecular sieves:
[0063] At 70°C, 40g of nonionic surfactant F127 was dissolved in 1000mL of deionized water, and then 2g of AMPS was added and stirred for 2h. After it was dissolved, 500g of Y-type precursor 2 solution was added dropwise, and the pH value of the solution was adjusted with sulfuric acid. After the addition was completed, the mixture was assembled for 40h, then transferred to a polytetrafluoroethylene reactor, crystallized for 4d, filtered, washed, dried, and calcined at 800°C for 8h to obtain a mesoporous molecular sieve product.
[0064] Embodiment 4:
[0065] A method for synthesizing a high-stability mesoporous molecular sieve assisted by a carboxylic acid copolymer comprises the following steps:
[0066] (1) Preparation of Y-type precursor 3:
[0067] Prepared with a molar ratio of Al2(SO4)3·18H2O:Na2O:SiO2:H2O=1:10:10:200, stirred at 100°C for 10h;
[0068] (2) Synthesis of mesoporous molecular sieves:
[0069] At 35°C, 100g of nonionic surfactant P123 was dissolved in 800mL of deionized water, and then 1g of AAMA was added and stirred for 1h. After it was dissolved, 500g of Y-type precursor 3 solution was added dropwise, and the pH value of the solution was adjusted with sulfuric acid. After the addition was completed, the mixture was assembled for 30h, then transferred to a polytetrafluoroethylene reactor, crystallized for 2d, filtered, washed, dried, and calcined at 600°C for 6h to obtain a mesoporous molecular sieve product.
[0070] Embodiment 5:
[0071] A method for synthesizing a high-stability mesoporous molecular sieve assisted by a carboxylic acid copolymer comprises the following steps:
[0072] (1) Preparation of Y-type precursor 4:
[0073] Molar ratio NaAlO2:Na2O:C8H 20 Prepare O4Si:H2O=1:15:15:300 and stir at 80°C for 8h;
[0074] (2) Synthesis of mesoporous molecular sieves:
[0075] At 50°C, 35g of nonionic surfactant F68 was dissolved in 500mL of deionized water, and then 0.5g of IA-Co-AA was added and stirred for 0.5h. After it was dissolved, 350g of Y-type precursor 4 solution was added dropwise, and the pH value of the solution was adjusted with sulfuric acid. After the addition was completed, the mixture was assembled for 25h, then transferred to a polytetrafluoroethylene reactor, crystallized for 2d, filtered, washed, dried, and calcined at 500°C for 8h to obtain a mesoporous molecular sieve product.
[0076] Embodiment 6:
[0077] A method for synthesizing a high-stability mesoporous molecular sieve assisted by a carboxylic acid copolymer comprises the following steps:
[0078] (1) Preparation of Y-type precursor 5:
[0079] Prepared with a molar ratio of AIP:Na2O:SiO2:H2O=1:16:15:400, stirred at 50°C for 10h;
[0080] (2) Synthesis of mesoporous molecular sieves:
[0081] At 35°C, 40g of nonionic surfactant F38 was dissolved in 600mL of deionized water, and then 1.5g of IA-Co-AA was added thereto, stirred for 0.5h, stirred for 2h, and after it was dissolved, 200g of Y-type precursor 5 solution was added dropwise thereto, and the pH value of the solution was adjusted with sulfuric acid. After the addition was completed, the mixture was assembled for 20h, and then transferred to a polytetrafluoroethylene reactor, crystallized for 3d, filtered, washed, dried, and calcined at 550°C for 4h to obtain a mesoporous molecular sieve product.
[0082] Embodiment 7:
[0083] A method for synthesizing a high-stability mesoporous molecular sieve assisted by a carboxylic acid copolymer comprises the following steps:
[0084] (1) Preparation of Y-type precursor 6:
[0085] Prepare with a molar ratio of AlCl3:Na2O:Na4SiO4:H2O=1:19:20:350 and stir at 35°C for 10h;
[0086] (2) Synthesis of mesoporous molecular sieves:
[0087] At 30°C, 50g of nonionic surfactant P123 was dissolved in 900mL of deionized water, and then 0.6g of POCA was added and stirred for 1h. After it was dissolved, 300g of Y-type precursor 6 solution was added dropwise, and the pH value of the solution was adjusted with sulfuric acid. After the addition was completed, the mixture was assembled for 24h, then transferred to a polytetrafluoroethylene reactor, crystallized for 4d, filtered, washed, dried, and calcined at 700°C for 5h to obtain a mesoporous molecular sieve product.
[0088] Embodiment 8:
[0089] A method for synthesizing a high-stability mesoporous molecular sieve assisted by a carboxylic acid copolymer comprises the following steps:
[0090] (1) Preparation of Y-type precursor 3:
[0091] Prepared with a molar ratio of Al2(SO4)3·18H2O:Na2O:SiO2:H2O=1:10:10:200, stirred at 100°C for 10h;
[0092] (2) Synthesis of mesoporous molecular sieves:
[0093] At 25°C, 20g of nonionic surfactant F127 was dissolved in 200mL of deionized water, and then 1.2g of AMPS was added and stirred for 0.5h. After it was dissolved, 450g of Y-type precursor 3 solution was added dropwise, and the pH value of the solution was adjusted with sulfuric acid. After the addition was completed, the mixture was assembled for 40h, and then transferred to a polytetrafluoroethylene reactor for crystallization for 3d. After filtering, washing, drying, and calcining at 800°C for 4h, the mesoporous molecular sieve product was obtained.
[0094] Embodiment 9:
[0095] A method for synthesizing a high-stability mesoporous molecular sieve assisted by a carboxylic acid copolymer comprises the following steps:
[0096] (1) Preparation of Y-type precursor 2:
[0097] Prepare with a molar ratio of Al(NO3)3:Na2O:SiO2:H2O=1:20:20:400 and stir at 40°C for 15h;
[0098] (2) Synthesis of mesoporous molecular sieves:
[0099] At 45°C, 10g of nonionic surfactant F38 was dissolved in 100mL of deionized water, and then 0.8g of AAMA was added and stirred for 1.2h. After it was dissolved, 150g of Y-type precursor 2 solution was added dropwise, and the pH value of the solution was adjusted with sulfuric acid. After the addition was completed, the mixture was assembled for 16h, then transferred to a polytetrafluoroethylene reactor, crystallized for 2d, filtered, washed, dried, and calcined at 400°C for 8h to obtain a mesoporous molecular sieve product.
[0100] Embodiment 10:
[0101] A method for synthesizing a high-stability mesoporous molecular sieve assisted by a carboxylic acid copolymer comprises the following steps:
[0102] (1) Preparation of Y-type precursor 5:
[0103] Prepared with a molar ratio of AIP:Na2O:SiO2:H2O=1:16:15:400, stirred at 50°C for 10h;
[0104] (2) Synthesis of mesoporous molecular sieves:
[0105] At 30°C, 50g of nonionic surfactant F68 was dissolved in 750mL of deionized water, and then 0.6g of IA-Co-AA was added and stirred for 1h. After it was dissolved, 300g of Y-type precursor 5 solution was added dropwise, and the pH value of the solution was adjusted with sulfuric acid. After the addition was completed, the mixture was assembled for 16h, then transferred to a polytetrafluoroethylene reactor, crystallized for 2d, filtered, washed, dried, and calcined at 400°C for 8h to obtain a mesoporous molecular sieve product.
[0106] Comparative Example 1:
[0107] (1) Preparation of Y-type precursor 1:
[0108] Prepared with a molar ratio of Al2(SO4)3·18H2O:Na2O:SiO2:H2O=1:18:15:320, stirred at 98°C for 8h;
[0109] (2) Synthesis of mesoporous molecular sieves:
[0110] At 35°C, 40g of nonionic surfactant F68 was dissolved in 600mL of deionized water and stirred for 0.5h. After it was dissolved, 350g of Y-type precursor 1 solution was added dropwise, and the pH value of the solution was adjusted with sulfuric acid. After the addition was completed, the mixture was assembled for 20h, then transferred to a polytetrafluoroethylene reactor, crystallized for 1d, filtered, washed, dried, and calcined at 550°C for 6h to obtain a mesoporous molecular sieve product.
[0111] Comparative Example 2:
[0112] (1) Preparation of Y-type precursor 1:
[0113] Prepared with a molar ratio of Al2(SO4)3·18H2O:Na2O:SiO2:H2O=1:18:15:320, stirred at 98°C for 8h;
[0114] (2) Synthesis of mesoporous molecular sieves:
[0115] At 35°C, 40g of nonionic surfactant F68 was dissolved in 600mL of deionized water, and then 0.6g of sodium α-olefin sulfonate was added and stirred for 0.5h. After it was dissolved, 350g of Y-type precursor 1 solution was added dropwise, and the pH value of the solution was adjusted with sulfuric acid. After the addition was completed, the mixture was assembled for 20h, and then transferred to a polytetrafluoroethylene reactor for crystallization for 1d. The mesoporous molecular sieve product was obtained after filtration, washing, drying, and calcination at 550°C for 6h.
[0116] Table 1 Physicochemical parameters of samples
[0117]
[0118] Comparative Example 1 is the relevant parameters in the sample when AAMA is not added. It can be seen from the table that the 2θ angle of the sample is large, resulting in a smaller unit cell parameter and a pore wall thickness of 5.61nm. While Example 1 is the relevant parameters of the sample when 0.6gAAMA is added under the same conditions. It can be seen that after adding AAMA, its 2θ angle is larger, resulting in a larger unit cell parameter. AAMA contains multiple -COOH bonds, which interact with the PEO segment in F68 to form a composite micelle. The presence of multiple carboxyl groups increases the electrostatic repulsion of the micelles; and there is a large steric hindrance itself, which increases the unit cell parameters of the micelle sample. When the pore size is close, the increase in the unit cell parameters will greatly increase the pore wall thickness of the molecular sieve.
[0119] Comparative Example 2 shows the relevant parameters of the sample after adding sodium α-olefin sulfonate. Sodium α-olefin sulfonate contains a hydrophilic group -SO3H, which interacts with the hydrophobic group of the block copolymer to disperse the composite micelles in the solution. This promotes the assembly of inorganic species and composite micelles and improves the order of the molecular sieve sample. This is similar to the addition of AAMA. However, the large steric hindrance effect of AAMA itself will increase the unit cell parameters of the molecular sieve sample, thereby increasing the pore wall thickness of the molecular sieve without affecting the pore size.
[0120] Figure 1 This is the XRD characterization result diagram of the mesoporous molecular sieve prepared in Example 1. From the figure, it can be seen that the product has a typical ordered two-dimensional mesoporous structure.
[0121] Figure 2 This is a diagram of the BET characterization results of the mesoporous molecular sieve prepared in Example 1. From the diagram, it can be seen that the product has a hysteresis loop that is unique to mesoporous materials.
[0122] Figure 3 This is a pore size distribution curve diagram of the mesoporous molecular sieve prepared in Example 1. From the diagram, it can be seen that the product has a mesoporous structure.
[0123] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for synthesizing a high-stability mesoporous molecular sieve assisted by a carboxylic acid copolymer, characterized in that: The following steps are involved: (1) Preparation of Y-type precursor: Aluminum source, Na2O, silicon source and water are stirred and mixed to obtain a Y-type precursor solution; (2) Carboxylic acid copolymers assisted by block nonionic surfactants to synthesize mesoporous molecular sieves: The nonionic surfactant is dissolved in water, and then the carboxylic acid copolymer is added and stirred. After the solution is dissolved, the Y-type precursor solution is added dropwise. After the addition is completed, the mixture is assembled and then transferred to a polytetrafluoroethylene reactor for crystallization. The mesoporous molecular sieve product is obtained through filtration, washing, drying and calcination.
2. The method for synthesizing high-stability mesoporous molecular sieves assisted by carboxylic acid copolymers according to claim 1, characterized in that: In the step (1), the molar ratio of the aluminum source, Na2O, silicon source and water is 1:10-20:10-20:200-400; the stirring in the step (1) is specifically: stirring at 40-100°C for 5-15h.
3. The method for synthesizing high-stability mesoporous molecular sieves assisted by carboxylic acid copolymers according to claim 1 or 2, characterized in that: In the step (1), the aluminum source is selected from one or more of aluminum sulfate 18hydrate (Al2(SO4)3·18H2O), aluminum nitrate (Al(NO3)3), sodium aluminate (NaAlO2), aluminum chloride (AlCl3), and aluminum isopropoxide (AIP); in the step (1), the silicon source is selected from one or more of tetraethyl orthosilicate (TEOS), sodium orthosilicate (Na4SiO4), water glass, silicon powder, and silica sol.
4. The method for synthesizing high-stability mesoporous molecular sieves assisted by carboxylic acid copolymers according to claim 3, characterized in that: The nonionic surfactant in step (2) is selected from polyethylene oxide-polypropylene oxide-polyethylene oxide PEO 20 PPO 70 PEO 20 (P123), Polyethylene oxide-Polypropylene oxide-Polyethylene oxide PEO 80 PPO 30 PEO 80 (F68), Polyethylene oxide-polypropylene oxide-polyethylene oxide PEO 106 PPO 70 PEO 106 (F127), Polyethylene oxide-Polypropylene oxide-Polyethylene oxide PEO 43 PPO 14 PEO 43 (F38) one or more block copolymers.
5. The method for synthesizing high-stability mesoporous molecular sieves assisted by carboxylic acid copolymers according to claim 4, characterized in that: In the step (2), the carboxylic acid copolymer is selected from one of methyl methacrylate copolymer (AMPS), phosphoryl carboxylic acid copolymer (POCA), maleic acid-acrylic acid copolymer (AAMA), and acrylic acid-itaconic acid copolymer (IA-Co-AA).
6. The method for synthesizing high-stability mesoporous molecular sieves assisted by carboxylic acid copolymers according to claim 1, characterized in that: In the step (2), the mass ratio of the carboxylic acid copolymer to the non-ionic surfactant is 1:50-300.
7. The method for synthesizing high-stability mesoporous molecular sieves assisted by carboxylic acid copolymers according to claim 1, characterized in that: In the step (2), the mass ratio of the carboxylic acid copolymer to water is 1:10-100.
8. The method for synthesizing high-stability mesoporous molecular sieves assisted by carboxylic acid copolymers according to claim 1, characterized in that: In the step (2), the crystallization temperature is 80-150° C., and the crystallization time is 1-4 days.
9. The method for synthesizing high-stability mesoporous molecular sieves assisted by carboxylic acid copolymers according to claim 1, characterized in that: The calcination conditions in step (2) are: temperature 400-800° C., 4-8 hours.
10. A mesoporous molecular sieve prepared by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Middle hole ZSM-5 zeolite microsphere and preparation method thereof
CN102001678A
Multiplayer coating system without titanium dioxide
CN102108232A
Synthetic method of mesoporous-microporous molecular sieve by raising hydrothermal stability
CN102745708A
Composite carrier, pH response type compound drug-loading system and preparation method of composite carrier
CN104548111A