Alumina-coated silica composite material and preparation method thereof
The coated alumina-silica composite material with a three-layer core-shell structure is formed by soaking and cleaning in stages, which solves the problems of incomplete coating layer and high cost in the existing technology, and achieves improved electrochemical performance and reduced production cost. Suitable for mass production.
Patent Information
- Application Number
- CN202411273299.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing technology, the low capacity and irreversible electrochemical reaction of graphite anode materials lead to a reduction in the energy density of lithium-ion batteries, and the use of atomic layer deposition to prepare a metal oxide coating layer is complex and costly, and nanometer silicon crystals react in water. As a result, the cladding layer is incomplete and the defects are difficult to repair.
By configuring sodium metaaluminate and hydrochloric acid solutions for sequential soaking and cleaning, a three-layer core-shell structure of alumina-coated silicon-oxygen composite material is formed. Alumina is used to repair defects, reducing production costs and being suitable for mass production.
The integrity and conductivity of the coating layer are improved, the loss of SiO and Si grains is reduced, the electrochemical performance is improved, the production cost is reduced, and it is suitable for large-scale production.
Smart Images

Figure CN118791028A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of negative electrode materials, and in particular to a silicon-oxygen composite material coated with aluminum oxide and a preparation method thereof. Background Art
[0002] With the rise of electric vehicles, the research on negative electrode materials is particularly important because it directly affects the performance and life of the battery. Traditional graphite negative electrode materials cannot meet the high capacity demand pursued by the current battery market due to their low capacity and initial efficiency. Among them, silicon monoxide (SiO)-based negative electrode materials are superior high-capacity negative electrode materials for commercial lithium-ion batteries (LIBs) due to their higher capacity than graphite and superior cycle life than other silicon-based negative electrode materials; however, these materials still have some problems. The more long-term problem is that the ICE is lower than 80%, which causes the lithium ions extracted from the positive electrode material in the first cycle to undergo an irreversible electrochemical reaction with SiO to form lithium silicate (Li 2 SiO 3 , Li 2 Si 2 O 5 and Li 4 SiO 4 ) is irreversibly consumed, reducing the actual energy density of LIBs, and lithium ions cannot be extracted again in the subsequent delithiation step.
[0003] How to solve the above SiO X The problems of the base anode material are imminent. Among them, the method of coating the carbon layer by vapor deposition is one of the more widely used methods. After coating the carbonaceous material, the ICE is significantly improved, up to about 77%. At the same time, the pre-SiO2 of the coated carbon layer is pre-physicalized to reduce the consumption of LIB on the positive electrode during the first cycle, and minimize the irreversible consumption of lithium ions from the positive electrode, such as: ①. The Chinese patent with application number 202310437793.2 and publication number CN116598446A provides a negative electrode material and a preparation method thereof, a negative electrode plate and a battery. The negative electrode material includes a pre-lithiated silicon-oxygen material, including but not limited to the pre-lithiated silicon-oxygen material and a metal oxide layer and a carbon layer sequentially coated on the surface from the inside to the outside, including preparing the metal oxide layer by atomic layer deposition and then mixing it with a carbon source intermediate and heating it for carbonization treatment; ②. A Chinese patent with application number 202011619509.6 and publication number CN112820863B discloses a modified pre-lithiated silicon oxide material, a preparation method, an application and a lithium-ion battery. This method pre-lithiates a silicon oxide material, which includes a pre-lithiated silicon oxide material and a coating layer. The pre-lithiated silicon oxide material includes lithium silicate and silicon grains, and the coating layer includes an aluminum oxide polymer. The pre-lithiated silicon oxide materials are respectively immersed in a sodium aluminate solution, filtered, and then the pre-lithiated silicon oxide material immersed in the sodium aluminate solution is immersed in a hydrochloric acid solution, filtered, dried, and heat treated to obtain the obtained product; ③. A Chinese patent with application number 202310300412.6 and publication number CN116314695A discloses a modified pre-lithiated silicon oxide material, a preparation method thereof, an electrode and a lithium-ion battery. The modified pre-lithiated silicon oxide material comprises a pre-lithiated silicon oxide precursor material and a defect repair material. The defect repair material is in-situ grown at the carbon-coated defects of the pre-lithiated silicon oxide precursor material.
[0004] In combination with the above technical solutions, most of the existing technologies have the following problems: (1) The metal oxide coating layer is prepared by atomic layer deposition. The thickness is controllable, but the process is complex and the cost is too high, which is not conducive to large-scale production. (2) The nano-silicon crystals provide most of the capacity of the pre-lithiation silicon-oxygen material. However, when cleaning the pre-physical and chemical materials, water will contact the core from the surface of the carbon layer destroyed by the silicon-oxygen material. Some nano-silicon crystals will react with water to generate hydrogen, which will lead to capacity loss and gas inhibition of the formation of a complete coating layer. In the case of an incomplete coating layer, the residual alkali may be too large. (3) During the pre-lithiation process, the volume of silicon and oxygen expands and defects are generated on the surface. The defects are prone to expose nano-silicon crystals, and Si+2H 2 O=SiO 2 +2H 2 ,Due to the generation of gas, it is difficult to coat the defects, and the coating layer is difficult to play the role of an effective waterproof layer.
[0005] In view of the above technical problems, the present invention provides a silicon-oxygen composite material coated with aluminum oxide and a preparation method thereof. Summary of the invention
[0006] The object of the present invention is to provide a silicon-oxygen composite material coated with aluminum oxide and a preparation method thereof, so as to solve the problems in the above-mentioned background technology.
[0007] To achieve the above object, the present invention provides the following technical solution: In a first aspect, the present invention provides a silicon-oxygen composite material coated with aluminum oxide, comprising the following steps: S1, prepare a sodium aluminate solution, immerse the pre-physicalized silica in the sodium aluminate solution, stir for 10 minutes, and filter to obtain a solid 1; S2, prepare a hydrochloric acid solution, immerse the solid 1 in the hydrochloric acid solution, stir for 5 minutes, and filter to obtain a solid 2; S3, repeating the soaking steps of S1 and S2 for 3 to 4 times with solid 2 to obtain solid 3; S4, adding solid 3 into purified water, stirring and washing for 20 min, and filtering to obtain solid 4; S5, placing the solid 4 in a vacuum dryer at 95°C and drying for 6 hours to finally obtain a silicon-oxygen composite material coated with aluminum oxide.
[0008] Preferably, the sodium aluminate solution is prepared by mixing sodium aluminate with pure water, and the content of sodium aluminate in the sodium aluminate solution is 0.5-10 wt %.
[0009] Preferably, the pre-physicalized silicon oxide is immersed in a sodium aluminate solution at a material weight ratio of 1:4.
[0010] Preferably, the hydrochloric acid solution is prepared from concentrated hydrochloric acid and pure water, and the content of concentrated hydrochloric acid in the hydrochloric acid solution is 0.49-9.8wt%.
[0011] Preferably, the solid 1 is immersed in a hydrochloric acid solution at a material weight ratio of 1:4.
[0012] Preferably, during the stirring and washing in step S4, the material weight ratio of the solid 3 to the purified water is 1:10.
[0013] The second aspect of the present invention provides a silicon-oxygen composite material coated with aluminum oxide obtained by the method of the first aspect of the present invention, wherein the composite material is a three-layer core-shell structure, wherein the three-layer core-shell structure comprises an inner core, an intermediate layer and an outermost layer; wherein the inner core is a Li-Si-O matrix, the intermediate layer is a carbon layer, and the outermost layer is an Al 2 O 3 Coating layer.
[0014] The present invention has at least the following beneficial effects: (1) The silicon-oxygen composite material coated with aluminum oxide and the preparation method thereof provided by the present invention use materials that are relatively easy to obtain and have low cost, are suitable for large-scale production, and reduce production costs; (2) The present invention provides a silicon-oxygen composite material coated with aluminum oxide and a preparation method thereof, wherein aluminum oxide is added to the outer coating layer for repair to reduce SiO X Internal SiO and Si grain loss, increasing electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is the XRD test diagram of the product obtained in Example 1 of the present invention; Figure 2Schematic diagram of the three-layer core-shell structure of the composite material of the present invention. DETAILED DESCRIPTION
[0016] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] The present invention provides a method for preparing a silicon-oxygen composite material coated with aluminum oxide, comprising the following steps: S1, prepare sodium aluminate solution, immerse pre-physicalized silica (D50 is 2-10 um) in the sodium aluminate solution at a material weight ratio of 1:4, stir for 10 minutes, filter and obtain solid 1; The sodium aluminate solution is prepared by mixing sodium aluminate with pure water, and the content of sodium aluminate in the sodium aluminate solution is 0.5-10wt%; S2, prepare hydrochloric acid solution, immerse solid 1 in the hydrochloric acid solution at a material weight ratio of 1:4, stir for 5 minutes, and filter to obtain solid 2; The hydrochloric acid solution is prepared by concentrating hydrochloric acid and pure water, and the content of the concentrating hydrochloric acid in the hydrochloric acid solution is 0.49-9.8wt%; S3, repeating the soaking steps of S1 and S2 for 3 to 4 times with solid 2 to obtain solid 3; S4, adding solid 3 into purified water at a material weight ratio of 1:10, stirring and washing for 20 minutes, and filtering to obtain solid 4; S5, placing the solid 4 in a vacuum dryer at 95°C and drying for 6 hours to finally obtain a silicon-oxygen composite material coated with aluminum oxide.
[0018] The present invention prepares sodium aluminate and hydrochloric acid into a low-concentration solution according to a certain ratio, and soaks the pre-treated silicon-oxygen composite material in batches, so that the defect positions of the pre-treated silicon-oxygen composite material react to form Al(OH) 3 Precipitation, and then oxidation of aluminum hydroxide to aluminum oxide by heating.
[0019] Based on the above technical solution, the present invention provides the following partial embodiments:
[0020] Example 1 (1) Preparation by soaking in sodium aluminate solution: Take 26g of sodium aluminate and dissolve it in 1200g of pure water. Wait until it is completely dissolved to form a sodium aluminate solution, and set it aside for use. Take 240ml of the sodium aluminate solution and place it in a beaker and stir. Take 60g of the material and put it into the beaker containing the sodium aluminate solution, stir for 10 minutes, and filter to obtain solid 1.
[0021] (2) Solid 1 is immersed in hydrochloric acid solution: Take 9.6g of concentrated hydrochloric acid and dissolve it in 1200g of pure water, stir to dissolve, prepare a hydrochloric acid solution with the same molar ratio as sodium aluminate, and set it aside for use; take 240ml of hydrochloric acid solution and place it in a beaker to stir, take out the solid soaked in sodium aluminate and put it in to stir, after stirring for 5 minutes, filter and obtain solid 2.
[0022] (3) Repeated coating modification: Repeat steps (1) (2) three times with the solid 2 obtained in (2) to obtain a solid 3.
[0023] (4) Solid 3 was placed in 10 times the volume of purified water for washing and stirring for 20 min to obtain solid 4.
[0024] (5) The solid 4 was placed in a vacuum oven at 95°C and dried for 6 h to obtain a silicon-oxygen composite material coated with aluminum oxide.
[0025] Example 2 The difference from Example 1 is that the content of sodium aluminate in the sodium aluminate solution of step (1) is 0.5wt%, and the content of concentrated hydrochloric acid in the hydrochloric acid solution of step (2) is 0.49wt%. The rest is the same as in Example 1, and the obtained coated pre-physicalized silicon oxide material is obtained.
[0026] Example 3 The difference from Example 1 is that the content of sodium aluminate in the sodium aluminate solution of step (1) is 1.5wt%, and the content of concentrated hydrochloric acid in the hydrochloric acid solution of step (2) is 1.47wt%. The rest is the same as in Example 1, and the obtained coated pre-physicalized silicon oxide material is obtained.
[0027] Example 4 The difference from Example 1 is that the content of sodium aluminate in the sodium aluminate solution of step (1) is 3.0wt%, and the content of concentrated hydrochloric acid in the hydrochloric acid solution of step (2) is 2.94wt%. The rest is the same as Example 1, and the obtained coated pre-physicalized silicon oxide material is obtained.
[0028] Example 5 The difference from Example 1 is that the content of sodium aluminate in the sodium aluminate solution of step (1) is 10.0wt%, and the content of concentrated hydrochloric acid in the hydrochloric acid solution of step (2) is 9.8wt%. The rest is the same as in Example 1, and the obtained coated pre-physicalized silicon oxide material is obtained.
[0029] Example 6 The difference from Example 1 is that step (3) is no longer repeated coating, and the rest is the same as Example 1, and the obtained coated pre-physicalized silicon oxide material.
[0030] A series of relevant performance tests were carried out on the products prepared in the above Examples 1-6, and the results are as follows: 1. XRD test: The modified pre-lithiated silicon-oxygen material obtained in Example 1 was tested using an X-ray powder diffractometer to obtain a diffraction pattern, as shown in FIG. Figure 1 shown.
[0031] from Figure 1 It can be seen that the composite material obtained by the present invention has diffraction peaks of silicon grains and Li 2 SiO 3 The diffraction peaks of the composite material indicate that the composite material contains crystalline silicon and lithium silicate phases.
[0032] 2. Slurry gas production and stability and power-off test: The samples prepared from the samples obtained in Examples 1 to 6 were taken as negative electrode materials, mixed with a conductive agent (Super-P) and a binder LA132 (15wt%) in a mass ratio of 70:20:10, and an appropriate amount of deionized water was added as a dispersant to form a slurry. The slurry was bagged and sealed, and the gas production was measured by the drainage method, that is, (0h drainage - xh drainage) / powder mass.
[0033] The samples prepared in Examples 1 to 6 were used as negative electrode materials and mixed with a conductive agent (Super-P) and a binder LA132 (15wt%) in a mass ratio of 70:20:10 to prepare a slurry, which was coated on a copper foil and dried in a vacuum oven to form a negative electrode sheet. A 1 mol / L LiPF6 electrolyte (the volume ratio of ethylene carbonate and diethyl carbonate in the solvent = 1:1) was used, a polypropylene microporous membrane was used as a separator, and a lithium sheet was used as the negative electrode. A button cell was assembled and the electrochemical performance was tested on a blue battery test system. The constant current charge and discharge was performed at 0.1C, and the voltage range was 0.005V-1.5V.
[0034] The results are shown in the following table:
[0035] The present invention uses a method of repairing coating defects by chemically reacting the surface of the pre-processed silicon oxide material, which is a solution coating operation, and can ensure that the coating material enters the defects of the material. This coating can effectively inhibit the gas production of the powder and reduce the electrode / electrolyte interface impedance. The coating method uses materials that are easy to obtain and have low cost, is suitable for large-scale production, and reduces production costs.
[0036] This method will also produce precipitates in the liquid during production, so the filter paper needs to be replaced frequently, otherwise the filtration efficiency will be affected; the pre-treated silicon-oxygen composite material after alumina repair can further improve the material's conductivity and enhance the rate performance.
[0037] The above shows and describes the basic principles, main features and advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and that the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.
[0038] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a silicon-oxygen composite material coated with aluminum oxide, characterized in that: The following steps are involved: S1, prepare a sodium aluminate solution, immerse the pre-physicalized silica in the sodium aluminate solution, stir for 10 minutes, and filter to obtain a solid 1; S2, prepare a hydrochloric acid solution, immerse the solid 1 in the hydrochloric acid solution, stir for 5 minutes, and filter to obtain a solid 2; S3, repeating the soaking steps of S1 and S2 for 3 to 4 times with solid 2 to obtain solid 3; S4, adding solid 3 into purified water, stirring and washing for 20 min, and filtering to obtain solid 4; S5, placing the solid 4 in a vacuum dryer at 95°C and drying for 6 hours to finally obtain a silicon-oxygen composite material coated with aluminum oxide.
2. The method for preparing a silicon-oxygen composite material coated with aluminum oxide according to claim 1, characterized in that: The sodium aluminate solution is prepared by mixing sodium aluminate with pure water, and the content of sodium aluminate in the sodium aluminate solution is 0.5-10 wt %.
3. The method for preparing a silicon-oxygen composite material coated with aluminum oxide according to claim 1, characterized in that: The pre-physicalized silicon oxide is immersed in a sodium aluminate solution at a material weight ratio of 1:
4.
4. The method for preparing a silicon-oxygen composite material coated with aluminum oxide according to claim 1, characterized in that: The hydrochloric acid solution is prepared by concentrating hydrochloric acid and pure water, and the content of the concentrating hydrochloric acid in the hydrochloric acid solution is 0.49-9.8 wt %.
5. The method for preparing a silicon-oxygen composite material coated with aluminum oxide according to claim 1, characterized in that: The solid 1 is immersed in a hydrochloric acid solution at a material weight ratio of 1:
4.
6. The method for preparing a silicon-oxygen composite material coated with aluminum oxide according to claim 1, characterized in that: During the stirring and washing in step S4, the weight ratio of the solid 3 to the purified water is 1:
10.
7. The silicon-oxygen composite material coated with aluminum oxide obtained by the method according to any one of claims 1 to 6, characterized in that: The composite material is a three-layer core-shell structure, which comprises an inner core, an intermediate layer and an outermost layer; the inner core is a Li-Si-O matrix, the intermediate layer is a carbon layer, and the outermost layer is an Al2O3 coating layer.
Citation Information
Patent Citations
Modified pre-lithiated silicon oxide materials, preparation methods, applications and lithium-ion batteries
CN112820863B
Modified pre-lithiated silica material, preparation method and application thereof and lithium ion battery
CN116314695A
Negative electrode material and preparation method thereof, negative electrode plate and battery
CN116598446A
Method for coating surface of titanium dioxide with compact alumina
CN111100481A
Preparation method of special titanium dioxide for color master batch with high melting filterability
CN114539816A
Cited By
Method for improving pre-lithium silica gas production based on aluminum phosphate modification and secondary carbon coating
CN119160923A
High-stability sodium titanate negative electrode material and preparation method and application thereof
CN120637459A
High-stability sodium titanate negative electrode material and preparation method and application thereof
CN120637459B