Method for efficiently producing sodium pyroantimonate

By adopting the methods of pulping, oxidation synthesis, filtration washing and air flow drying in the production process of sodium pyroantimonate, and using catalysts to improve the Sb(III) conversion rate and reduce hydrogen peroxide consumption, the Sb(III) conversion rate in the existing technology is solved. The problem of low and high hydrogen peroxide consumption has been achieved, and efficient and automated production of sodium pyroantimonate has been achieved, reducing costs and improving product quality.

CN118791040APending Publication Date: 2024-10-18GUANGXI WANSHIZHI RARE & PRECIOUS METAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410791122.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In the process of producing sodium pyroantimonate in the existing technology, the conversion rate of Sb(III) is low, the consumption of hydrogen peroxide is large, the product quality is poor, the production efficiency is low, and the process is not automated, resulting in high costs and unstable product quality.

Method used

A method including pulping, oxidation synthesis, filtration washing and air flow drying is adopted. Antimony trioxide and NaOH solution are added to the reaction kettle, and then hydrogen peroxide is added to perform the oxidation reaction. The catalyst is used to increase the Sb(III) conversion rate, and High-quality sodium pyroantimonate is prepared through an airflow dryer to achieve automation and integration of the process.

Benefits of technology

The conversion rate of Sb(III) is improved, the consumption of hydrogen peroxide is reduced, the product quality of sodium pyroantimonate is improved, the automation of the process and batch industrial production are realized, the production cost is reduced, and the product quality meets professional standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791040A_ABST
    Figure CN118791040A_ABST
Patent Text Reader

Abstract

The invention discloses a method for efficiently producing sodium pyroantimonate, which comprises the following steps: pumping antimony trioxide into a closed slurrying tank from a stock bin through a pneumatic conveying pump, adding a NaOH solution, slurrying, mixing with a catalyst, and pumping into a reaction kettle through a pump; pumping hydrogen peroxide into the slurry, and continuously stirring and reacting in the reaction kettle to generate a sodium antimonate solution; the sodium antimonate solution is subjected to solid-liquid separation through a centrifugal machine, a solid product is washed with water in the centrifugal machine, wet sodium antimonate is obtained after washing, and mother liquor is recycled; and drying the wet sodium antimonate by adopting an air flow dryer, separating, settling and hermetically screening to obtain a sodium pyroantimonate product. The catalyst is added, so that the Sb (III) conversion rate can be increased, the consumption of hydrogen peroxide can be reduced, the production method provided by the invention can realize process automation and integrated batch industrial production, can realize production under normal pressure and lower temperature conditions, and greatly reduces the cost and saves the energy consumption while ensuring the product quality of the sodium pyroantimonate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a heavy metal metallurgical process in the field of nonferrous metallurgy, and in particular to a method for efficiently producing sodium pyroantimonate. Background Art

[0002] Antimony is a silvery-white metal with brittleness, poor electrical and thermal conductivity. It is mainly used in alloys, military industry, flame retardants and glass industries. my country is the country with the largest antimony production in the world, accounting for more than 80% of the world's antimony production. my country has irreplaceable advantages in antimony resources and production. The mineral raw materials for antimony smelting mainly include stibnite, antimony gold ore and brittle sulfur lead antimony ore. Antimony soot is a by-product of heavy metal smelting and an important secondary raw material for recovering antimony. The main products of antimony are metal antimony ingots, antimony white and sodium antimonite pyrochlore. Among them, sodium antimonite pyrochlore is mainly used as a clarifier and decolorizer for industrial glass. The glass products made from it have the advantages of high transparency, no discoloration under light, and low toxicity. They are widely used in TV picture tubes, high-grade glass, enamel industry, electronic industry semiconductors and other fields. It accounts for a high proportion of antimony products and is a fine chemical product with broad economic prospects.

[0003] The sodium nitrate oxidation method is a traditional method for preparing sodium antimonate by using metallic antimony or antimony trioxide as raw materials and oxidizing with sodium nitrate under high temperature alkaline conditions. First, metallic antimony is mixed with an excess of sodium nitrate, and then roasted at high temperature in a rotary kiln to oxidize the antimony to pentavalent. Finally, the sodium nitrate is washed with water to remove the sodium nitrate, and then dried and crushed to produce the sodium pyroantimonate product. The sodium nitrate oxidation method has the advantages of simple process, short flow and easy operation, but it cannot effectively remove impurities during the production process, and the waste gas in the production process cannot be completely eliminated. The product quality is low and has been eliminated.

[0004] The chlorination method is to oxidize and leach the antimony-containing raw materials with chlorine in a hydrochloric acid system, and then neutralize and hydrolyze the leachate with sodium hydroxide to produce sodium pyroantimonate precipitate, which is then washed and dried to obtain the sodium pyroantimonate product. The chlorination method has the advantages of low raw material requirements and good product quality, but it has the disadvantages of long process flow, severe equipment corrosion and large amount of wastewater.

[0005] The potassium salt method is based on the fact that potassium pyroantimonate has a high solubility in aqueous solution, while sodium pyroantimonate is almost insoluble in water. First, Sb(III) is oxidized to Sb(V) and dissolved in a potassium hydroxide system using hydrogen peroxide. After liquid-solid separation, the solution reacts with sodium hydroxide to produce sodium pyroantimonate. The main advantage of the potassium salt method is that the sodium pyroantimonate product has good quality, but the disadvantage is that the potassium salt inclusion loss in the intermediate product is serious, resulting in excessively high production costs.

[0006] A more commonly used and convenient method is the direct oxidation method, which is a method for preparing sodium antimonate in one step by directly oxidizing antimony trioxide with hydrogen peroxide in a sodium hydroxide solution. In this method, antimony trioxide, sodium hydroxide and hydrogen peroxide are added to a reactor in proportion, and when the slurry is heated to a certain temperature, a hydrogen peroxide solution is added dropwise for oxidation reaction, and the reaction product is washed with water and dried to obtain a sodium antimonate product. The oxidation reflux method has the advantages of simple process, short flow and easy operation, but has the disadvantages of low Sb(III) conversion rate in the product, large hydrogen peroxide consumption, poor product quality and low production efficiency. Therefore, it is necessary to invent an industrial method that can improve the Sb(III) conversion rate, reduce the hydrogen peroxide consumption, and realize process automation and integration for efficient production of sodium antimonate. Summary of the invention

[0007] In view of the above shortcomings, the present invention provides a method for efficiently producing sodium pyroantimonate, which can improve the Sb(III) conversion rate, reduce the consumption of hydrogen peroxide, improve the product quality of sodium pyroantimonate, realize process automation, integrated batch industrial production, and significantly reduce costs. The specific technical scheme is as follows:

[0008] A method for efficiently producing sodium pyroantimonate comprises the following steps:

[0009] (1) Pulping

[0010] Antimony trioxide is stored in a silo, and pumped from the silo into a closed slurry tank by a pneumatic conveying pump, and NaOH solution is added, and the temperature is raised to 60-80°C with stirring, and stirring is continued for 10-30 minutes. After slurrying, it is mixed with the catalyst and pumped into the reactor;

[0011] The silo is manually charged, and a small amount of dust is generated during the process, which is discharged in an unorganized form;

[0012] (2) Oxidative synthesis

[0013] The oxidation process is carried out in a reactor, and hydrogen peroxide is pumped into the slurry after slurrying in step (1) at a pumping rate of 1.0-10.0 kg / min. The reactor is continuously stirred to react and generate a sodium antimonate solution. The reaction principle is:

[0014] Sb2O3+2NaOH+2H2O2+3H2O=2NaSbO3·3H2O

[0015] The reaction heat in the reactor is removed by indirect cooling with cooling water. As the reaction is gradually completed, the temperature in the reactor gradually decreases, and sodium antimonate precipitates rapidly.

[0016] (3) Filtration and washing

[0017] The sodium antimonate slurry is separated into solid and liquid by a centrifuge to obtain a solid product and a separation mother liquor, wherein the separation mother liquor is returned for utilization, and the solid product is washed with water in the centrifuge to obtain wet sodium antimonate and a washing liquid after washing; the washing liquid is collected and sent to an evaporator for heating, evaporation and concentration to obtain antimony slag and a concentrated mother liquor, and the antimony slag is treated in a side-blowing reduction refining furnace;

[0018] (4) Airflow drying

[0019] The wet sodium antimonate is dried by an air flow dryer. The wet sodium antimonate is fed into the lower part of the air flow tube by a screw feeder, and the air is fed into the preheater by a blower and heated to 80-90°C (the heat source is the power supply) and then blown into the air flow tube. The blowing air velocity in the tube is 10-20m / s, and the velocity in the tube depends on the size and density of the wet particles; the dried particles enter the cyclone separator for separation and sedimentation, and the dry materials are discharged through the discharge drum after sedimentation, and the waste gas is discharged through the upper end of the bag filter exhaust pipe; the dried sodium antimonate is closed screened, and the fine sodium antimonate is collected, and the large-particle coarse sodium antimonate is ground. The waste gas generated by screening and grinding is treated by a bag filter and discharged from the DA009 exhaust pipe, and the particles on the bag filter are collected and combined with the ground sodium antimonate and fine sodium antimonate to obtain the sodium pyroantimonate product.

[0020] Preferably, the catalyst comprises the following raw materials in parts by mass: 5-8 parts of quaternary ammonium salt solution, 1-1.5 parts of titanium chloride or bromide, and 2-4 parts of metal vanadate solution.

[0021] Preferably, the metal vanadate is orthometallic vanadate AVO3, where A comprises one of Ca, Sr, Ba and La.

[0022] Preferably, the preparation method of the catalyst is as follows:

[0023] (1) preparing a quaternary ammonium salt solution with a mass fraction of 10-20%, adding titanium chloride or bromide, and stirring evenly;

[0024] (2) adding a 20-30% by mass metal vanadate solution to the solution obtained in step (1), heating to 35-50° C., and stirring for 30-60 min;

[0025] (3) concentrating the solution in step (2) under reduced pressure and drying to obtain a catalyst;

[0026] Preferably, the usage amount of the catalyst is 1-5% of the mass of antimony trioxide.

[0027] Preferably, the solid-liquid ratio of the antimony trioxide to the NaOH solution is 1:20-30; the solid-liquid ratio of the antimony trioxide to the hydrogen peroxide is 1:5-15.

[0028] Preferably, the oxidation process is carried out at 30-40°C and normal pressure, and the reaction time is 60-120 minutes.

[0029] Preferably, the concentrated mother liquor produced in step (3) of the method for producing sodium pyroantimonate is evaporated using a triple-effect evaporator to remove excess water, the evaporated concentrated mother liquor is returned to the reactor for reuse, and the condensed water is reused for washing the solid product; the design scale of the evaporator is 2 t / h, the heat source is provided by steam from an electric steam generator, and the antimony slag produced during the evaporation process is returned to the side-blown reduction refining furnace for treatment.

[0030] Preferably, the pH value of the reaction solution in step (2) of the method for producing sodium pyroantimonate is between 11 and 13.

[0031] Preferably, the mass fraction of the NaOH solution is 25-35%, and the mass fraction of the hydrogen peroxide solution is 35-45%.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The invention provides a method for efficiently producing sodium pyroantimonate, which is suitable for the industrial production of sodium pyroantimonate, can improve the Sb(III) conversion rate, reduce the consumption of hydrogen peroxide, and improve the product quality of sodium pyroantimonate. The method can realize process automation and integrated batch production. The pulping, oxidation synthesis, washing and filtering, and airflow drying processes are smoothly connected, and the equipment is divided into work and cooperates, and can be operated at the same time to efficiently produce high-quality sodium pyroantimonate. The cost is greatly reduced while the product quality of sodium pyroantimonate is guaranteed. The product quality of sodium pyroantimonate meets the first-level standard of professional standard ZBG12019-89.

[0034] The catalyst prepared by the invention catalyzes the oxidation of hydrogen peroxide, reduces the consumption of hydrogen peroxide, promotes the conversion of Sb(III), reduces the amount of hydrogen peroxide used and improves the antimony conversion rate. If the amount of hydrogen peroxide used is too small, the conversion rate of trivalent antimony will be low, affecting the quality of the final product. If the amount of hydrogen peroxide used is too large, the processing cost will be wasted. Under the action of the catalyst, the invention can realize the reaction at 30-40 DEG C and normal pressure. The reaction temperature has a great influence on the reaction. If the reaction temperature is too low, the particles of the product are fine and it is difficult to wash and filter. If the reaction temperature is too high, the product structure changes and it is not easy to react with the alkali solution, affecting the product quality. However, the invention can ensure the antimony conversion rate and the high quality of the product at a relatively low temperature and normal pressure, saving energy consumption and cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below.

[0036] Figure 1The process flow and pollution node diagram of the sodium antimonate production system of the present invention;

[0037] Figure 2 It is a process flow chart of the air flow dryer of the present invention. DETAILED DESCRIPTION

[0038] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.

[0039] Example 1

[0040] Combination Figure 1 The method for efficiently producing sodium pyroantimonate of this embodiment comprises the following steps:

[0041] (1) Preparation of Catalyst

[0042] Prepare a quaternary ammonium salt solution with a mass fraction of 10%, add titanium tetrabromide, stir evenly, then add a potassium vanadate solution with a mass fraction of 20%, heat to 35°C, stir for 30 minutes; concentrate under reduced pressure, and dry to obtain a catalyst;

[0043] The mass ratio of the quaternary ammonium salt solution to the titanium tetrabromide and potassium vanadate solution is 5:1:2;

[0044] (2) Pulping

[0045] Antimony trioxide is placed in a silo by artificial feeding, and is pumped from the silo into a closed slurry tank by a pneumatic conveying pump, and a NaOH solution with a mass fraction of 25% is added, and the temperature is raised to 60°C with stirring, and the stirring is continued for 10 minutes. After slurrying, it is mixed with a catalyst and pumped into a reactor; the amount of the catalyst used is 1% of the mass of antimony trioxide; the solid-liquid ratio of the antimony trioxide to the NaOH solution is 1:20; the solid-liquid ratio of the antimony trioxide to the hydrogen peroxide is 1:5;

[0046] (3) Oxidative synthesis

[0047] The oxidation process is carried out in a reactor at room temperature and pressure. A hydrogen peroxide solution with a mass fraction of 35% is pumped into the slurry after slurrying in step (2) at a pumping rate of 1.0 kg / min. The reactor is continuously stirred for reaction. The reaction time is 60 minutes. The reaction heat in the reactor is removed by indirect cooling with cooling water. As the reaction is gradually completed, the temperature in the reactor gradually decreases, sodium antimonate is precipitated, and a sodium antimonate solution is generated.

[0048] (4) Filtration and washing

[0049] The sodium antimonate slurry is separated into solid and liquid by a centrifuge to obtain a solid product and a separation mother liquor, wherein the separation mother liquor is returned for utilization, and the solid product is washed with water in the centrifuge to obtain wet sodium antimonate and a washing liquid after washing; the washing liquid is collected and sent to an evaporator for heating, evaporation and concentration to obtain antimony slag and a concentrated mother liquor, and the antimony slag is treated in a side-blowing reduction refining furnace;

[0050] (5) Airflow drying

[0051] The wet sodium antimonate is dried using an air flow dryer. Figure 2 The wet sodium antimonate is fed into the lower part of the air flow pipe by a screw feeder, and the air is fed into the preheater by a blower and heated to 80°C before being blown into the air flow pipe. The blowing velocity in the pipe is 10m / s; the dried particles enter the cyclone separator for separation and sedimentation, and the dry materials are discharged through the discharge drum after sedimentation, and the waste gas is discharged through the upper end of the bag filter exhaust pipe; the dried sodium antimonate is closed screened to collect the fine sodium antimonate, and the coarse sodium antimonate with large particle size is ground. The waste gas generated by screening and grinding is treated by a bag dust collector and then discharged from the DA009 exhaust pipe. The particles on the bag dust collector are collected and combined with the ground sodium antimonate and fine sodium antimonate to obtain the sodium antimonate pyrochlore product.

[0052] In this embodiment, the concentrated mother liquor produced in step (4) is evaporated using a triple-effect evaporator to remove excess water. The evaporated concentrated mother liquor is returned to the reactor for reuse, and the condensed water is reused for washing the solid product. The design scale of the evaporator is 2 t / h, and the heat source is provided by the steam of the electric steam generator. The antimony slag produced during the evaporation process is returned to the side-blown reduction refining furnace for treatment.

[0053] The pH value of the reaction solution in step (3) of this embodiment is 11.

[0054] Example 2

[0055] Combination Figure 1 The method for efficiently producing sodium pyroantimonate of this embodiment comprises the following steps:

[0056] (1) Preparation of Catalyst

[0057] Prepare a quaternary ammonium salt solution with a mass fraction of 20%, add titanium tetrachloride, stir evenly, then add a strontium vanadate solution with a mass fraction of 30%, heat to 50°C, stir for 60 minutes; concentrate under reduced pressure, and dry to obtain a catalyst;

[0058] The mass ratio of the quaternary ammonium salt solution to the titanium tetrachloride and strontium vanadate solution is 8:1.5:4;

[0059] (2) Pulping

[0060] Antimony trioxide is placed in a silo by artificial feeding, and is pumped from the silo into a closed slurry tank by a pneumatic conveying pump, and a NaOH solution with a mass fraction of 35% is added, and the temperature is raised to 80°C with stirring, and the stirring is continued for 30 minutes. After slurrying, it is mixed with a catalyst and pumped into a reactor; the amount of the catalyst used is 5% of the mass of antimony trioxide; the solid-liquid ratio of the antimony trioxide to the NaOH solution is 1:30; the solid-liquid ratio of the antimony trioxide to the hydrogen peroxide is 1:15;

[0061] (3) Oxidative synthesis

[0062] The oxidation process is carried out in a reactor at room temperature and pressure. Hydrogen peroxide with a mass fraction of 45% is pumped into the slurry after slurrying in step (2) at a pumping rate of 10.0 kg / min. The reactor is continuously stirred for reaction. The reaction time is 120 min. The reaction heat in the reactor is removed by indirect cooling with cooling water. As the reaction is gradually completed, the temperature in the reactor gradually decreases, sodium antimonate is precipitated, and a sodium antimonate solution is generated.

[0063] (4) Filtration and washing

[0064] The sodium antimonate slurry is separated into solid and liquid by a centrifuge to obtain a solid product and a separation mother liquor, wherein the separation mother liquor is returned for utilization, and the solid product is washed with water in the centrifuge to obtain wet sodium antimonate and a washing liquid after washing; the washing liquid is collected and sent to an evaporator for heating, evaporation and concentration to obtain antimony slag and a concentrated mother liquor, and the antimony slag is treated in a side-blowing reduction refining furnace;

[0065] (5) Airflow drying

[0066] The wet sodium antimonate is dried using an air flow dryer. Figure 2 The wet sodium antimonate is fed into the lower part of the air flow pipe through a screw feeder, and the air is fed into the preheater by a blower and heated to 90°C before being blown into the air flow pipe. The blowing velocity in the pipe is 20m / s; the dried particles enter the cyclone separator for separation and sedimentation, and the dry material is discharged through the unloading drum after sedimentation, and the waste gas is discharged through the upper end of the bag filter exhaust pipe; the dried sodium antimonate is closed screened to collect the fine sodium antimonate, and the coarse sodium antimonate with large particle size is ground. The waste gas generated by screening and grinding is treated by a bag dust collector and then discharged from the DA009 exhaust pipe. The particles on the bag dust collector are collected and combined with the ground sodium antimonate and fine sodium antimonate to obtain the sodium antimonate pyrochlore product.

[0067] In this embodiment, the concentrated mother liquor produced in step (4) is evaporated using a triple-effect evaporator to remove excess water. The evaporated concentrated mother liquor is returned to the reactor for reuse, and the condensed water is reused for washing the solid product. The design scale of the evaporator is 2 t / h, and the heat source is provided by steam from an electric steam generator. The antimony slag produced during the evaporation process is returned to the side-blown reduction refining furnace for treatment.

[0068] The pH value of the reaction solution in step (3) of this embodiment is 13.

[0069] Example 3

[0070] Combination Figure 1 The method for efficiently producing sodium pyroantimonate of this embodiment comprises the following steps:

[0071] (1) Preparation of Catalyst

[0072] Prepare a quaternary ammonium salt solution with a mass fraction of 15%, add titanium tetrabromide, stir evenly, then add a 25% barium vanadate solution with a mass fraction, heat to 42°C, stir for 45 minutes; concentrate under reduced pressure, and dry to obtain a catalyst;

[0073] The mass ratio of the quaternary ammonium salt solution to the titanium tetrabromide and barium vanadate solution is 6:1.2:3;

[0074] (2) Pulping

[0075] Antimony trioxide is placed in a silo by artificial feeding, and is pumped from the silo into a closed slurry tank by a pneumatic conveying pump, and a NaOH solution with a mass fraction of 30% is added, and the temperature is raised to 70°C with stirring, and the stirring is continued for 20 minutes. After slurrying, it is mixed with a catalyst and pumped into a reactor; the amount of the catalyst used is 3% of the mass of antimony trioxide; the solid-liquid ratio of the antimony trioxide to the NaOH solution is 1:25; the solid-liquid ratio of the antimony trioxide to the hydrogen peroxide is 1:10;

[0076] (3) Oxidative synthesis

[0077] The oxidation process is carried out in a reactor at room temperature and pressure. A hydrogen peroxide solution with a mass fraction of 40% is pumped into the slurry after slurrying in step (2) at a pumping rate of 5.0 kg / min. The reactor is continuously stirred for reaction. The reaction time is 90 min. The reaction heat in the reactor is removed by indirect cooling with cooling water. As the reaction is gradually completed, the temperature in the reactor gradually decreases, sodium antimonate is precipitated, and a sodium antimonate solution is generated.

[0078] (4) Filtration and washing

[0079] The sodium antimonate slurry is separated into solid and liquid by a centrifuge to obtain a solid product and a separation mother liquor, wherein the separation mother liquor is returned for utilization, and the solid product is washed with water in the centrifuge to obtain wet sodium antimonate and a washing liquid after washing; the washing liquid is collected and sent to an evaporator for heating, evaporation and concentration to obtain antimony slag and a concentrated mother liquor, and the antimony slag is treated in a side-blowing reduction refining furnace;

[0080] (5) Airflow drying

[0081] The wet sodium antimonate is dried using an air flow dryer. Figure 2The wet sodium antimonate is fed into the lower part of the air flow pipe by a screw feeder, and the air is fed into the preheater by a blower and heated to 85°C before being blown into the air flow pipe. The blowing velocity in the pipe is 15m / s; the dried particles enter the cyclone separator for separation and sedimentation, and the dry material is discharged through the unloading drum after sedimentation, and the waste gas is discharged through the upper end of the bag filter exhaust pipe; the dried sodium antimonate is closed screened to collect the fine sodium antimonate, and the coarse sodium antimonate with large particle size is ground. The waste gas generated by screening and grinding is treated by a bag dust collector and then discharged from the DA009 exhaust pipe. The particles on the bag dust collector are collected and combined with the ground sodium antimonate and fine sodium antimonate to obtain the sodium antimonate pyrochlore product.

[0082] In this embodiment, the concentrated mother liquor produced in step (3) is evaporated using a triple-effect evaporator to remove excess water. The evaporated concentrated mother liquor is returned to the reactor for reuse, and the condensed water is reused for washing the solid product. The design scale of the evaporator is 2 t / h, and the heat source is provided by steam from an electric steam generator. The antimony slag produced during the evaporation process is returned to the side-blown reduction refining furnace for treatment.

[0083] The pH value of the reaction solution in step (3) of this embodiment is 12.

[0084] Comparative Example 1

[0085] The difference from Example 3 is that no catalyst was added.

[0086] Comparative Example 2

[0087] The difference from Example 3 is that the catalyst is antimony pentachloride.

[0088] Comparative Example 3

[0089] The difference from Example 3 is that the preparation method of the catalyst is different, as follows:

[0090] Prepare a quaternary ammonium salt solution with a mass fraction of 15%, add barium sulfate, stir evenly, then add a 35% barium vanadate solution with a mass fraction, and stir at room temperature for 45 minutes; concentrate under reduced pressure, and dry to obtain a catalyst; the mass ratio of the quaternary ammonium salt solution to the barium sulfate and barium vanadate solutions is 3:1:2.5.

[0091] Comparative Example 4

[0092] The difference from Example 3 is that the preparation method of sodium pyroantimonate is different, as follows:

[0093] Prepare a sodium hydroxide solution with a mass fraction of 30% and a temperature of 65°C, add sodium pyroantimonate seeds in an amount of 20.0 kg / m 3, antimony oxide and 28% by mass hydrogen peroxide were added respectively, the adding speed of antimony oxide was controlled to be 10.0 kg / min, and the adding speed of hydrogen peroxide was controlled to be 10.0 kg / min. After all the materials were added, the reaction was continued for 90 minutes. Vacuum filtration was used for liquid-solid separation, and the solid product was dried to obtain sodium pyroantimonate product.

[0094] The products obtained in Examples 1-3 and Comparative Examples 1-4 were subjected to quality inspection, and the inspection results are shown in Table 1.

[0095] Table 1

[0096]

[0097] It can be seen from Table 1 that the component content of the sodium pyroantimonate product obtained in Examples 1-3 meets the first-class specifications of the professional standard ZBG12019-89 for the quality of sodium pyroantimonate products, the antimony conversion rate is improved, and the small content of trivalent antimony indicates that the conversion rate of trivalent antimony is very high, and the product quality is better. The catalyst of the present invention catalyzes the oxidation of hydrogen peroxide, reduces the consumption of hydrogen peroxide, and can also react at normal temperature and pressure to save resources; the method of the present invention is suitable for the industrial production of sodium pyroantimonate, can realize process automation and integrated batch production, pulping, oxidation synthesis, washing and filtering, and airflow drying processes are smoothly connected, and each equipment cooperates in division of labor, can operate simultaneously and efficiently produce high-quality sodium pyroantimonate, and greatly reduce costs while ensuring the product quality of sodium pyroantimonate.

[0098] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A method for efficiently producing sodium pyroantimonate, characterized in that: The method comprises the following steps: (1) Pulping Antimony trioxide is stored in a silo, and pumped from the silo into a closed slurry tank by a pneumatic conveying pump, and NaOH solution is added, and the temperature is raised to 60-80°C with stirring, and stirring is continued for 10-30 minutes. After slurrying, it is mixed with the catalyst and pumped into the reactor; (2) Oxidative synthesis The oxidation process is carried out in a reactor, and hydrogen peroxide is pumped into the slurry after slurrying in step (1) at a pumping rate of 1.0-10.0 kg / min. The reactor is continuously stirred to react and generate a sodium antimonate solution; (3) Filtration and washing The sodium antimonate slurry is separated into solid and liquid by a centrifuge to obtain a solid product and a separation mother liquor, wherein the separation mother liquor is returned for utilization, and the solid product is washed with water in the centrifuge to obtain wet sodium antimonate and a washing liquid after washing; the washing liquid is collected and sent to an evaporator for heating, evaporation and concentration to obtain antimony slag and a concentrated mother liquor, and the antimony slag is treated in a side-blowing reduction refining furnace; (4) Airflow drying The wet sodium antimonate is dried by an air flow dryer. The wet sodium antimonate is fed into the lower part of the air flow pipe through a screw feeder. The air is fed into the preheater by a blower and heated to 80-90°C before being blown into the air flow pipe. The blowing air velocity in the pipe is 10-20 m / s. The dried particles enter the cyclone separator for separation and sedimentation. The dry material is discharged through a discharge drum after sedimentation. The waste gas is discharged through the upper end of the bag filter exhaust pipe. The dried sodium antimonate is sieved in a closed manner to collect the fine sodium antimonate. The coarse sodium antimonate with a large particle size is ground. The waste gas generated by screening and grinding is treated by a bag dust collector and then discharged from an exhaust pipe. The particles on the bag dust collector are collected and combined with the ground sodium antimonate and fine sodium antimonate to obtain a sodium pyroantimonate product. The catalyst comprises the following raw materials in parts by weight: 5-8 parts of quaternary ammonium salt solution, 1-1.5 parts of titanium chloride or bromide, and 2-4 parts of metal vanadate solution.

2. The method for efficiently producing sodium pyroantimonate according to claim 1, characterized in that: The metal vanadate is orthometallic vanadate AVO3, wherein A includes one of Ca, Sr, Ba and La.

3. The method for efficiently producing sodium pyroantimonate according to claim 1, characterized in that: The preparation method of the catalyst is as follows: (1) preparing a quaternary ammonium salt solution with a mass fraction of 10-20%, adding titanium chloride or bromide, and stirring evenly; (2) adding a 20-30% by mass metal vanadate solution to the solution obtained in step (1), heating to 35-50° C., and stirring for 30-60 min; (3) Concentrating the solution in step (2) under reduced pressure and drying to obtain a catalyst.

4. The method for efficiently producing sodium pyroantimonate according to claim 1, characterized in that: The usage amount of the catalyst is 1-5% of the mass of antimony trioxide.

5. The method for efficiently producing sodium pyroantimonate according to claim 1, characterized in that: The solid-liquid ratio of the antimony trioxide to the NaOH solution is 1:20-30; the solid-liquid ratio of the antimony trioxide to the hydrogen peroxide is 1:5-15.

6. The method for efficiently producing sodium pyroantimonate according to claim 1, characterized in that: The oxidation process is carried out at 30-40°C and normal pressure, and the reaction time is 60-120 minutes.

7. The method for efficiently producing sodium pyroantimonate according to claim 1, characterized in that: The concentrated mother liquor produced in step (3) is evaporated using a triple-effect evaporator to remove excess water, and the evaporated concentrated mother liquor is returned to the reactor for reuse, and the condensed water is reused for washing the solid product.

8. The method for efficiently producing sodium pyroantimonate according to claim 7, characterized in that: The design scale of the evaporator is 2t / h. The heat source is provided by the steam of the electric steam generator. The antimony slag produced during the evaporation process is returned to the side-blowing reduction refining furnace for treatment.

9. The method according to claim 1, characterized in that: The pH value of the reaction solution in step (2) is between 11 and 13.

10. The method according to claim 1, characterized in that: The mass fraction of the NaOH solution is 25-35%, and the mass fraction of the hydrogen peroxide solution is 35-45%.