Preparation method of dielectric-adjustable high-temperature-resistant thermal-insulation stealth integrated material

By using stirring method and gradient molding technology in alumina nanopowder and chopped carbon fiber composite aerogel, a two-level network structure is constructed, which solves the problems of existing high-temperature absorbing materials in terms of high temperature resistance, lightweight, heat insulation, and stealth. Insufficient, the dielectric constant is adjustable and the thermal insulation performance is improved, forming a high temperature resistant, lightweight and low-cost aerogel material.

CN118791283APending Publication Date: 2024-10-18CRUISE (SUZHOU) NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410852241.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing high-temperature absorbing materials have shortcomings in multi-functional coupling such as high temperature resistance, lightweight, heat insulation, and stealth. In particular, they are incompatible with heat insulation and broadband stealth functions at high temperatures, and traditional coated absorbing materials increase the weight of the aircraft. And problems such as cracking and peeling are prone to occur under high temperature thermal stress.

Method used

By using the stirring method in the composite aerogel of alumina nanopowder and chopped carbon fiber to achieve uniform dispersion of carbon fiber, combined with gradient molding and solvent replacement technology, a two-level network structure is constructed to achieve adjustability of dielectric constant and thermal insulation. The performance is improved to form a lightweight and high-temperature resistant aerogel material.

Benefits of technology

The prepared airgel material has a heat-resistant temperature of up to 1200°C in an oxygen-free and oxygen-poor environment, has a wide range of dielectric constants, moderate thermal conductivity, low density, simple process and low cost, which solves the problem of traditional materials at high temperatures. Insufficient performance and increased weight issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791283A_ABST
    Figure CN118791283A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a dielectric-adjustable high-temperature-resistant thermal-insulation stealth integrated material, which comprises the following steps: introducing different contents of short carbon fibers into an alumina precursor dispersion liquid by adopting a stirring method, preparing different contents of carbon fiber / alumina nanowire clusters by adopting a hydrothermal method, and then carrying out compression molding to obtain the dielectric-adjustable high-temperature-resistant thermal-insulation stealth integrated material. Carrying out solvent replacement on the formed block; and finally, carrying out supercritical drying and heat treatment in an inert atmosphere. According to the preparation method disclosed by the invention, the aluminum oxide nanowires with high length-diameter ratio are subjected to three-dimensional lap joint to construct an aluminum oxide nanowire network structure with uniformly distributed carbon fibers, and the density of the aerogel is controlled through compression molding, so that the preparation of the integrated aerogel with low cost, adjustable dielectric constant, light weight, efficient heat insulation and stealth is realized. According to the invention, uniformly distributed carbon fibers are introduced into the self-supporting nanowire skeleton to form a conductive network path, and the self-supporting nanowire has the characteristics of high temperature resistance, light weight, large-range adjustable dielectric constant, integration of heat insulation and stealth and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aerogel preparation, and in particular to a method for preparing a dielectrically adjustable high-temperature resistant, heat-insulating and stealthy integrated material. Background Art

[0002] The demand for multifunctional integrated materials with high temperature resistance, heat insulation, stealth and light weight for new aerospace vehicles is becoming increasingly urgent. For example, the tail nozzles and nose cones of airborne weapons such as fighter jets and cruise missiles, as well as the engine air intakes and nozzles, can reach an operating temperature of 700°C or even 1000°C. Traditional magnetic, polymer-based, and carbon-based stealth materials show good electromagnetic wave absorption performance at room temperature, but have various limitations at high temperatures. First, the application of polymers in electromagnetic wave absorption at high temperatures is limited due to their relatively low melting point / softening / decomposition temperature (<300°C); secondly, magnetic loss-type materials lose their advantages when the use temperature exceeds the Curie point, and cannot meet the above-mentioned application requirements such as high temperature resistance, light weight, and wide absorption bandwidth. Carbon-based stealth materials are prone to oxidation and stealth performance failure in an oxygen environment without coating protection. Therefore, dielectric loss-type high-temperature resistant ceramic materials are considered to be a potential high-temperature absorbing material. Existing high-temperature absorbing materials have shortcomings such as low tolerance temperature, high density, narrow absorption bandwidth, and high thermal conductivity, which limit their wider application. Therefore, the development of multifunctional coupling materials that are resistant to high temperatures, lightweight, heat-insulating, and stealthy is urgent.

[0003] Aerogel material is a gel material whose dispersion medium is gas. It is a nanoporous solid material with a network structure composed of colloidal particles or polymer molecules. The size of the pores in the material is in the nanometer order of magnitude. Its porosity is as high as 80-99.8%, the typical size of the pores is 1-100nm, and the specific surface area is 200-1000m 2 / g, and the density can be as low as 3kg / m 3 , the room temperature thermal conductivity can be as low as 0.012W / m·K. It is precisely because of these characteristics that aerogel materials have broad application potential in thermal, acoustic, optics, microelectronics, and particle detection. At present, due to the unique nanostructure of aerogels, which can effectively reduce convection conduction and solid-phase conduction, the most widely used field of aerogels is still the field of thermal insulation. Adding absorbers to aerogel materials is an effective way to achieve dielectrically adjustable broadband electromagnetic stealth and thermal insulation integration. However, existing thermal insulation stealth materials cannot well integrate thermal insulation and broadband stealth functions at high temperatures, and have shortcomings such as low tolerance temperature, small dielectric constant adjustment range, and narrow effective absorption band.

[0004] Chinese patent CN 115627119 A discloses a lightweight, heat-resistant, thermal-insulating stealth coating, a coating and a preparation method thereof. The method prepares a lightweight, closed-cell, wave-absorbing and thermal-insulating filler and mixes it with a coating base material composed of a matrix film-forming material, a reinforcing filler, hollow microspheres, and chopped carbon fibers, and solidifies it to obtain a lightweight, heat-resistant, thermal-insulating stealth coating. The coating prepared using the coating has a lower comprehensive density and thermal conductivity, improves the high-frequency broadband absorption characteristics of the coating, and can be used as a heat-resistant, heat-insulating stealth material for aircraft. However, the maximum temperature that the thermal-insulating stealth coating in the patent can withstand does not exceed 500°C, which cannot meet the more stringent temperature and environmental requirements of new aerospace aircraft. In addition, the wave-absorbing material in the form of a coating will more or less increase the weight of the aircraft, allowing a limited design thickness, and the wave-absorbing coating is prone to cracking and peeling under high-temperature thermal stress. Compared with traditional coating stealth materials, structured stealth materials have a larger structural space, a more flexible structural form, and adjustable electromagnetic wave transmission characteristics. They can not only increase the wave-absorbing effect and bandwidth, but also withstand various complex flight environments. The patent of the present invention can make up for the shortcomings of the above patents. The prepared aerogel can withstand temperatures of up to 1200°C in oxygen-free and oxygen-deficient environments, and can also achieve integrated molding and molding of complex structural components.

[0005] Carbon fiber is a high-performance material that not only has good mechanical properties such as high strength and high modulus, but also has extremely high thermal stability in a non-oxidizing environment. It can remain stable at high temperatures exceeding 2000°C without decomposition or melting. In air, the temperature resistance of carbon fiber is usually between 400°C and 500°C. In addition, carbon fiber exhibits good electrical conductivity and can therefore be used as a conductive filler in a wave-transmitting matrix to adjust the electrical conductivity and dielectric properties of the composite material. However, how to evenly distribute carbon fibers in aerogel materials is still a difficult point.

[0006] The method for dispersing carbon fibers in Chinese patent CN 115231897 A requires the addition of surfactants, and uses both ultrasound and stirring, but the maintenance time after uniform dispersion is short, only 10 to 50 minutes, and the temperature, pH value, time control and other conditions required for uniform dispersion are strict. In addition, the methods for dispersing carbon fibers in Chinese patents CN 116063061 A and CN 113860848 A both require surface treatment or modification of carbon fibers, such as desizing carbon fibers, nitric acid oxidation treatment, and surface modification grafting treatment with silane coupling agents KH-550 and KH-560 to obtain modified carbon fibers, which is cumbersome and complex, with high cost and long time cycle. In addition, the modified carbon fibers may be damaged, and surface defects and structural changes may occur, resulting in a decrease in their strength and electrical conductivity, which limits their wider application as a conductive phase dispersed in aerogels to adjust their dielectric and mechanical properties. The patent of the present invention can make up for the shortcomings of the above patents, and achieve long-term uniform and stable dispersion of carbon fibers through a simple stirring method, and successfully prepare a composite aerogel in which carbon fibers are uniformly distributed in an alumina nanowire network structure. The method used is simple and easy, and does not require the addition of any dispersant or surface modification of the carbon fibers, with low cost and simple process.

[0007] With the development of science and technology, the aerospace field has put forward higher requirements for the temperature resistance, light weight, effective absorption bandwidth and other multifunctional and efficient coupling of thermal insulation / stealth integrated materials. At present, there is no method to achieve aerogel materials with the characteristics of high temperature resistance, light weight, low cost, high efficiency thermal insulation / stealth, and integrated molding at the same time. Therefore, it is necessary to develop a thermal insulation / stealth integrated aerogel material that is easy to mold, low cost, high temperature resistant and has flexible and adjustable dielectric properties. Summary of the invention

[0008] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing a dielectrically adjustable high-temperature resistant, heat-insulating and stealth integrated material.

[0009] In a first aspect, the present invention provides a method for preparing a dielectrically adjustable high-temperature resistant, heat-insulating and stealthy integrated material, the method comprising the following steps:

[0010] (1) Dissolve 1-30 g of aluminum oxide nanopowder (particle size 5-50 nm) in 10-200 mL of water, add a mixed solution of 0.001-1 mol / L hydrochloric acid, 0.001-1 mol / L acetic acid, and 0.001-1 mol / L sulfuric acid as an adsorbent, and obtain an aluminum oxide precursor dispersion.

[0011] (2) Add 1% to 50% of the mass of the alumina nanopowder in the form of chopped carbon fibers (the length of the chopped carbon fibers is 0.5 to 10 mm) to the dispersion obtained in step (1), and stir evenly with a high-speed disperser (stirring speed 500 to 3000 r / min) to obtain a precursor dispersion that is uniform and stable for a long time. React at 100 to 300° C. for 1 to 20 hours to obtain an alumina nanowire-carbon fiber wet gel with a diameter of 10 to 100 nm and a length of 1 to 20 μm.

[0012] (3) The alumina nanowire-carbon fiber cluster obtained in step (2) is subjected to gradient molding, and is rapidly molded by using a graded molding pressure with a gradient increase to achieve rapid orientation of the chopped carbon fibers, wherein the molding pressure ranges from 0.5 to 20 MPa, and the molding time under each molding pressure is 5 to 40 min.

[0013] (4) The alumina nanowire-carbon fiber composite gel obtained in step (3) is placed in 1 to 20 times ethanol for solvent replacement, and the replacement is performed 1 to 5 times, each time for 1 to 10 days.

[0014] (5) supercritically drying the composite gel after the solvent replacement in step (4) to obtain an aerogel material.

[0015] (6) The aerogel obtained in step (5) is subjected to a low-temperature heat treatment process in a nitrogen or argon atmosphere to obtain a lightweight aerogel with an adjustable dielectric constant.

[0016] (7) The prepared aerogel has a heat resistance of 1200°C in an oxygen-free and oxygen-deficient environment, and the dielectric constant is adjustable in a wide range. Within 1 to 18 GHz, the real part can be adjusted in the range of 1 to 35, and the imaginary part can be adjusted in the range of 0.01 to 100. The room temperature thermal conductivity is 0.030-0.060 W / m·K, the thermal conductivity at 1000°C is 0.05-0.1 W / m·K, and the density is 0.1-0.3 g / cm 3 .

[0017] In a second aspect, the present invention provides a dielectrically adjustable high temperature resistant, heat insulating and stealth integrated material as described in the first aspect of the present invention.

[0018] Compared with the prior art, the present invention has at least the following beneficial effects:

[0019] (1) The present invention is different from other carbon fiber composite aerogel insulation materials. In this study, an alumina precursor dispersion with a certain viscosity is used to disperse short chopped carbon fibers of different lengths and contents stably and evenly for a long time through different stirring processes. This solves the problem of fiber sedimentation and uneven distribution in the solution in other carbon fiber composite aerogel materials, and there is no need to add a dispersant or modify the carbon fiber, so the process is simple and the cost is low.

[0020] (2) The present invention is different from other high-temperature resistant aerogel insulation materials prepared by doping and modification. In this study, nanowires with longer lengths are used as the main units for the assembly process. The nanowires prepared in typical embodiments have a diameter as low as 10 to 100 nm and a length of 1 to 20 μm, which not only ensures a low thermal conductivity, but also improves the overall temperature resistance of the material due to the self-supporting effect of the three-dimensional network structure.

[0021] (3) Nanowire-carbon fiber clusters with relatively large aspect ratios can realize a physically cross-linked wet gel network structure rather than cross-linking through chemical bonds. The wet gel can be repeatedly shaped, with strong process applicability and high utilization rate.

[0022] (4) The present invention evenly distributes large-scale (micrometer-millimeter scale) chopped carbon fibers in a small-scale (nanometer-micrometer scale) high aspect ratio alumina nanowire skeleton structure to construct a two-level network structure. The alumina nanowire skeleton serves as a good wave-transmitting matrix, and by introducing a certain proportion of wave absorbers, precise control of a wide range of dielectric constants can be achieved.

[0023] (5) In the two-level network structure constructed by the present invention, the carbon fibers are three-dimensionally overlapped to form a conductive path, thereby improving the conductive loss of the alumina-carbon fiber composite aerogel, and achieving a wide range of adjustable dielectric constants of the composite aerogel by regulating the carbon fiber content, length and distribution.

[0024] (6) Nanowires have the functions of self-supporting and self-toughening skeletons, eliminating the fiber reinforcement process of traditional aerogel composite materials, and their lightweight performance is improved by more than 50% compared with similar aerogel products. In addition, carbon fibers with a length of millimeters further enhance the mechanical properties of aerogels.

[0025] (7) In this patent, by regulating the molding process, on the one hand, alumina nanowire-carbon fiber composite aerogels with different densities can be obtained. On the other hand, for chopped carbon fibers with a certain content and length, the dielectric constant of the composite aerogel can be controlled by density regulation and gradient molding, providing a material basis for constructing broadband stealth / thermal insulation materials.

[0026] (8) The alumina nanowire-carbon fiber composite aerogel in this patent can withstand temperatures up to 1200°C in oxygen-free and oxygen-deficient environments and has good high-temperature stability. On the one hand, compared with silica-based aerogel materials with a temperature resistance of 600 to 800°C, the γ-alumina aerogel prepared by the present invention is a material with very stable chemical properties and can maintain good structural integrity in a high-temperature thermal environment. On the other hand, the alumina nanowire aerogel has a highly porous three-dimensional network structure, which can achieve thermal insulation properties and reduce the ambient temperature of the carbon fiber. At the same time, the aerogel nanoporous structure can effectively prevent air convection, reduce the oxygen component, and reduce the oxidation rate of the carbon fiber to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a preparation flow chart of the present invention.

[0028] Figure 2 This is a physical picture of the alumina nanowire-carbon fiber composite aerogel prepared in Implementation Option 1.

[0029] Figure 3 is a SEM image of aluminum oxide nanowires in the aerogel prepared in Implementation Example 1.

[0030] Figure 4 This is a SEM image of the alumina nanowire-carbon fiber composite aerogel prepared in Implementation Option 1.

[0031] Figure 5 This is a diagram of the dielectric properties of carbon fiber-alumina nanowire composite aerogels with different contents prepared in Implementation Option 1. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0033] In a first aspect, the present invention provides a method for preparing a dielectrically adjustable high temperature resistant thermal insulation stealth integrated material, the method comprising the following steps:

[0034] The present invention will be further described below by way of examples, but the protection scope of the present invention is not limited to these embodiments.

[0035] Example 1

[0036] (1) 6 g of aluminum oxide nanopowder (particle size: 20 nm) was dissolved in 100 mL of water, 0.02 mol / L of hydrochloric acid, 0.02 mol / L of acetic acid and 0.02 mol / L of sulfuric acid were added as adsorbents, and the mixture was stirred thoroughly to obtain an aluminum oxide precursor dispersion.

[0037] (2) Add 0.9 g of carbon fiber with a length of 3 mm to the dispersion obtained in step (1) and disperse uniformly, and obtain a uniform and stable dispersion by stirring at a stirring speed of 1000 r / min. The dispersion is reacted at 220° C. for 7 h to obtain a wet gel of alumina nanowire-carbon fiber clusters with a diameter of 50 nm and a length of 1 to 20 μm.

[0038] (3) The alumina nanowire-carbon fiber cluster obtained in step (2) is subjected to gradient molding, and molding is carried out at a molding pressure of 2 MPa for 10 min, 4 MPa for 30 min, and 6 MPa for 10 min, and is rapidly formed under the gradient increasing molding pressure.

[0039] (4) The alumina nanowire-carbon fiber composite gel obtained in step (3) was placed in 5 times ethanol for solvent replacement, and the replacement was performed 3 times, each time for 3 days.

[0040] (5) supercritically drying the composite gel after the solvent replacement in step (4) to obtain an aerogel material.

[0041] (6) The aerogel obtained in step (5) is subjected to a heat treatment at 800° C. in a nitrogen atmosphere to obtain a lightweight aerogel with adjustable dielectric constant.

[0042] (7) The prepared aerogel has a heat resistance temperature of 1200°C in an oxygen-free and oxygen-deficient environment, a real part of the dielectric constant of 16 to 7.8, and an imaginary part of the dielectric constant of 11.4 to 4.6 in the frequency range of 1 to 18 GHz. The room temperature thermal conductivity is 0.043 W / m·K, and the density is 0.167 g / cm 3 .

[0043] Example 2

[0044] Example 2 is basically the same as Example 1, except that the amount of alumina nanopowder in step 1 is 25 g.

[0045] The thermal insulation and dielectric properties of the aerogel material in Example 2 were tested, and it was found that the surface of the aerogel material was flat and uniform in color, and it did not fall off when gently touched. Other performance indicators are shown in Table 1.

[0046] Example 3

[0047] Example 3 is basically the same as Example 1, except that the carbon fiber content in step 2 is 1.8 g.

[0048] The thermal insulation and dielectric properties of the aerogel material in Example 3 were tested, and it was found that the surface of the aerogel material was smooth and the color was uniform. Compared with the aerogel in Example 1, the color was darker and there was no falling off when gently touched. Other performance indicators are shown in Table 1.

[0049] Example 4

[0050] Example 4 is substantially the same as Example 1, except that the carbon fiber used in step 2 is 5 mm in length.

[0051] The thermal insulation and dielectric properties of the aerogel material in Example 4 were tested, and it was found that the surface of the aerogel material was flat and uniform in color, and it did not fall off when gently touched. Other performance indicators are shown in Table 1.

[0052] Example 5

[0053] Example 5 is basically the same as Example 1, except that the molding process in step 3 does not undergo gradient molding, but is only molded at a pressure of 0.05 MPa for 50 minutes.

[0054] The thermal insulation and dielectric properties of the aerogel material in Example 5 were tested, and it was found that the surface of the aerogel material had microcracks, and blocks fell off when gently touched. Other performance indicators are shown in Table 1.

[0055] Example 6

[0056] Example 6 is substantially the same as Example 1, except that: in step 4, solvent replacement is performed only twice.

[0057] The thermal insulation and dielectric properties of the aerogel material in Example 6 were tested, and it was found that the surface of the aerogel material had cracks and depressions and was slightly moist after supercritical drying. Other performance indicators are shown in Table 1.

[0058] Example 7

[0059] Example 7 is substantially the same as Example 1, except that the prepared aerogel does not undergo the final heat treatment process.

[0060] The aerogel surface in Example 7 is smooth without any cracking or falling off problems.

[0061] Example 8

[0062] Example 8 is substantially the same as Example 1, except that no chopped carbon fibers are added in step 2.

[0063] The aerogel surface in Example 8 is smooth without any cracking or falling off problems.

[0064] Comparative Example 1

[0065] Comparative Example 1 is substantially the same as Example 1, except that: in step 1, a spherical nanocrystal solution with a diameter of 15 nm is used instead of nanowire clusters for the forming process, and the subsequent steps are the same.

[0066] The results showed that the obtained material was a powder rather than an aerogel block.

[0067] Comparative Example 2

[0068] Comparative Example 2 is substantially the same as Example 1, except that in step 2, ultrasonic dispersion of the chopped carbon fibers is adopted.

[0069] The results show that the chopped carbon fibers in the dispersion are sedimented, and the carbon fibers in the wet gel obtained after the reaction are obviously unevenly distributed. The thermal insulation and dielectric properties of the alumina aerogel material in Comparative Example 2 are tested, and it is found that the surface color of the aerogel material is uneven and there is obvious carbon fiber agglomeration. Other performance indicators are shown in Table 1.

[0070] Comparative Example 3

[0071] Comparative Example 3 is substantially the same as Example 1, except that 0.001 mol / L hydrochloric acid is added as an adsorbent in step 1.

[0072] The results show that the obtained alumina precursor dispersion has low viscosity, the carbon fiber is evenly dispersed and stable for a short time, and the wet gel obtained in step 2 has obvious color gradient changes. The aerogel obtained in step 6 has problems of different color depths and uneven distribution of carbon fibers.

[0073] Comparative Example 4

[0074] Comparative Example 4 is substantially the same as Example 1, except that: the gradient molding process is not performed in step 2;

[0075] During the SEM test, it was found that there were a large number of pores inside the prepared material, causing defects.

[0076] Comparative Example 5

[0077] Comparative Example 5 is substantially the same as Example 1, except that Step 1 and Step 2 are changed to disperse the chopped carbon fibers in the silica sol system by stirring.

[0078] The results show that the chopped carbon fibers dispersed in silica sol only undergo significant sedimentation in a very short period of time.

[0079] The performance indicators of the high temperature resistant, heat insulating and stealth integrated aerogel materials of Examples 1 to 8 and the aerogel materials of Comparative Examples 1 to 5 are shown in Table 1.

[0080] Table 1: Performance indicators of the alumina-carbon fiber composite aerogel materials prepared in Examples 1 to 8 and the aerogel materials in Comparative Examples 1 to 5.

[0081]

[0082] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a dielectrically adjustable high-temperature resistant, heat-insulating and stealth integrated material, characterized in that: The method comprises the following steps: (1) The chopped carbon fibers with different contents and lengths are uniformly and stably dispersed in the alumina precursor solution by mechanical stirring. The stirring speed is 500-3000 r / min. The distribution of the chopped carbon fibers in the dispersion is controlled by selecting different rotation speeds. (2) A mixture of hydrochloric acid, acetic acid and sulfuric acid was used as a catalyst to prepare a high aspect ratio alumina nanowire-carbon fiber wet gel through a high temperature hydrothermal reaction. (3) The alumina nanowire-carbon fiber clusters obtained in step (2) are subjected to gradient molding, and are rapidly formed by using a graded molding pressure with a gradient increase to achieve rapid orientation of the chopped carbon fibers, wherein the molding pressure ranges from 0.5 to 20 MPa, and the molding time under each molding pressure is 5 to 40 min. (4) The alumina nanowire-carbon fiber composite gel obtained in step (3) is placed in 1 to 20 times ethanol for solvent replacement, and the replacement is performed 1 to 5 times, each time for 1 to 10 days. (5) supercritically drying the wet gel after the solvent replacement in step (4) to obtain an aerogel material. (6) The aerogel obtained in step (5) is subjected to a low-temperature heat treatment process in a nitrogen or argon atmosphere to obtain a lightweight aerogel with an adjustable dielectric constant. (7) The prepared aerogel has a heat resistance of 1200°C in an oxygen-free and oxygen-deficient environment, and the dielectric constant is adjustable in a wide range. Within 1 to 18 GHz, the real part can be adjusted in the range of 1 to 35, and the imaginary part can be adjusted in the range of 0.01 to 100. The room temperature thermal conductivity is 0.030-0.060 W / m·K, the thermal conductivity at 1000°C is 0.05-0.1 W / m·K, and the density is 0.1-0.3 g / cm 3 .

Citation Information

Patent Citations

  • Chopped carbon fiber reinforced aluminum silicate ceramic-based composite material and preparation method thereof

    CN111718180A

  • Alumina-carbon composite nanofiber aerogel material and preparation method thereof