Production method of polyethylene wax with high adhesion for pigment

By adding polar molecules and catalysts to polyethylene wax, a polyethylene wax with high adhesion is formed, which solves the problem of insufficient adhesion of conventional polyethylene wax and significantly improves the adhesion of pigments and the wear resistance of the coating.

CN118791653AInactive Publication Date: 2024-10-18GUANGDONG TAILI NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411023804.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The non-polar nature of conventional polyethylene wax results in reduced adhesion, affecting the adhesion of pigments and the abrasion resistance of the coating.

Method used

By adding polar molecules such as maleic anhydride, dodecyl alcohol and isocyanate to polyethylene wax to form an ester bond, urea or urea bond structure to enhance its adhesion, and use specific catalysts such as di-tert-butyl peroxide Accelerate the grafting reaction with triisobutylaluminum to form polyethylene wax with a certain cross-linking density.

Benefits of technology

Significantly improves the adhesion and wear resistance of polyethylene wax, enhances the durability and stability of the coating, and prevents coating peeling and wear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the field of macromolecules, in particular to a production method of high-adhesion polyethylene wax for pigments. The production method of the high-adhesion polyethylene wax for the pigment comprises the following steps: S1, preparing the polyethylene wax: adding low-density polyethylene and a solvent into a plastic extruder, setting parameters of the plastic extruder, and after stirring is finished, spraying substances in the plastic extruder into a cooling tank at a high speed to obtain low-molecular-weight polyethylene wax; s2, polyethylene wax modification: adding polyethylene wax, maleic anhydride, dodecyl alcohol, isocyanate and a catalyst into a three-neck flask, introducing inert gas nitrogen, heating and stirring to obtain a crude product, adding acetone into the three-neck flask, heating, melting, refluxing, cooling to room temperature, washing with ethanol, filtering, and drying to obtain the polyethylene wax with high adhesive force.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymers, in particular to a method for producing a polyethylene wax with high adhesion for pigments. Background Art

[0002] As a carrier of color, pigments play an indispensable role in the plastics, coatings, inks and other industries. High-quality pigments not only need to have good color expression, but also excellent physical and chemical stability. In the production and application of pigments, factors such as dispersibility, wettability and glossiness have a direct impact on the comprehensive performance of pigments. Polyethylene wax, with its unique physical and chemical properties, plays an important role in improving the performance of pigments.

[0003] Polyethylene wax is a thermoplastic polymer material with low viscosity, high hardness and good thermal stability. In terms of molecular structure, polyethylene wax has a long carbon chain and low polarity, which makes it have excellent solubility in a variety of solvents. In addition, polyethylene wax has a wide melting point range and can maintain a stable physical state at different processing temperatures.

[0004] Polyethylene wax is widely used as a pigment additive due to its excellent dispersibility, wettability and gloss-enhancing properties. It can coat pigment particles, improve dispersibility, prevent sedimentation, enhance the contact between pigment and substrate, improve wettability and adhesion, thereby improving the wear resistance and gloss of the coating, making the coating more uniform, durable and attractive. However, conventional polyethylene waxes are mostly non-polar molecules with relatively low surface energy. When added to pigments in the form of additives, polyethylene wax may migrate to the surface of the coating and form a thin wax film, resulting in reduced adhesion of the pigment. Therefore, there is still room for improvement. Summary of the invention

[0005] In order to improve the adhesion of polyethylene wax, the present application provides a polyethylene wax with high adhesion for pigments.

[0006] In a first aspect, the present application provides a method for producing a polyethylene wax with high adhesion for pigments, using the following technical solution: A method for producing a polyethylene wax with high adhesion for pigments, comprising the following steps: S1, preparation of polyethylene wax: S1-1, add low-density polyethylene and solvent into the plastic extruder, set the temperature of the plastic extruder conveying end to 200-210°C, the temperature of the melting end to 220-230°C, the temperature of the connecting pipe to 180-200°C, the screw speed to 5-10r / min, and continue stirring for 20-30 minutes; S1-2, after the stirring is finished, the material in the plastic extruder is extruded at a speed of 0.5-1.0m 3 / s spray into the cooling tank to obtain low molecular weight polyethylene wax; S2, polyethylene wax modification: S2-1, add 50-60 parts of polyethylene wax, 10-15 parts of maleic anhydride, 5-8 parts of dodecyl alcohol, 5-8 parts of isocyanate, and 0.5-1 parts of catalyst into a three-necked flask, introduce inert nitrogen gas, heat to 140-160°C, and stir for 30-50 minutes to obtain a crude product; S2-2, add acetone into a three-necked flask, heat to melt and reflux, cool to room temperature, wash with ethanol, filter, and dry to obtain a polyethylene wax with high adhesion.

[0007] By adopting the above technical scheme, maleic anhydride, dodecyl alcohol, and isocyanate are added during the reaction. Maleic anhydride, dodecyl alcohol, and isocyanate are all polar molecules. The carboxylic anhydride functional group of maleic anhydride can react with active oxygen to form an ester bond; isocyanate can react with active hydrogen atoms in polyethylene wax to form urea or urea bond structure to complete grafting; the hydroxyl group (-OH) of dodecyl alcohol and the reactive site in polyethylene wax undergo substitution reaction to form an ether bond (-O-) connection, and the three can synergistically effectively enhance the adhesion of polyethylene wax. At the same time, since dodecyl alcohol has a long hydrophobic structure, it is grafted on polyethylene wax in combination with isocyanate and maleic anhydride, which helps to form polyethylene wax with a certain crosslinking density and structural motion activity, improves the wear resistance of polyethylene wax, and is not easy to reduce the wear resistance of polyethylene wax due to the grafting of polar molecules.

[0008] Preferably, the catalyst comprises one or more of di-tert-butyl peroxide (DTBP), dibenzoyl peroxide (BPO), tert-butyl peroxydibenzoate (TBPB), triethylaluminum (TEA), and triisobutylaluminum (TIBA).

[0009] By adopting the above technical solution and using the above one or more substances as catalysts, the activation energy of the reaction can be significantly reduced, the rate of the grafting reaction can be increased, and the reaction can be completed in a shorter time.

[0010] Preferably, the catalyst is composed of di-tert-butyl peroxide and triisobutylaluminum in a mass ratio of 0.2:(0.3-0.8).

[0011] By adopting the above technical scheme, the co-catalytic effect can be achieved by using di-tert-butyl peroxide and triisobutylaluminum as catalysts, which can effectively enhance the generation of free radicals and accelerate the polymerization reaction to form polymer chains; at the same time, the synergy of a specific mass of di-tert-butyl peroxide and triisobutylaluminum can also help promote the directional conversion of the grafting reaction, reduce disordered cross-linking or chain transfer reactions, and improve the adhesion of polyethylene wax.

[0012] Preferably, the isocyanate includes one or more of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate and dicyclohexylmethane diisocyanate.

[0013] By adopting the above technical scheme, isocyanate is added during the polyethylene wax grafting reaction, and the isocyanate can react with the active hydrogen atoms in the polyethylene wax to form urea or urea bond structure to complete the grafting; the surface polarity of the grafted modified polyethylene wax is increased, which effectively improves the adhesion of the grafted polyethylene wax.

[0014] Preferably, the isocyanate is composed of isophorone diisocyanate and dicyclohexylmethane diisocyanate in a mass ratio of (2-5):3.

[0015] By adopting the above technical solution, isophorone diisocyanate and dicyclohexylmethane diisocyanate are mixed in a specific ratio, and IPDI and HMDI can react chemically with the surface of the substrate to form a strong chemical bond or intermolecular force, thereby enhancing the adhesion between the coating and the substrate. This chemical bonding ability can ensure that the coating is not easy to peel off or peel off, and improve the durability and stability of the coating; at the same time, it can be cross-linked with other polymers or resins to form a network structure, thereby enhancing the hardness and wear resistance of the coating. By forming a wear-resistant cross-linked structure, the coating can better resist wear and scratches.

[0016] Preferably, in S2-2, the time for heating, melting and reflux is 1-2 hours.

[0017] By adopting the above technical solution, heating reflux for 1-2 hours can promote the circulation of the crude reaction product, help achieve more uniform mixing between the reactants, avoid local overheating or incomplete reaction, and improve the purity of the product.

[0018] Preferably, the solvent in step S1-1 is petroleum ether.

[0019] By adopting the above technical solution, petroleum ether is used as a carrier to dissolve the raw material or cracking product, which facilitates the cracking reaction; at the same time, petroleum ether can reduce the overall viscosity of the system, making the low-density polyethylene easier to stir and handle.

[0020] In a second aspect, the present application provides a polyethylene wax with high adhesion for pigments, using the following technical solution: A polyethylene wax with high adhesion for pigments is prepared by the method.

[0021] In summary, this application has the following beneficial effects: 1. By adding maleic anhydride, dodecyl alcohol and isocyanate during the reaction, maleic anhydride, dodecyl alcohol and isocyanate are all polar molecules. The carboxylic anhydride functional group of maleic anhydride can react with active oxygen to form an ester bond; isocyanate can react with active hydrogen atoms in polyethylene wax to form urea or urea bond structure to complete grafting; the hydroxyl group (-OH) of dodecyl alcohol and the reactive active site in polyethylene wax undergo substitution reaction to form an ether bond (-O-) connection. The three can synergistically effectively enhance the adhesion of polyethylene wax. At the same time, since dodecyl alcohol has a long hydrophobic structure, it is grafted on polyethylene wax with isocyanate and maleic anhydride, which helps to form polyethylene wax with a certain cross-linking density and structural motion activity, improve the wear resistance of polyethylene wax, and is not easy to reduce the wear resistance of polyethylene wax due to the grafting of polar molecules.

[0022] 2. By using di-tert-butyl peroxide and triisobutylaluminum as catalysts, a co-catalytic effect can be achieved, which can effectively enhance the generation of free radicals and accelerate the polymerization reaction to form polymer chains; at the same time, a specific mass of di-tert-butyl peroxide and triisobutylaluminum work together to promote the directional conversion of the grafting reaction, reduce disordered cross-linking or chain transfer reactions, and improve the adhesion of polyethylene wax.

[0023] 3. By mixing isophorone diisocyanate and dicyclohexylmethane diisocyanate in a specific ratio, IPDI and HMDI can react chemically with the surface of the substrate to form a strong chemical bond or intermolecular force, thereby enhancing the adhesion between the coating and the substrate. This chemical bonding ability can ensure that the coating is not easy to peel off or peel off, and improve the durability and stability of the coating; at the same time, it can cross-link with other polymers or resins to form a network structure, thereby enhancing the hardness and wear resistance of the coating. By forming a wear-resistant cross-linked structure, the coating can better resist wear and scratches. DETAILED DESCRIPTION

[0024] The present application is further described in detail below with reference to the embodiments.

[0025] The raw materials of the following examples and comparative examples are all commercially available, as follows: Low-density polyethylene was purchased from Dongguan Nabaichuan Plastic Chemical Co., Ltd., model M202; The CAS number of maleic anhydride is 108-31-6; The CAS number of glutaric anhydride is 108-55-4; The CAS number of polyethylene glycol is 25322-68-3; The CAS number of dodecyl alcohol is 14848-65-8; The CAS number of isophorone diisocyanate is 4098-71-9; The CAS number of dicyclohexylmethane diisocyanate is 5124-30-1; The CAS number of di-tert-butyl peroxide is 110-05-4; The CAS number of triisobutylaluminum is 100-99-2; The CAS number of polypropylene carbonate is 25511-85-7; The CAS number of polycarbonate polyether is 92451-01-9; The CAS number of toluene diisocyanate is 26471-62-5; The CAS number of dibenzoyl peroxide is 94-36-0; The CAS number of triisobutylaluminum is 100-99-2.

[0026] Example 1 A method for producing a polyethylene wax with high adhesion for pigments comprises the following steps: S1, preparation of polyethylene wax: S1-1, add low-density polyethylene and petroleum ether into the plastic extruder, set the temperature of the plastic extruder delivery end to 200°C, the temperature of the melting end to 220°C, the temperature of the connecting pipe to 180°C, the screw speed to 5r / min, and continue stirring for 20 minutes; S1-2, after the stirring is finished, the material in the plastic extruder is extruded at a speed of 0.5m 3 / s spray into the cooling tank to obtain low molecular weight polyethylene wax; S2, polyethylene wax modification: S2-1, by weight, add 50 g of polyethylene wax, 10 g of maleic anhydride, 5 g of dodecyl alcohol, 2 g of isophorone diisocyanate, 3 kg of dicyclohexylmethane diisocyanate, 0.2 g of di-tert-butyl peroxide, and 0.3 g of triisobutylaluminum into a three-necked flask, introduce inert nitrogen gas, heat to 140°C, and stir at a speed of 50 r / min for 30 minutes to obtain a crude product; S2-2, add acetone into the three-necked flask, melt and reflux at 105 for 1 hour, then cool to room temperature, wash with ethanol, filter and dry to obtain polyethylene wax with high adhesion.

[0027] Example 2 A method for producing a polyethylene wax with high adhesion for pigments comprises the following steps: S1, preparation of polyethylene wax: S1-1, add low-density polyethylene and petroleum ether into the plastic extruder, set the temperature of the plastic extruder delivery end to 210°C, the temperature of the melting end to 230°C, the temperature of the connecting pipe to 200°C, the screw speed to 10r / min, and continue stirring for 30 minutes; S1-2, after the stirring is finished, the material in the plastic extruder is extruded at a speed of 1.0m 3 / s spray into the cooling tank to obtain low molecular weight polyethylene wax; S2, polyethylene wax modification: S2-1, by weight, add 60 g of polyethylene wax, 15 g of maleic anhydride, 8 g of dodecyl alcohol, 5 g of isophorone diisocyanate, 3 kg of dicyclohexylmethane diisocyanate, 0.2 g of di-tert-butyl peroxide, and 0.8 g of triisobutylaluminum into a three-necked flask, introduce inert nitrogen gas, heat to 160°C, and stir at a speed of 50 r / min for 50 minutes to obtain a crude product; S2-2, add acetone into the three-necked flask, melt and reflux at 105 for 2 hours, then cool to room temperature, wash with ethanol, filter and dry to obtain polyethylene wax with high adhesion.

[0028] Example 3 A method for producing a polyethylene wax with high adhesion for pigments comprises the following steps: S1, preparation of polyethylene wax: S1-1, add low-density polyethylene and petroleum ether into the plastic extruder, set the temperature of the plastic extruder delivery end to 205°C, the temperature of the melting end to 225°C, the temperature of the connecting pipe to 190°C, the screw speed to 7r / min, and continue stirring for 25 minutes; S1-2, after the stirring is finished, the material in the plastic extruder is extruded at 0.75m 3 / s spray into the cooling tank to obtain low molecular weight polyethylene wax; S2, polyethylene wax modification: S2-1, by mass, add 55g of polyethylene wax, 12g of maleic anhydride, 6.5g of dodecyl alcohol, 3.5g of isophorone diisocyanate, 3kg of dicyclohexylmethane diisocyanate, 0.2g of di-tert-butyl peroxide, and 0.55g of triisobutylaluminum into a three-necked flask, introduce inert gas nitrogen, heat to 150°C, and stir at a speed of 50r / min for 40 minutes to obtain a crude product; S2-2, add acetone into the three-necked flask, melt and reflux at 105 for 1.5 hours, then cool to room temperature, wash with ethanol, filter, and dry to obtain a polyethylene wax with high adhesion.

[0029] Example 4 The difference from Example 3 is that di-tert-butyl peroxide is replaced by an equal amount of dibenzoyl peroxide.

[0030] Example 5 The difference from Example 3 is that an equal amount of triisobutylaluminum is used to replace triisobutylaluminum.

[0031] Example 6 The difference from Example 3 is that isophorone diisocyanate is replaced by an equal amount of toluene diisocyanate.

[0032] Example 7 The difference from Example 3 is that dicyclohexylmethane diisocyanate is replaced by an equal amount of toluene diisocyanate.

[0033] Comparative Example 1 The difference from Example 3 is that maleic anhydride is replaced by an equal amount of glutaric anhydride.

[0034] Comparative Example 2 The difference from Example 3 is that dodecyl alcohol is replaced by an equal amount of polyethylene glycol.

[0035] Comparative Example 3 The difference from Example 3 is that an equal amount of polyester resin is used to replace isocyanate, and the polycarbonate consists of 3.5 g of polypropylene carbonate and 3 g of polycarbonate polyether.

[0036] Experiment 1 The polyethylene wax with high adhesion for pigments prepared in the above examples and comparative examples was tested according to the liquid ink adhesion fastness test method GB / T13217.7-2009, and each group was tested three times to obtain the average value.

[0037] The above experimental test data are detailed in Table 1.

[0038] Experiment 2 The polyethylene wax with high adhesion for pigments prepared in the above examples and comparative examples was tested according to the test method for abrasion resistance of ink layer in letterpress decoration printed products in GB / T7706-2008, and each group was tested three times to obtain the average value.

[0039] The above experimental test data are detailed in Table 1.

[0040] Table 1 According to the data comparison of Example 3 and Comparative Examples 1-3 in Table 1, it can be obtained that maleic anhydride, dodecyl alcohol, and isocyanate are added during the reaction of Example 3, and the polyethylene wax with high adhesion for pigments prepared by maleic anhydride, dodecyl alcohol, and isocyanate has good adhesion fastness and wear resistance. Comparative Examples 1-3 use equal amounts of glutaric anhydride, polyethylene glycol, and polyester resin to replace maleic anhydride, dodecyl alcohol, and isocyanate, and the wear resistance of the prepared polyethylene wax is reduced. It shows that maleic anhydride, dodecyl alcohol, and isocyanate are added during the reaction, and the three can effectively enhance the adhesion of polyethylene wax in synergy. At the same time, since dodecyl alcohol has a long hydrophobic structure, it is grafted on polyethylene wax with isocyanate and maleic anhydride, which helps to form polyethylene wax with a certain cross-linking density and structural motion activity, improves the wear resistance of polyethylene wax, and is not easy to reduce the wear resistance of polyethylene wax due to the grafting of polar molecules.

[0041] According to the data comparison of Example 3 and Examples 4-5 in Table 1, it can be obtained that a specific mass of di-tert-butyl peroxide cooperates with triisobutyl aluminum to promote the directional conversion of the grafting reaction, reduce disordered cross-linking or chain transfer reactions, and improve the adhesion of the polyethylene wax.

[0042] According to the data comparison of Example 3 and Examples 6-7 in Table 1, it can be obtained that by mixing isophorone diisocyanate and dicyclohexylmethane diisocyanate in a specific ratio, it can be cross-linked with other polymers or resins to form a network structure, thereby enhancing the hardness and wear resistance of the coating. By forming a wear-resistant cross-linked structure, the coating can better resist wear and scratches.

[0043] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A method for producing a polyethylene wax with high adhesion for pigments, characterized in that: The following steps are involved: S1, preparation of polyethylene wax: S1-1, add low-density polyethylene and solvent into the plastic extruder, set the temperature of the plastic extruder conveying end to 200-210°C, the temperature of the melting end to 220-230°C, the temperature of the connecting pipe to 180-200°C, the screw speed to 5-10r / min, and continue stirring for 20-30 minutes; S1-2, after the stirring is finished, the material in the plastic extruder is extruded at a speed of 0.5-1.0m 3 / s spray into the cooling tank to obtain low molecular weight polyethylene wax; S2, polyethylene wax modification: S2-1, add 50-60 parts of polyethylene wax, 10-15 parts of maleic anhydride, 5-8 parts of dodecyl alcohol, 5-8 parts of isocyanate, and 0.5-1 parts of catalyst into a three-necked flask, introduce inert nitrogen gas, heat to 140-160°C, and stir for 30-50 minutes to obtain a crude product; S2-2, add acetone into a three-necked flask, heat to melt and reflux, cool to room temperature, wash with ethanol, filter, and dry to obtain a polyethylene wax with high adhesion.

2. The method for producing a polyethylene wax with high adhesion for pigments according to claim 1, characterized in that: The catalyst includes one or more of di-tert-butyl peroxide (DTBP), dibenzoyl peroxide (BPO), tert-butyl peroxydibenzoate (TBPB), triethylaluminum (TEA), and triisobutylaluminum (TIBA).

3. The method for producing a polyethylene wax with high adhesion for pigments according to claim 2, characterized in that: The catalyst is composed of di-tert-butyl peroxide and triisobutyl aluminum in a mass ratio of 0.2:(0.3-0.8).

4. The method for producing a polyethylene wax with high adhesion for pigments according to claim 1, characterized in that: The isocyanate includes one or more of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate and dicyclohexylmethane diisocyanate.

5. The method for producing a polyethylene wax with high adhesion for pigments according to claim 4, characterized in that: The isocyanate is composed of isophorone diisocyanate and dicyclohexylmethane diisocyanate in a mass ratio of (2-5):

3.

6. The method for producing a polyethylene wax with high adhesion for pigments according to claim 1, characterized in that: In the S2-2, the heating, melting and reflux time is 1-2 hours.

7. The method for producing a polyethylene wax with high adhesion for pigments according to claim 1, characterized in that: The solvent in step S1-1 is petroleum ether.

8. A method for producing a polyethylene wax with high adhesion for pigments, characterized in that: The polyethylene wax with high adhesion for pigments is prepared by the production method of any one of claims 1 to 7.

Citation Information

Patent Citations

  • Preparation method of stem grafting polyethylene wax

    CN110343217A

  • Special polar and high-adhesion polyethylene wax for road marking paint and preparation method of special polar and high-adhesion polyethylene wax

    CN110372821A

  • Preparation method of polyethylene wax with low molecular weight distribution index

    CN112694552A

  • Preparation method and application of high lubricated oxidized polyethylene wax

    CN113185626A

  • Preparing process of solid phase grafted polyolefin wax copolymer

    CN1986588A