Novel impact modifier as well as preparation method and application thereof
By using specific components and preparation methods in the toughening agent to form a new impact modifier with a core-shell structure, the problem of insufficient flame retardancy of the existing toughening agents is solved, and it is achieved without affecting other properties. Improve the flame retardant and impact resistance of the resin to meet UL flame retardant requirements.
Patent Information
- Application Number
- CN202410776658.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-17
AI Technical Summary
Existing tougheners have insufficient flame retardancy after being added to plastics, making it difficult to meet UL flame retardant requirements and affecting other properties.
A new impact modifier is used, which consists of specific components, including butadiene components containing diene groups, alkyl methacrylates, vinyl aromatic monomers, urethane-containing and Functional monomers, initiators, emulsifiers and pH buffers with long carbon silicon chains form a core-shell structure through specific preparation methods to improve flame retardancy and impact resistance.
This new impact modifier can significantly improve the flame retardant and impact resistance of the resin without adding flame retardants, meeting UL flame retardant requirements while maintaining good transparency and processing performance.
Smart Images

Figure BDA0004895877520000031 
Figure BDA0004895877520000181 
Figure BDA0004895877520000191
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials, and in particular relates to a novel impact modifier and a preparation method and application thereof. Background Art
[0002] As people pursue lightweight, the application scope of plastics (such as polycarbonate PC, polyvinyl chloride PVC, polypropylene PP, etc.) is getting wider and wider, such as in the fields of electrical appliances, automobiles, home appliances, etc. These plastics need to be in contact with electricity or be in a high-temperature environment for a long time. For the sake of safety, these materials are required to have certain flame retardant properties.
[0003] In the production process of plastics, due to the requirements of impact resistance, it is necessary to add core-shell polymers (such as methyl methacrylate-butadiene-styrene terpolymer (MBS), styrene-butadiene thermoplastic elastomer (SBS), acrylonitrile-butadiene-styrene copolymer (ABS), ethylene-vinyl acetate copolymer (EVA), acrylate copolymer (ACR), etc.) to the plastics. These core-shell polymers are collectively referred to as toughening agents, which have the functions of reducing the brittleness of composite materials and improving the impact resistance of composite materials. However, these types of toughening agents are highly flammable, and adding them to plastics will significantly reduce the flame retardancy of the plastics, making them unable to meet the flame retardancy requirements of UL (Underwriters Laboratory).
[0004] At present, a common improvement method is to introduce phosphorus into the toughening agent to meet the flame retardant requirements. For example, Chinese patent document CN104704051A discloses a method that can improve the flame retardancy of the resulting toughening agent by introducing an emulsifier containing phosphorus to form a toughening agent containing phosphorus after flocculation; Chinese patent document CN109689701A discloses a method that introduces an alkaline phosphate on the basis of introducing an emulsifier containing phosphorus to further improve the flame retardancy of the resulting toughening agent. However, by only introducing phosphorus into the preparation system of the toughening agent, its flame retardancy is still not enough to meet the use requirements.
[0005] In view of this, how to significantly improve the flame retardancy of the toughening agent without affecting other properties is a direction worthy of research. Summary of the invention
[0006] The purpose of the present invention is to provide a new impact modifier and its preparation method and application in view of the technical problems existing in the performance improvement of existing toughening agents. The obtained impact modifier (for example, without adding a flame retardant) can simultaneously have excellent impact resistance and flame retardant properties, and can meet the flame retardant requirements while improving the impact resistance of the resin.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] In a first aspect, a novel impact modifier is provided, which is a product obtained by preparing a modifier composition; based on the total weight (such as 100wt%) of the modifier composition, the modifier composition comprises the following components:
[0009] A) at least one butadiene component containing diene groups, 40-95 wt% (e.g., 42 wt%, 45 wt%, 50 wt%, 52 wt%, 54 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 90 wt%), preferably 51.5-79.5 wt%;
[0010] B) at least one alkyl (meth)acrylate, 1-30 wt% (e.g., 2 wt%, 4 wt%, 5 wt%, 8 wt%, 10 wt%, 15 wt%, 18 wt%, 20 wt%, 22 wt%, 24 wt%, 25 wt%, 28 wt%), preferably 4-25 wt%;
[0011] C) at least one vinyl aromatic monomer, 1-30 wt% (e.g., 2 wt%, 4 wt%, 5 wt%, 8 wt%, 10 wt%, 15 wt%, 18 wt%, 20 wt%, 22 wt%, 24 wt%, 25 wt%, 28 wt%), preferably 1.6-25 wt%;
[0012] D) at least one functional monomer containing carbamate and long carbon silicon chain, 0.1-10wt% (e.g., 0.2wt%, 0.4wt%, 0.5wt%, 0.8wt%, 1wt%, 2wt%, 4wt%, 5wt%, 6wt%, 8wt%, 9wt%), preferably 0.7-7wt%;
[0013] E) initiator, 0.01-1 wt% (e.g., 0.02 wt%, 0.04 wt%, 0.05 wt%, 0.08 wt%, 0.1 wt%, 0.2 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.8 wt%, 0.9 wt%), preferably 0.02-0.5 wt%;
[0014] F) emulsifier, 0.2-5wt% (e.g., 0.3wt%, 0.4wt%, 0.5wt%, 0.8wt%, 1wt%, 2wt%, 2.5wt%, 3.5wt%, 4wt%, 4.5wt%), preferably 0.5-3wt%;
[0015] G) pH buffer, 0.01-1 wt% (e.g., 0.02 wt%, 0.04 wt%, 0.05 wt%, 0.08 wt%, 0.1 wt%, 0.2 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.8 wt%, 0.9 wt%), preferably 0.03-0.5 wt%.
[0016] According to the novel impact modifier provided by the present invention, in some embodiments, the butadiene component containing a diene group is selected from one or more of 1,3-butadiene, isoprene and chloroprene, preferably 1,3-butadiene.
[0017] In some embodiments, the alkyl (meth)acrylate is selected from one or more of methyl acrylate, methyl methacrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isopropyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate and isooctyl (meth)acrylate, preferably methyl methacrylate and / or n-butyl acrylate.
[0018] In some embodiments, the vinyl aromatic monomer is selected from one or more of styrene, 2-methylstyrene, 4-methylstyrene, 2-(n-butyl)styrene, 4-(n-butyl)styrene, 4-(n-decyl)styrene and divinylbenzene, preferably styrene.
[0019] In some embodiments, the functional monomer containing carbamate and long carbon silicon chain is a product obtained by reacting ethyl isocyanate (alkyl) acrylate with hydroxyl-terminated polydimethylsiloxane. The steps and process conditions for reacting ethyl isocyanate (alkyl) acrylate with hydroxyl-terminated polydimethylsiloxane can be conventional operations in the art and will not be described in detail here.
[0020] In some embodiments, the functional monomer containing carbamate and a long carbon-silicon chain can have a specific structure as shown in the following formula I:
[0021]
[0022] In the formula, R1 is H or C n H 2n+1 (n≥1, for example, 2, 3, 4, 5, 6, 8, 10), R2 is C n H 2n (n≥1, for example, 2, 3, 4, 5, 6, 8, 10), R3 is C x H y O z(1≤x≤10, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10; 1≤y≤10, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10; 0≤z≤5, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10).
[0023] In some embodiments, the molecular weight of the functional monomer containing carbamate and long carbon silicon chain is 300-8000 g / mol (for example, 400 g / mol, 450 g / mol, 550 g / mol, 600 g / mol, 800 g / mol, 1000 g / mol, 1500 g / mol, 2000 g / mol, 2500 g / mol, 3000 g / mol, 4000 g / mol, 5000 g / mol, 6000 g / mol, 7000 g / mol), preferably 500-2000 g / mol.
[0024] In some embodiments, the initiator is selected from one or more of peroxides (such as potassium persulfate, ammonium persulfate, sodium persulfate), azo initiators (such as azobisisobutyronitrile) and redox system initiators, preferably redox system initiators.
[0025] The redox system initiator can be produced by the reaction of an oxidizing agent (such as tert-butyl hydroperoxide, cumene hydroperoxide, terpene hydroperoxide) and a reducing agent (such as bleaching powder, sodium pyrosulfite, hydrosulfite, ferrous sulfate, sodium salt of ethylenediaminetetraacetic acid).
[0026] In some embodiments, the emulsifier is selected from one or more of anionic surfactants, nonionic surfactants, anionic nonionic surfactants and cationic surfactants, preferably anionic surfactants and / or anionic nonionic surfactants (such as fatty acid salts and / or fatty alcohol ether phosphates and salts thereof).
[0027] In some embodiments, the anionic surfactant may be, but is not limited to, fatty acid salts, alkyl sulfates, alkyl benzene sulfonates, alkyl phosphates, dialkyl sulfosuccinates, and the like.
[0028] In some embodiments, the nonionic surfactant may be, but is not limited to, polyoxyethylene alkyl ether, polyoxyethylene fatty acid ester, and the like.
[0029] In some embodiments, the anionic nonionic surfactant may be, but is not limited to, fatty alcohol ether phosphate esters and salts thereof or sulfate esters.
[0030] In some embodiments, the cationic surfactant may be, but is not limited to, sorbitol fatty acid esters, glycerol fatty acid esters, and alkylamine salts.
[0031] In some embodiments, the pH buffer is selected from one or more of sodium carbonate, sodium bicarbonate, tripotassium phosphate, potassium carbonate, potassium bicarbonate and sodium dihydrogen phosphate, preferably tripotassium phosphate.
[0032] In some embodiments, the novel impact modifier is a core-shell polymer having: (A) a rubber core, such as a copolymer containing a diene; and (B) an outer shell, mainly comprising a hard polymer, such as a polymer formed from alkyl (meth)acrylate and vinyl aromatic monomer units.
[0033] In some embodiments, the polymerized monomers of the novel impact modifier include core monomers and shell monomers, and the mass ratio of the core monomers to the shell monomers is (70-85):(15-30).
[0034] For example, the polymerized monomers of the novel impact modifier include core layer monomers and shell layer monomers composed as follows:
[0035] (A) 70-85 parts of core layer monomers, comprising: based on 100 parts by total weight of the core layer monomers, 0-10 parts of a vinyl aromatic monomer, 0.1-15 parts of a functional monomer containing carbamate and a long carbon silicon chain, and 85-99.9 parts of a butadiene component containing a diene group;
[0036] (B) 15-30 parts of shell monomers, which include: alkyl (meth)acrylate, vinyl aromatic monomer; wherein the weight ratio of alkyl (meth)acrylate to vinyl aromatic monomer can be 4:1-1:1 (e.g., 3:1, 2:1, 1.85:1, 1.5:1).
[0037] In a second aspect, a method for preparing the novel impact modifier as described above is provided, comprising the following steps:
[0038] (1) adding a rubber core layer monomer, a pH buffer, an initiator and an emulsifier accounting for 2 wt%-100 wt% (e.g., 3 wt%, 4 wt%, 5 wt%, 8 wt%, 10 wt%, 20 wt%, 40 wt%, 50 wt%) of the total amount of the emulsifier into a reaction kettle, stirring and heating (e.g., heating to 50-70° C.); then adding the remaining emulsifier into the reaction kettle within 2-10 h (e.g., 3 h, 4 h, 5 h, 6 h, 8 h), reacting until the system pressure remains unchanged (e.g., it can be reduced to between 0.1 and 0.3 MPa), to obtain a rubber core emulsion; the rubber core layer monomer comprises a butadiene component containing a diene group, a functional monomer containing a carbamate and a long carbon silicon chain, and an optional vinyl aromatic monomer;
[0039] (2) adding an initiator and a shell monomer to the rubber core emulsion, stirring and heating (e.g., heating to 50-80° C.), and keeping the temperature for 1-3 hours (e.g., 1.5 hours, 2 hours, 2.5 hours) after the addition is completed to obtain a grafted emulsion with a core-shell structure; the shell monomer comprises an alkyl (meth)acrylate and a vinyl aromatic monomer;
[0040] (3) flocculating and drying the emulsion obtained in step (2) to obtain a novel impact modifier powder.
[0041] According to the preparation method provided by the present invention, in some embodiments, the reaction temperature in step (1) is 50-70°C (eg, 55°C, 60°C, 65°C).
[0042] In some embodiments, the reaction temperature of step (2) is 60-80°C (eg, 65°C, 70°C, 75°C).
[0043] In some embodiments, the flocculation temperature in step (3) is 25-60°C (e.g., 30°C, 40°C, 50°C, 55°C); the flocculant is selected from an inorganic acid or a metal salt; such as, one or more of hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, calcium chloride, magnesium sulfate, calcium acetate and aluminum sulfate.
[0044] In some embodiments, during the drying process of step (3), the drying process is performed until the moisture content of the material is less than or equal to 1%. The drying process conditions can be selected conventionally in the art.
[0045] When preparing the grafted emulsion having a core-shell structure, the rubber core emulsion may be subjected to a VOC removal operation to remove unreacted butadiene monomers in the system.
[0046] The novel impact modifier of the present invention has good impact resistance and can be mixed with resins such as polyvinyl chloride and polycarbonate to improve the impact resistance of the resin without affecting the transparency. It can also be used in many occasions, such as calendered sheets, injection molded products, blow molded products or extruded products.
[0047] In a third aspect, a use of the novel impact modifier as described above or the novel impact modifier prepared by the preparation method as described above in polycarbonate plastic is provided.
[0048] The application method of the novel impact modifier in polycarbonate plastics can be achieved through conventional operations in the art.
[0049] Compared with the prior art, the beneficial effects of the technical solution of the present invention are mainly reflected in:
[0050] 1) In the impact modifier formula of the present invention, functional monomers containing silicon and carbamate are selected for polymerization, wherein the silicon can form a dense silicon dioxide layer when burning, thereby isolating the transfer of oxygen and energy, and the nitrogen in the carbamate can produce nitrogen and nitric oxide and other substances when burning, diluting the concentration of oxygen; these products can reduce the flame temperature and thermal radiation intensity, and the silicon and nitrogen are in the same molecular structure, and the silicon and nitrogen have a strong synergistic effect, which can improve the flame retardant performance of the impact modifier and its application in resin;
[0051] 2) Compared with other flame retardant monomers, the impact modifier of the present invention uses functional monomers containing silicon and carbamate. Since siloxane is distributed in a longer molecular chain, it has a lower glass transition temperature, and its molecular chain has stronger mobility, which can absorb more energy when impacted, thereby improving the impact resistance of the impact modifier and its application in resin;
[0052] 3) The novel impact modifier of the present invention has a simple preparation process, is easy to operate, and is safe and non-toxic in the polymerization formula; the functional monomer containing a special structure has a low polarity and can be well polymerized with the diene monomer. DETAILED DESCRIPTION
[0053] In order to understand the technical features and content of the present invention in detail, the preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described in the embodiments, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. For those who do not specify specific conditions in the embodiments, they are carried out according to normal conditions or the conditions recommended by the manufacturer.
[0054] In the following examples and comparative examples, the sources of some reagents or raw materials used, if the manufacturer of the reagents or raw materials is not indicated, are conventional products that can be purchased from the market.
[0055] in:
[0056] Butadiene: Wanhua Chemical Company;
[0057] Methyl methacrylate (MMA): Wanhua Chemical Company;
[0058] Styrene (St): Wanhua Chemical Company;
[0059] Isopropyl hydrogen peroxide (CHP): Aladdin Chemical Reagent Company;
[0060] Tert-butyl hydroperoxide (BHP): Guangzhou Yuanchuang Chemical Co., Ltd.;
[0061] Ferrous sulfate heptahydrate: Aladdin Chemical Reagent Company;
[0062] Ethylenediaminetetraacetic acid disodium salt: Aladdin Chemical Reagent Company;
[0063] Sodium formaldehyde sulfoxylate (SFS), Aladdin Chemical Reagent Company;
[0064] Sodium polyoxyethylene alkyl ether phosphate: Solvay Chemical Company;
[0065] Tripotassium phosphate: Aladdin Chemical Reagent Company;
[0066] Antioxidant IRGANOX 1076: BASF Chemical Co., Ltd.
[0067] Calcium chloride: Aladdin Chemical Reagent Co., Ltd.
[0068] Example of preparation of functional monomers containing carbamate and long carbon-silicon chains:
[0069] The preparation process of functional monomer-1 containing carbamate and long carbon silicon chain (hereinafter referred to as functional monomer S-1) is as follows: in the presence of 100ppm of organic bismuth catalyst 8108, isocyanate ethyl methacrylate and KF6001 (hydroxyl-modified two-end type silicone oil) purchased from Xinyue Company are added into a stirring reactor in a molar ratio of 1:1, and reacted at 70°C until the NCO value is 0% and the reaction is stopped to obtain functional monomer S-1; its molecular weight is 1964g / mol.
[0070] The preparation process of functional monomer-2 containing carbamate and long carbon silicon chain (hereinafter referred to as functional monomer S-2) is as follows: in the presence of 100 ppm of organic bismuth catalyst 8108, isocyanate ethyl acrylate and C2812 (hydroxyl-modified two-terminal silicone oil) purchased from Momentive are added into a stirring reactor in a molar ratio of 1:1, and reacted at 75°C until the NCO value is 0% and the reaction is stopped to obtain functional monomer S-2; its molecular weight is 2141 g / mol.
[0071] In the following examples and comparative examples, the amount of each component used is in parts by weight.
[0072] Embodiment 1:
[0073] The preparation method of the impact modifier comprises the following steps:
[0074] (1) Preparation of butadiene rubber core polymer emulsion
[0075] In a pressure-resistant polymerization reactor with a stirrer, stirring is started and 200 parts of pure water, 0.3 parts of tripotassium phosphate, 0.0012 parts of ferrous sulfate heptahydrate, 0.008 parts of disodium ethylenediaminetetraacetic acid (EDTA), 0.03 parts of polyoxyethylene alkyl ether sodium phosphate, and 5 parts of functional monomer (S-1) are added; at the same time, the gas inside the pressure-resistant polymerization reactor is evacuated and replaced with nitrogen to fully remove oxygen; then, 95 parts of butadiene (Bd), 0.05 parts of sodium formaldehyde sulfoxylate (SFS) and 0.2 parts of isopropyl hydrogen peroxide (CHP) are added into the pressure-resistant polymerization reactor; and 1.4 parts of polyoxyethylene alkyl ether sodium phosphate are dripped into the pressure-resistant polymerization reactor within 6 hours; a polymerization reaction is carried out at 50° C. until the system pressure does not change and the polymerization conversion rate is 98wt%; after the polymerization is completed, the unreacted butadiene monomer in the system is removed to obtain a rubber core aqueous latex containing polybutadiene rubber as a main component;
[0076] (2) Preparation of graft copolymer emulsion
[0077] Based on 100 parts by weight of the total solid content of the rubber core aqueous latex obtained in step (1), 71 parts by weight of the solid content of the rubber core aqueous latex obtained in step (1) are added to a pressure-resistant polymerization reactor equipped with a stirrer, and the gas in the reactor is replaced with nitrogen to remove oxygen; the reaction raw materials are added under stirring at 60° C. to carry out polymerization reaction, namely: (a) 22 parts of methyl methacrylate (MMA) and 7 parts of styrene (St) are continuously added to the reactor over 60 minutes, and (b) 0.07 parts of tert-butyl hydroperoxide (BHP) and 0.1 parts of sodium formaldehyde sulfoxylate (SFS) are all added to the reactor over 2 hours; and the addition of MMA and St is started simultaneously with the addition of BHP and SFS; after the addition of all the amounts of BHP and SFS is completed, the reaction solution is further kept at 60° C. for 1 hour to terminate the polymerization reaction, thereby obtaining a graft copolymer emulsion having a core-shell structure;
[0078] (3) Flocculation and drying
[0079] Based on 100 parts by weight of the solid content of the graft copolymer emulsion with a core-shell structure obtained in step (2), 2 parts of IRGANOX 1076 [n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate] as a phenolic antioxidant are added to the graft copolymer emulsion obtained in step (2), and then flocculation and coagulation are carried out at 54° C. with 767 parts of calcium chloride aqueous solution (concentration of 0.3wt%), followed by water washing, and then drying the dehydrated material at 45° C. until its water content is less than 1wt%, to obtain a powdery graft copolymer-1.
[0080] Embodiment 2:
[0081] The preparation method of the impact modifier comprises the following steps:
[0082] (1) Preparation of butadiene rubber core polymer emulsion
[0083] In a pressure-resistant polymerization reactor with a stirrer, stirring is started and 200 parts of pure water, 0.2 parts of tripotassium phosphate, 0.0012 parts of ferrous sulfate heptahydrate, 0.008 parts of disodium ethylenediaminetetraacetic acid (EDTA), 0.03 parts of polyoxyethylene alkyl ether sodium phosphate, and 10 parts of functional monomer (S-1) are added; at the same time, the gas inside the pressure-resistant polymerization reactor is evacuated and replaced with nitrogen to fully remove oxygen; then, 90 parts of butadiene (Bd), 0.05 parts of sodium formaldehyde sulfoxylate (SFS) and 0.2 parts of isopropyl hydrogen peroxide (CHP) are added into the pressure-resistant polymerization reactor; and 1.4 parts of polyoxyethylene alkyl ether sodium phosphate are dripped into the pressure-resistant polymerization reactor within 6 hours; a polymerization reaction is carried out at 50° C. until the system pressure does not change and the polymerization conversion rate is 99wt%; after the polymerization is completed, the unreacted butadiene monomer in the system is removed to obtain a rubber core aqueous latex containing polybutadiene rubber as a main component;
[0084] (2) Preparation of graft copolymer emulsion
[0085] Based on the total solid content of the rubber core aqueous latex obtained in step (1) as 100 parts by weight, 71 parts by weight of the solid content of the rubber core aqueous latex obtained in step (1) are added to a pressure-resistant polymerization reactor equipped with a stirrer, and at the same time, the gas in the reactor is replaced with nitrogen to remove oxygen; 22 parts of methyl methacrylate (MMA) and 7 parts of styrene (St) are added to the reactor, and after stirring for five minutes, heating is turned on. After the system temperature rises to 60° C., a mixture of 0.07 parts of tert-butyl hydroperoxide (BHP) and 5 parts of water and a mixture of 0.1 parts of sodium formaldehyde sulfoxylate (SFS) and 4 parts of water are added to the reactor to carry out polymerization; after the addition of the raw materials is completed, the reaction solution is maintained at 65° C. for 2 hours. After the polymerization is completed, a graft copolymer emulsion with a core-shell structure is obtained;
[0086] (3) Flocculation and drying
[0087] Based on 100 parts by weight of the solid content of the graft copolymer emulsion with a core-shell structure obtained in step (2), 2 parts of IRGANOX 1076 [n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate] as a phenolic antioxidant are added to the graft copolymer emulsion obtained in step (2), and then flocculation and coagulation are carried out at 60° C. with 810 parts of calcium chloride aqueous solution (concentration of 0.14wt%), followed by water washing, and then drying the dehydrated material at 60° C. until its water content is less than 1wt%, to obtain a powdery graft copolymer-2.
[0088] Embodiment 3:
[0089] (1) Preparation of butadiene rubber core polymer emulsion
[0090] In a pressure-resistant polymerization reactor with a stirrer, stirring is started and 200 parts of pure water, 0.03 parts of tripotassium phosphate, 0.0012 parts of ferrous sulfate heptahydrate, 0.008 parts of disodium ethylenediaminetetraacetic acid (EDTA), 0.03 parts of polyoxyethylene alkyl ether sodium phosphate, and 10 parts of functional monomer (S-1) are added; at the same time, the gas inside the pressure-resistant polymerization reactor is evacuated and replaced with nitrogen to fully remove oxygen; then, 90 parts of butadiene (Bd), 0.05 parts of sodium formaldehyde sulfoxylate (SFS) and 0.2 parts of isopropyl hydrogen peroxide (CHP) are added into the pressure-resistant polymerization reactor; and 1.4 parts of polyoxyethylene alkyl ether sodium phosphate are dripped into the pressure-resistant polymerization reactor within 6 hours; a polymerization reaction is carried out at 50° C. until the system pressure does not change and the polymerization conversion rate is 99wt%; after the polymerization is completed, the unreacted butadiene monomer in the system is removed to obtain a rubber core aqueous latex containing polybutadiene rubber as a main component;
[0091] (2) Preparation of graft copolymer emulsion
[0092] Based on the total solid content of the rubber core aqueous latex obtained in step (1) as 100 parts by weight, 80 parts by weight of the solid content of the rubber core aqueous latex obtained in step (1) are added into a pressure-resistant polymerization reactor equipped with a stirrer, and at the same time, the gas in the reactor is replaced with nitrogen to remove oxygen; 13 parts of methyl methacrylate (MMA) and 7 parts of styrene (St) are added into the reactor, and after stirring for five minutes, heating is turned on. After the system temperature rises to 60° C., a mixture of 0.14 parts of tert-butyl hydroperoxide (BHP) and 5 parts of water and a mixture of 0.1 parts of sodium formaldehyde sulfoxylate (SFS) and 4 parts of water are added into the reactor to carry out polymerization; after the addition of the raw materials is completed, the reaction solution is maintained at 60° C. for 1 hour. After the polymerization is completed, a graft copolymer emulsion with a core-shell structure is obtained;
[0093] (3) Flocculation and drying
[0094] Based on 100 parts by weight of the solid content of the graft copolymer emulsion with a core-shell structure obtained in step (2), 2 parts of IRGANOX 1076 [n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate] as a phenolic antioxidant are added to the graft copolymer emulsion obtained in step (2), and then flocculation and coagulation are carried out at 49° C. with 805 parts of an aqueous solution of calcium chloride (concentration of 0.18wt%), followed by water washing, and then drying the dehydrated material at 50° C. until its water content is less than 1wt%, to obtain a powdery graft copolymer-3.
[0095] Embodiment 4:
[0096] The preparation method of the impact modifier comprises the following steps:
[0097] (1) Preparation of butadiene rubber core polymer emulsion
[0098] In a pressure-resistant polymerization reactor with a stirrer, stirring is started and 200 parts of pure water, 0.3 parts of tripotassium phosphate, 0.0012 parts of ferrous sulfate heptahydrate, 0.008 parts of disodium ethylenediaminetetraacetic acid (EDTA), 0.03 parts of polyoxyethylene alkyl ether sodium phosphate, and 5 parts of functional monomer (S-2) are added; at the same time, the gas inside the pressure-resistant polymerization reactor is evacuated and replaced with nitrogen to fully remove oxygen; then, 95 parts of butadiene (Bd), 0.05 parts of sodium formaldehyde sulfoxylate (SFS) and 0.2 parts of isopropyl hydrogen peroxide (CHP) are added into the pressure-resistant polymerization reactor; and 1.4 parts of polyoxyethylene alkyl ether sodium phosphate are dripped into the pressure-resistant polymerization reactor within 6 hours; a polymerization reaction is carried out at 50° C. until the system pressure does not change and the polymerization conversion rate is 98wt%; after the polymerization is completed, the unreacted butadiene monomer in the system is removed to obtain a rubber core aqueous latex containing polybutadiene rubber as the main component;
[0099] (2) Preparation of graft copolymer emulsion
[0100] Based on 100 parts by weight of the total solid content of the rubber core aqueous latex obtained in step (1), 71 parts by weight of the solid content of the rubber core aqueous latex obtained in step (1) are added to a pressure-resistant polymerization reactor equipped with a stirrer, and the gas in the reactor is replaced with nitrogen to remove oxygen; the reaction raw materials are added under stirring at 60° C. to carry out polymerization reaction, namely: (a) 22 parts of methyl methacrylate (MMA) and 7 parts of styrene (St) are continuously added to the reactor over 60 minutes, and (b) 0.07 parts of tert-butyl hydroperoxide (BHP) and 0.1 parts of sodium formaldehyde sulfoxylate (SFS) are all added to the reactor over 2 hours; and the addition of MMA and St is started simultaneously with the addition of BHP and SFS; after the addition of all the amounts of BHP and SFS is completed, the reaction solution is further kept at 60° C. for 1 hour to terminate the polymerization reaction, thereby obtaining a graft copolymer emulsion having a core-shell structure;
[0101] (3) Flocculation and drying
[0102] Based on 100 parts by weight of the solid content of the graft copolymer emulsion with a core-shell structure obtained in step (2), 2 parts of IRGANOX 1076 [n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate] as a phenolic antioxidant are added to the graft copolymer emulsion obtained in step (2), and then flocculation and coagulation are carried out at 51° C. with 800 parts of calcium chloride aqueous solution (concentration of 0.14wt%), followed by water washing, and then drying the dehydrated material at 45° C. until its water content is less than 1wt%, to obtain a powdery graft copolymer-4.
[0103] Embodiment 5:
[0104] The preparation method of the impact modifier comprises the following steps:
[0105] (1) Preparation of butadiene rubber core polymer emulsion
[0106] In a pressure-resistant polymerization reactor with a stirrer, stirring is started and 200 parts of pure water, 0.3 parts of tripotassium phosphate, 0.0012 parts of ferrous sulfate heptahydrate, 0.008 parts of disodium ethylenediaminetetraacetic acid (EDTA), 0.03 parts of polyoxyethylene alkyl ether sodium phosphate, and 0.2 parts of functional monomer (S-2) are added; at the same time, the gas inside the pressure-resistant polymerization reactor is evacuated and replaced with nitrogen to fully remove oxygen; then, 99.8 parts of butadiene (Bd), 0.05 parts of sodium formaldehyde sulfoxylate (SFS) and 0.2 parts of isopropyl hydrogen peroxide (CHP) are added into the pressure-resistant polymerization reactor; and 1.4 parts of polyoxyethylene alkyl ether sodium phosphate are dripped into the pressure-resistant polymerization reactor within 6 hours; a polymerization reaction is carried out at 50° C. until the system pressure does not change and the polymerization conversion rate is 98wt%; after the polymerization is completed, the unreacted butadiene monomer in the system is removed to obtain a rubber core aqueous latex containing polybutadiene rubber as the main component;
[0107] (2) Preparation of graft copolymer emulsion
[0108] Based on 100 parts by weight of the total solid content of the rubber core aqueous latex obtained in step (1), 71 parts by weight of the solid content of the rubber core aqueous latex obtained in step (1) are added to a pressure-resistant polymerization reactor equipped with a stirrer. At the same time, the gas in the reactor is replaced with nitrogen to remove oxygen, and the reaction raw materials are added under stirring at 60° C. to carry out polymerization reaction, namely: (a) 22 parts of methyl methacrylate (MMA) and 7 parts of styrene (St) are continuously added to the reactor over 60 minutes, and (b) 0.07 parts of tert-butyl hydroperoxide (BHP) and 0.1 parts of sodium formaldehyde sulfoxylate (SFS) are all added to the reactor over 2 hours; and the addition of MMA and St is started simultaneously with the addition of BHP and SFS; after the addition of all the amounts of BHP and SFS is completed, the reaction solution is further kept at 60° C. for 1 hour to terminate the polymerization reaction, thereby obtaining a graft copolymer emulsion having a core-shell structure;
[0109] (3) Flocculation and drying
[0110] Based on 100 parts by weight of the solid content of the graft copolymer emulsion with a core-shell structure obtained in step (2), 2 parts of IRGANOX 1076 [n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate] as a phenolic antioxidant are added to the graft copolymer emulsion obtained in step (2), and then flocculation and coagulation are carried out at 52° C. with 790 parts of calcium chloride aqueous solution (concentration of 0.14wt%), followed by water washing, and then drying the dehydrated material at 45° C. until its water content is less than 1wt%, to obtain a powdery graft copolymer-5.
[0111] Embodiment 6:
[0112] The preparation method of the impact modifier comprises the following steps:
[0113] (1) Preparation of butadiene rubber core polymer emulsion
[0114] In a pressure-resistant polymerization reactor with a stirrer, stirring is started and 200 parts of pure water, 0.3 parts of tripotassium phosphate, 0.0012 parts of ferrous sulfate heptahydrate, 0.008 parts of disodium ethylenediaminetetraacetic acid (EDTA), 0.03 parts of polyoxyethylene alkyl ether sodium phosphate, and 2.5 parts of functional monomer (S-2) are added; at the same time, the gas inside the pressure-resistant polymerization reactor is evacuated and replaced with nitrogen to fully remove oxygen; then, 97.5 parts of butadiene (Bd), 0.05 parts of sodium formaldehyde sulfoxylate (SFS) and 0.2 parts of isopropyl hydrogen peroxide (CHP) are added into the pressure-resistant polymerization reactor; and 1.4 parts of polyoxyethylene alkyl ether sodium phosphate are dripped into the pressure-resistant polymerization reactor within 6 hours; a polymerization reaction is carried out at 50° C. until the system pressure does not change and the polymerization conversion rate is 98wt%; after the polymerization is completed, the unreacted butadiene monomer in the system is removed to obtain a rubber core aqueous latex containing polybutadiene rubber as the main component;
[0115] (2) Preparation of graft copolymer emulsion
[0116] Based on 100 parts by weight of the total solid content of the rubber core aqueous latex obtained in step (1), 71 parts by weight of the solid content of the rubber core aqueous latex obtained in step (1) are added to a pressure-resistant polymerization reactor equipped with a stirrer. At the same time, the gas in the reactor is replaced with nitrogen to remove oxygen. The reaction raw materials are added under stirring at 60° C. to carry out polymerization reaction, namely: (a) 22 parts of methyl methacrylate (MMA) and 7 parts of styrene (St) are continuously added to the reactor over 60 minutes, and (b) 0.07 parts of tert-butyl hydroperoxide (BHP) and 0.1 parts of sodium formaldehyde sulfoxylate (SFS) are all added to the reactor over 2 hours; and the addition of MMA and St is started simultaneously with the addition of BHP and SFS; after the addition of all the amounts of BHP and SFS is completed, the reaction solution is further kept at 60° C. for 1 hour to terminate the polymerization reaction, thereby obtaining a graft copolymer emulsion having a core-shell structure;
[0117] (3) Flocculation and drying
[0118] Based on 100 parts by weight of the solid content of the graft copolymer emulsion with a core-shell structure obtained in step (2), 2 parts of IRGANOX 1076 [n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate] as a phenolic antioxidant are added to the graft copolymer emulsion obtained in step (2), and then flocculation and coagulation are carried out at 48° C. with 780 parts of calcium chloride aqueous solution (concentration of 0.28wt%), followed by water washing, and then drying the dehydrated material at 45° C. until its water content is less than 1wt%, to obtain a powdery graft copolymer-6.
[0119] Comparative Example 1:
[0120] The preparation method of the impact modifier comprises the following steps:
[0121] (1) Preparation of butadiene rubber core polymer emulsion
[0122] In a pressure-resistant polymerization reactor with a stirrer, stirring is started and 200 parts of pure water, 0.3 parts of tripotassium phosphate, 0.0012 parts of ferrous sulfate heptahydrate, 0.008 parts of disodium ethylenediaminetetraacetic acid (EDTA), and 0.03 parts of polyoxyethylene alkyl ether sodium phosphate are added; at the same time, the gas inside the pressure-resistant polymerization reactor is evacuated and replaced with nitrogen to fully remove oxygen; then, 100 parts of butadiene (Bd), 0.05 parts of sodium formaldehyde sulfoxylate (SFS) and 0.2 parts of isopropyl hydrogen peroxide (CHP) are added into the pressure-resistant polymerization reactor; and 1.4 parts of polyoxyethylene alkyl ether sodium phosphate are dripped into the pressure-resistant polymerization reactor within 6 hours; a polymerization reaction is carried out at 50° C. until the system pressure does not change and the polymerization conversion rate is 98wt%; after the polymerization is completed, the unreacted butadiene monomer in the system is removed to obtain a rubber core aqueous latex containing polybutadiene rubber as the main component;
[0123] (2) Preparation of graft copolymer emulsion
[0124] Based on 100 parts by weight of the total solid content of the rubber core aqueous latex obtained in step (1), 71 parts by weight of the solid content of the rubber core aqueous latex obtained in step (1) are added into a pressure-resistant polymerization reactor equipped with a stirrer, and the gas in the reactor is replaced with nitrogen to remove oxygen; the reaction raw materials are added under stirring at 60° C. to carry out polymerization reaction, namely: (a) 22 parts of methyl methacrylate (MMA) and 7 parts of styrene (St) are continuously added into the reactor over 60 minutes, and (b) 0.07 parts of tert-butyl hydroperoxide (BHP) and 0.1 parts of sodium formaldehyde sulfoxylate (SFS) are all added into the reactor over 2 hours; and the addition of MMA and St is started simultaneously with the addition of BHP and SFS; after the addition of all the amounts of BHP and SFS is completed, the reaction solution is further kept at 60° C. for 1 hour to terminate the polymerization reaction, thereby obtaining a graft copolymer emulsion having a core-shell structure;
[0125] (3) Flocculation and drying
[0126] Based on 100 parts by weight of the solid content of the graft copolymer emulsion with a core-shell structure obtained in step (2), 2 parts of IRGANOX 1076 [n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate] as a phenolic antioxidant are added to the graft copolymer emulsion obtained in step (2), and then flocculation and coagulation are carried out at 45° C. with 790 parts of calcium chloride aqueous solution (concentration of 0.25wt%), followed by water washing, and then drying the dehydrated material at 45° C. until its water content is less than 1wt%, to obtain a powdery graft copolymer-1'.
[0127] Comparative Example 2:
[0128] The preparation method of the impact modifier comprises the following steps:
[0129] (1) Preparation of butadiene rubber core polymer emulsion
[0130] In a pressure-resistant polymerization reactor with a stirrer, stirring is started and 200 parts of pure water, 0.3 parts of tripotassium phosphate, 0.0012 parts of ferrous sulfate heptahydrate, 0.008 parts of disodium ethylenediaminetetraacetic acid (EDTA), 0.03 parts of polyoxyethylene alkyl ether sodium phosphate, and 20 parts of functional monomer (S-2) are added; at the same time, the gas inside the pressure-resistant polymerization reactor is evacuated and replaced with nitrogen to fully remove oxygen; then, 80 parts of butadiene (Bd), 0.05 parts of sodium formaldehyde sulfoxylate (SFS) and 0.2 parts of isopropyl hydrogen peroxide (CHP) are added into the pressure-resistant polymerization reactor; and 1.4 parts of polyoxyethylene alkyl ether sodium phosphate are dripped into the pressure-resistant polymerization reactor within 6 hours; a polymerization reaction is carried out at 50° C. until the system pressure does not change and the polymerization conversion rate is 98wt%; after the polymerization is completed, the unreacted butadiene monomer in the system is removed to obtain a rubber core aqueous latex containing polybutadiene rubber as the main component.
[0131] (2) Preparation of graft copolymer emulsion
[0132] Based on 100 parts by weight of the total solid content of the rubber core aqueous latex obtained in step (1), 71 parts by weight of the solid content of the rubber core aqueous latex obtained in step (1) are added into a pressure-resistant polymerization reactor equipped with a stirrer, and the gas in the reactor is replaced with nitrogen to remove oxygen; the reaction raw materials are added under stirring at 60° C. to carry out polymerization reaction, namely: (a) 22 parts of methyl methacrylate (MMA) and 7 parts of styrene (St) are continuously added into the reactor over 60 minutes, and (b) 0.07 parts of tert-butyl hydroperoxide (BHP) and 0.1 parts of sodium formaldehyde sulfoxylate (SFS) are all added into the reactor over 2 hours; and the addition of MMA and St is started simultaneously with the addition of BHP and SFS; after the addition of all the amounts of BHP and SFS is completed, the reaction solution is further kept at 60° C. for 1 hour to terminate the polymerization reaction, thereby obtaining a graft copolymer emulsion having a core-shell structure;
[0133] (3) Flocculation and drying
[0134] Based on 100 parts by weight of the solid content of the graft copolymer emulsion with a core-shell structure obtained in step (2), 2 parts of IRGANOX 1076 [n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate] as a phenolic antioxidant are added to the graft copolymer emulsion obtained in step (2), and then flocculation and coagulation are carried out at 50° C. with 800 parts of calcium chloride aqueous solution (concentration of 0.2wt%), followed by water washing, and then drying the dehydrated material at 45° C. until its water content is less than 1wt%, to obtain a powdery graft copolymer-2'.
[0135] Performance Test:
[0136] The powdery graft copolymer (impact modifier) prepared in each embodiment and comparative example is blended with A1105 polycarbonate resin obtained from Wanhua Chemical; in the blend, the content of the powdery graft copolymer accounts for 5wt%. Then, for each group of blends obtained, the impact strength is tested according to ISO 180 / ASTM D256, the low temperature (-30°C) notched impact is tested (according to ISO 180 / ASTM D256), the 50W vertical burning test (1.5mm) (UL94), and the color difference of the sample obtained after injection molding is tested according to ASTM-E1925. The performance test results of the powdery graft copolymer (impact modifier) prepared in each embodiment and comparative example and its application in resin are shown in Table 1 below.
[0137] Table 1 Performance test results
[0138]
[0139]
[0140] It can be seen from the results in Table 1 that the functional monomers containing silicon and carbamate are selected for polymerization in the impact modifier formula obtained in each embodiment, which can improve the flame retardant and impact resistance of the impact modifier and its application in resin; at the same time, each test sample can maintain a low color difference value under high temperature processing conditions of 320°C, indicating that the obtained impact modifier has good heat resistance.
[0141] In Comparative Example 1, no functional monomer containing silicon and carbamate was added, and the resulting impact modifier and its application to the resin had very poor flame retardant properties and poor impact resistance. Although functional monomer containing silicon and carbamate was added in Comparative Example 2, the amount added was too large, and the resulting impact modifier and its application to the resin had greatly improved flame retardant properties, but poor impact resistance.
[0142] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the spirit of the present invention.
Claims
1. A novel impact modifier, characterized in that: It is a product prepared by a modifier composition; based on the total weight of the modifier composition, the modifier composition includes the following components: A) at least one butadiene component containing diene groups, 40-95 wt%, preferably 51.5-79.5 wt%; B) at least one alkyl (meth)acrylate, 1-30 wt %, preferably 4-25 wt %; C) at least one vinyl aromatic monomer, 1-30 wt%, preferably 1.6-25 wt%; D) at least one functional monomer containing carbamate and long carbon silicon chain, 0.1-10wt%, preferably 0.7-7wt%; E) initiator, 0.01-1 wt%, preferably 0.02-0.5 wt%; F) emulsifier, 0.2-5wt%, preferably 0.5-3wt%; G) pH buffer, 0.01-1 wt%, preferably 0.03-0.5 wt%.
2. The novel impact modifier according to claim 1, characterized in that: The butadiene component containing a diene group is selected from one or more of 1,3-butadiene, isoprene and chloroprene, preferably 1,3-butadiene.
3. The novel impact modifier according to claim 1 or 2, characterized in that: The alkyl (meth)acrylate is selected from one or more of methyl acrylate, methyl methacrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isopropyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate and isooctyl (meth)acrylate, preferably methyl methacrylate and / or n-butyl acrylate.
4. The novel impact modifier according to any one of claims 1 to 3, characterized in that: The vinyl aromatic monomer is one or more selected from styrene, 2-methylstyrene, 4-methylstyrene, 2-(n-butyl)styrene, 4-(n-butyl)styrene, 4-(n-decyl)styrene and divinylbenzene, preferably styrene.
5. The novel impact modifier according to any one of claims 1 to 4, characterized in that: The functional monomer containing carbamate and long carbon silicon chain is a product obtained by reacting ethyl isocyanate (alkyl) acrylate with hydroxyl-terminated polydimethylsiloxane; The molecular weight of the functional monomer containing carbamate and long carbon silicon chain is 300-8000 g / mol, preferably 500-2000 g / mol.
6. The novel impact modifier according to any one of claims 1 to 5, characterized in that: The initiator is selected from one or more of peroxides, azo initiators and redox system initiators, preferably a redox system initiator.
7. The novel impact modifier according to any one of claims 1 to 6, characterized in that: The emulsifier is selected from one or more of anionic surfactants, nonionic surfactants, anionic nonionic surfactants and cationic surfactants, preferably anionic surfactants and / or anionic nonionic surfactants; The pH buffer is selected from one or more of sodium carbonate, sodium bicarbonate, tripotassium phosphate, potassium carbonate, potassium bicarbonate and sodium dihydrogen phosphate, preferably tripotassium phosphate.
8. The method for preparing the novel impact modifier according to any one of claims 1 to 7, characterized in that: The steps include: (1) adding a rubber core layer monomer, a pH buffer, an initiator and an emulsifier accounting for 2wt%-100wt% of the total amount of the emulsifier into a reaction kettle, stirring and heating; then adding the remaining emulsifier into the reaction kettle within 2-10 hours, reacting until the system pressure remains unchanged, to obtain a rubber core emulsion; the rubber core layer monomer includes a butadiene component containing a diene group, a functional monomer containing a carbamate and a long carbon silicon chain, and an optional vinyl aromatic monomer; (2) adding an initiator and a shell monomer to the rubber core emulsion, stirring and heating, and keeping the temperature for 1-3 hours after the addition is completed to obtain a grafted emulsion with a core-shell structure; the shell monomer includes an alkyl (meth)acrylate and a vinyl aromatic monomer; (3) flocculating and drying the emulsion obtained in step (2) to obtain a novel impact modifier powder.
9. The preparation method according to claim 8, characterized in that: The reaction temperature in step (1) is 50-70°C; The reaction temperature in step (2) is 60-80°C; The flocculation temperature in step (3) is 25-60° C.; the flocculant is selected from an inorganic acid or a metal salt; During the drying process of step (3), the material is dried until the moisture content is less than or equal to 1%.
10. Use of the novel impact modifier according to any one of claims 1 to 7 or the novel impact modifier prepared by the preparation method according to any one of claims 8 to 9 in polycarbonate plastics.
Citation Information
Patent Citations
High-silicon-content organic silicon-polyurethane-acrylate composite coating agent and preparation method thereof
CN102585650A
Preparation method of graft copolymer with excellent impact strength
CN112759717A
Preparation method of environment-friendly low-smoke flame-retardant high-impact polystyrene
CN113444333A
Methyl methacrylate-butadiene-styrene impact reinforcing agent comprising alkoxy silane compound, preparation method thereof and thermoplastic resin comprising the same
KR1020150057977A
Compounds having a polymerizable acylurethane structure, and their production and process of using