Method for continuously and stably producing polymer polyol
By detecting and extracting the water content of the isopropyl alcohol solution, and performing appropriate extraction and polymerization reactions during the polymer polyol production process, the problem of uneven particles caused by excessive water content in the polymer polyol production is solved. The continuous, stable and efficient production of polymer polyols is achieved.
Patent Information
- Application Number
- CN202411061188.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-18
AI Technical Summary
In the production process of polymer polyols, the increased water content in recycled isopropyl alcohol results in uneven product particles, affecting product quality and production continuity. Existing solutions increase production and hazardous waste treatment costs.
By detecting the water content of the recovered isopropyl alcohol solution, if it exceeds 12%, extract and stir it with styrene, let it stand and then layer it to reduce the water content, and add the required amount of acrylonitrile and polyether during the polymerization reaction. and initiator for polymerization reaction, followed by multiple flash evaporations and filtration to ensure product quality and production continuity.
It realizes the continuous and stable production of polymer polyol, reduces the water content in recycled isopropyl alcohol, ensures that the product particles are uniform and the size is less than 75 μm, and improves production efficiency and product quality.
Smart Images

Figure BDA0004977901510000031
Abstract
Description
Technical Field
[0001] The invention relates to a method for continuous and stable production of polymer polyols. Background Art
[0002] In the production process of polymer polyols, vinyl-containing macromolecular monomer polyethers and chain transfer agents are usually added during mixing. The chain transfer agent plays a role in controlling the molecular weight of the polymer during the synthesis process, reducing the phenomenon of product interconnection and increasing the stability of the polymer polyol. It is an indispensable part of the polymerization process. The commonly used chain transfer agent is isopropyl alcohol.
[0003] After the polymer polyol material arrives at the flash evaporation system, the isopropyl alcohol in the material will be recovered through the recovery system for secondary utilization. However, while recovering the isopropyl alcohol, the removed water and other components will also enter the isopropyl alcohol recovery system, resulting in a higher water content in the recovered isopropyl alcohol. When the water content in the recovered isopropyl alcohol exceeds 12%, a large number of uneven particles will appear in the polymer polyol, affecting the quality of the product.
[0004] Since the boiling points of the components in the isopropanol aqueous solution are close, it is difficult to remove water from the isopropanol solution through the distillation process. The existing process is to treat the high-water content recovered isopropanol as hazardous waste and then add fresh isopropanol to the production system, but this will increase the cost of production and hazardous waste treatment.
[0005] Patent CN 114195957A discloses a method for preparing polymer polyols, which controls the water content by adding an appropriate amount of fresh isopropanol to the recycled isopropanol, but this will increase production costs and cause the production line to be discontinuous. Therefore, a process is urgently needed in industrial production to produce polymer polyols continuously and efficiently. Summary of the invention
[0006] The technical problem to be solved by the present invention is that, in the prior art, during the production process of polymer polyols, macromolecular monomers and isopropanol need to be added, and after a series of reactions, the water content in the recovered isopropanol solution increases, resulting in a large number of uneven particles in the polymer polyols, leading to product instability, affecting its quality and performance, and also affecting the production capacity. A new continuous and stable production of polymer polyols is provided, and the method has the advantages of stable product quality, continuous production of polymer polyols and efficient production.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: a method for continuous and stable production of polymer polyols, comprising the following steps:
[0008] (1) After the polymer polyol material passes through the flash tank, most of the isopropanol and unreacted styrene and acrylonitrile monomers will be evaporated and pumped into a recovery tank for recycling and reuse; the mixed recovery solution containing styrene, acrylonitrile, isopropanol and water in the recovery tank is recorded as solution A, and the instrument automatically detects the water content in solution A. When the water content in solution A is less than 12%, it can directly enter the prepolymer production line for production; when the water content in solution A is greater than 12%, it is mixed with the re-added styrene solution B at a mass ratio of 1:0.8-1.4 and stirred for 1-20 minutes to obtain solution C.
[0009] (2) Solution C is allowed to stand for 30 to 75 minutes, and the lower aqueous phase is an isopropanol solution containing a small amount of styrene, which is sent to sewage treatment; the upper layer is an oil phase containing acrylonitrile, styrene, isopropanol and a water content of less than 12%;
[0010] (3) After analyzing the content of each component in the oil phase, the required amount of acrylonitrile, polyether and initiator are added to the oil phase, and the mixed liquid is pumped into the reaction system at a flow rate of 3 to 5 t / h, and a polymerization reaction is carried out at a temperature of 110 to 140° C. and a pressure of 0.4 to 0.5 MPa, wherein the required amount refers to the amount missing calculated according to the process ratio;
[0011] (4) After the polymerization reaction is completed, a polymer polyol material is obtained, which is flash-evaporated in a flash tank under a vacuum state, and the evaporated styrene, isopropanol, and acrylonitrile monomers are condensed and then enter a recovery tank;
[0012] (5) The material after the secondary flash evaporation enters the third flash tank. In order to make the monomer in the material evaporate more cleanly, the third flash tank is heated at 90 to 100 m 3 / h flow rate of water vapor for bubbling to improve the flash evaporation effect of the third flash tank;
[0013] (6) The material from which the monomer is removed in the third flash tank passes through a cooler and enters an intermediate tank. After the required antioxidant is added, the material is fully circulated and homogenized. The polymer polyol in the intermediate tank is then pumped into a filter for filtration to separate the solid particles in the material from the liquid. The material in the filtrate tank is then pumped into a finished product tank.
[0014] In the above technical solution, when the water content in solution A in step (1) is greater than 10%, styrene can be used for extraction.
[0015] In the above technical solution, the mass ratio of the mixed recovery solution A to the re-added styrene solution B in step (1) is 1:1.3.
[0016] In the above technical solution, the stirring time of the mixed recovery solution A and the re-added styrene solution B in step (1) is 10 minutes.
[0017] In the above technical solution, in step (2), the standing time of solution C is 45 to 60 minutes.
[0018] In the above technical solution, the polymerization reaction temperature in step (3) is 125-130°C.
[0019] In the above technical solution, the polymerization reaction pressure in step (3) is 0.43-0.45 MPa.
[0020] The invention provides a method for continuously and stably producing a polymer polyol. When the water content in the recovered isopropanol solution obtained after flash evaporation is greater than 12%, the recovered isopropanol solution is fully stirred with styrene and allowed to stand, and the water and oil layers are separated. The lower water phase is discharged through a drainage pipeline, thereby reducing the water content in the recovered isopropanol and obtaining an oil phase with a water content of less than 12%. After the remaining required raw materials are added to the oil phase, the production process is continued, so that particles in the product are uniform and can be continuously and stably produced. When the ratio of the recovered isopropanol solution to the styrene extraction is 1:1.3, the water content of the oil phase can be reduced to 2.1%. The inventor surprisingly found that the particles in the polymer polyol are uniform and have a size of less than 75 μm, thereby realizing continuous and efficient production, thereby achieving stable product quality and achieving better technical effects. DETAILED DESCRIPTION
[0021] The present invention is further described below in conjunction with specific embodiments.
[0022] Example 1
[0023] The method for continuous and stable production of a polymer polyol according to the present invention comprises the following steps:
[0024] (1) The instrument automatically detects that the water content in the recovered isopropanol solution is greater than 12%, and then determines that the mass ratio of the recovered isopropanol solution to the styrene extraction is 1:1.3, and feeds 10 tons of the recovered isopropanol solution and 13 tons of styrene simultaneously and stirs for 10 minutes;
[0025] (2) The mixed solution was allowed to stand for 45 min to separate the water and oil phases, and the lower aqueous phase was discharged;
[0026] (3) analyzing that the water content in the oil phase is less than 12%, further analyzing the components, and then adding the amount of acrylonitrile, polyether and initiator that are missing in the process ratio to carry out polymerization reaction;
[0027] (4) After flash evaporation, the required amount of antioxidant is added and circulated and homogenized, and then the mixture is filtered through a filter, and finally the filtrate is pumped into a finished product tank to obtain the finished product.
[0028] Embodiments 2 to 7
[0029] The experimental steps of Examples 2 to 7 are consistent with those of Example 1, except that the extraction mass ratios of the recovered isopropanol solution and the added styrene solution are different. Specific experimental data are shown in Table 1.
[0030] Table 1 Extraction mass ratio and experimental data of recovered isopropanol solution and added styrene solution of Examples 1 to 7
[0031]
[0032] As can be seen from Table 1, the embodiments of the present invention can achieve the water content of the recovered isopropanol solution to be less than 12% and the particle size in the product to be less than 75μm, especially when the extraction ratio of the recovered isopropanol solution and the added styrene solution is 1:1.3, the water content in the solution can be less than 2.5%; in the traditional production site, if the water content in the recovered isopropanol solution exceeds 12%, a large number of uneven particles will appear when the product is filtered, which slows down the filtration speed and affects the product quality and production capacity. The present invention greatly reduces the water content in the recovered isopropanol solution. In summary, the production method of a polymer polyol described in the present invention has the advantages of stable product quality, continuous production of polymer polyols and efficient production.
Claims
1. A method for continuous and stable production of polymer polyols, comprising the following steps: (1) After the polymer polyol material passes through the flash tank, most of the isopropanol and unreacted styrene and acrylonitrile monomers will be evaporated and pumped into the recovery tank for recycling and reuse; the mixed recovery solution containing styrene, acrylonitrile, isopropanol and water in the recovery tank is recorded as solution A, and the instrument automatically detects the water content in solution A. When the water content in solution A is less than 12%, it can directly enter the prepolymer production line for production; when the water content in solution A is greater than 12%, it is mixed with the re-added styrene solution B at a mass ratio of 1:0.8-1.4 and stirred for 1-20 minutes to obtain solution C; (2) Solution C is allowed to stand for 30 to 75 minutes, and the lower aqueous phase is an isopropanol solution containing a small amount of styrene, which is sent to sewage treatment; the upper layer is an oil phase containing acrylonitrile, styrene, isopropanol and a water content of less than 12%; (3) After analyzing the content of each component in the oil phase, the required amount of acrylonitrile, polyether and initiator are added to the oil phase, and the mixed liquid is pumped into the reaction system at a flow rate of 3 to 5 t / h, and a polymerization reaction is carried out at a temperature of 110 to 140° C. and a pressure of 0.4 to 0.5 MPa, wherein the required amount refers to the amount missing for preparing the polymer polyol calculated according to the process ratio; (4) After the polymerization reaction is completed, a polymer polyol material is obtained, which is flash-evaporated in a flash tank under a vacuum state, and the evaporated styrene, isopropanol, and acrylonitrile monomers are condensed and then enter a recovery tank; (5) The material after the secondary flash evaporation enters the third flash tank. In order to make the monomer in the material evaporate more cleanly, the third flash tank is heated at 90 to 100 m 3 / h flow rate of water vapor for bubbling to improve the flash evaporation effect of the third flash tank; (6) The material from which the monomer is removed in the third flash tank passes through a cooler and enters an intermediate tank. After adding the required amount of antioxidant, the material is fully circulated and homogenized. The polymer polyol in the intermediate tank is then pumped into a filter for filtration. The solid particles in the material are separated from the solid and liquid and then enter the filtrate tank. The material in the filtrate tank is then pumped into a finished product tank.
2. The method according to claim 1, characterized in that When the water content in solution A in step (1) is greater than 10%, styrene can be used for extraction.
3. The method according to claim 1, characterized in that In the step (1), the mass ratio of the mixed recovery solution A to the re-added styrene solution B is 1:1.
3.
4. The method according to claim 1, characterized in that: The stirring time of mixing the recovered solution A and the newly added styrene solution B in the step (1) is 5 to 15 minutes.
5. The method according to claim 1, characterized in that The standing time of solution C in step (2) is 45 to 60 minutes.
6. The method according to claim 1, characterized in that The polymerization reaction temperature in step (3) is 125-130°C.
7. The method according to claim 1, characterized in that The polymerization reaction pressure in step (3) is 0.43-0.45 MPa.
Citation Information
Patent Citations
Preparation method of polymer polyol
CN114195957A