Water-based polyurethane emulsion for direct coating foaming of sneaker leather and sneaker leather

By using a direct-coating foaming process and a specific combination of water-based polyurethane emulsion in sports shoe leather, the problem of insufficient strength and folding resistance of sports shoe leather is solved, achieving efficient peel strength and normal temperature folding resistance, and avoiding the need for drying cracking, meeting environmental and performance requirements.

CN118791701AActive Publication Date: 2024-10-18XUCHUAN CHEM SUZHOU
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411083239.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-18
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

Solvent-based polyurethane resin is still used in the field of sports shoe leather, resulting in slow progress in environmental protection. Water-based polyurethane has a small molecular weight and low strength. It is difficult to improve the peel strength and normal temperature folding resistance, and is prone to drying cracking problems.

Method used

The direct coating foaming process is used to produce water-based polyurethane emulsion for sports shoe leather. The raw materials include diisocyanate, polyol compounds, chain extenders, neutralizers and catalysts. The combination of water chain extender and N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide improves the crack resistance and adhesion of polyurethane, and forms hydrogen bonds to enhance peel strength and folding resistance. performance.

Benefits of technology

It achieves better peel strength and normal temperature folding resistance of sports shoe leather, avoids cracking problems during the drying process, and meets the requirements of environmental protection and excellent performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004984408910000061
    Figure BDA0004984408910000061
Patent Text Reader

Abstract

The invention discloses a waterborne polyurethane emulsion for direct coating foaming of sports shoe leather. The waterborne polyurethane emulsion is prepared from the following raw materials: diisocyanate, a polyol compound, a chain extender, a neutralizer, a catalyst and water, wherein the chain extender is prepared from single-ended dihydroxy polyether with a Y-shaped structure, a hydrophilic chain extender containing carboxyl, a micromolecular dihydric alcohol chain extender, an amine chain extender and N, N-bis (2-ethoxyl)-3-aminopropionyl glycinamide. The invention further discloses a preparation method of the waterborne polyurethane emulsion for direct coating foaming of the sports shoe leather. The invention further discloses sports shoe leather which comprises non-woven fabric and foaming emulsion, and raw materials of the foaming emulsion comprise a thickening agent, a foaming agent, a curing agent and the waterborne polyurethane emulsion. The invention also discloses a preparation method of the sports shoe leather. The sports shoe leather has good peel strength and normal-temperature folding resistance, and meanwhile the problem of drying cracking is not prone to occurring in the production and processing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of microfiber leather, in particular to a direct-coating foaming water-based polyurethane emulsion for sports shoe leather, and sports shoe leather. Background Art

[0002] Since the 20th century, synthetic leather products have been widely used in civil fields such as sofas, bags, shoes, electronic packaging, home building materials, etc. due to their excellent physical and mechanical properties and colorful appearance and patterns. However, traditional synthetic leather products still use a large amount of toxic and harmful solvents such as DMF, butanone, and ethyl acetate.

[0003] In the context of environmental protection and green manufacturing, the synthetic leather industry has also ushered in a new generation of environmentally friendly synthetic leather products. At present, sofa furniture synthetic leather is prepared by solvent-free, which has excellent performance, low temperature and environmental protection. Luggage and clothing leather have lower requirements for physical properties, and are generally prepared by water-based polyurethane foaming process, which has also completed the green environmental protection of the product. At present, only the sports shoe leather field in the market continues to use solvent-based polyurethane resin and adopts wet process for processing.

[0004] With people's demand for environmental protection, in the field of sports shoe leather, there are also sports shoe leathers prepared by solvent-free method, but there are problems of glue brushing and injection molding delamination in the later stage of shoe making. When using water-based polyurethane to produce sports shoe leather, it is difficult to break through the peel strength and room temperature folding resistance due to the small molecular weight and low strength of water-based polyurethane. At the same time, sports shoe leather generally has a high coating amount and is prone to cracking during the drying process. Therefore, the environmental protection of sports shoe leather has been slow. It is necessary to provide a water-based polyurethane emulsion that is both environmentally friendly and can meet the requirements of sports shoe leather. Summary of the invention

[0005] Based on the technical problems existing in the background technology, the present invention proposes a water-based polyurethane emulsion for direct coating and foaming of sports shoe leather, and sports shoe leather. The water-based polyurethane emulsion of the present invention adopts a direct coating and foaming process to produce sports shoe leather, so that the sports shoe leather not only has good peel strength and folding resistance at room temperature, but also is not prone to drying cracking during the production and processing process.

[0006] The invention provides a water-based polyurethane emulsion for direct foaming of sports shoe leather, the raw materials of which include: diisocyanate, polyol compound, chain extender, neutralizer, catalyst and water;

[0007] The chain extenders include: single-ended dihydroxy polyether with a Y-shaped structure, carboxyl-containing hydrophilic chain extenders, small molecule diol chain extenders, amine chain extenders, and N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide.

[0008] Preferably, the single-terminated dihydroxy polyether with a Y-shaped structure is YmerN120.

[0009] The single-terminal dihydroxy polyether with a Y-shaped structure is a nonionic hydrophilic chain extender.

[0010] The above YmerN120 was purchased from Swedish Pasto Group.

[0011] Preferably, the carboxyl-containing hydrophilic chain extender is one or both of dimethylolpropionic acid and dihydroxybutyric acid.

[0012] Preferably, the amine chain extender is one or more of ethylenediamine, isophoronediamine, diethylenetriamine, and hydroxyethylethylenediamine.

[0013] Preferably, the amine chain extender is a mixture of ethylenediamine and hydroxyethylethylenediamine in a weight ratio of 3-4:1.

[0014] Preferably, the polyol compound is one or both of polytetramethylene glycol and adipic acid-based polyester polyol.

[0015] Preferably, the polyol compound is a mixture of polytetrahydrofuran diol and adipic acid-based polyester polyol in a weight ratio of 2-2.2:1.

[0016] Preferably, the diisocyanate is an aliphatic diisocyanate.

[0017] Preferably, the small molecule diol chain extender is one or more of ethylene glycol, 1,4-butanediol, and neopentyl glycol.

[0018] Preferably, the neutralizing agent is one or both of triethylamine and triethanolamine.

[0019] Preferably, the weight ratio of the single-terminal bishydroxy polyether with a Y-shaped structure to the carboxyl-containing hydrophilic chain extender is 0.5-0.9:1.

[0020] Preferably, the weight ratio of the carboxyl-containing hydrophilic chain extender, the amine chain extender, N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide, and the small molecule diol chain extender is 1:0.6-0.9:0.14-0.2:0.3-0.5.

[0021] Preferably, the weight ratio of diisocyanate to polyol compound is 6-9:17-27.

[0022] Preferably, the weight ratio of diisocyanate to chain extender is 6-9:1-2.1.

[0023] Preferably, the weight ratio of diisocyanate to catalyst is 6-9:0.002-0.005.

[0024] Preferably, the weight ratio of diisocyanate to water is 6-9:30-48.

[0025] Preferably, the weight ratio of diisocyanate to neutralizer is 6-9:0.2-0.5.

[0026] The raw materials of the above-mentioned water-based polyurethane emulsion for direct foaming of sports shoe leather may also include: antioxidants, etc. The weight ratio of diisocyanate to antioxidant is 6-9:0.016-0.03.

[0027] The aliphatic diisocyanate may be one or more of isophorone diisocyanate, hexamethylene diisocyanate, and dicyclohexylmethane diisocyanate. The adipic acid-based polyester polyol may be adipic acid neopentyl glycol polyester polyol or the like.

[0028] The catalyst may be an organic bismuth catalyst MB20; the antioxidant may be one or both of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 2,2'-methylenebis(4-methyl-6-tert-butylphenol).

[0029] The above-mentioned N,N-bis(2-hydroxyethyl)-3-aminopropionyl glycinamide can be purchased from the market, or can be prepared by Michael addition reaction of acryloyl glycinamide and diethanolamine. The specific preparation steps include: dissolving acryloyl glycinamide in a mixed solvent of water and methanol, adding a methanol solution of diethanolamine, stirring at 35-45° C. for 20-30 hours, removing water and methanol, washing the remaining solid with acetone until the pH is neutral, and drying to obtain N,N-bis(2-hydroxyethyl)-3-aminopropionyl glycinamide. Preferably, the molar ratio of acryloyl glycinamide to diethanolamine is 1-1.2:1.

[0030] The present invention also proposes a method for preparing the above-mentioned water-based polyurethane emulsion for direct coating and foaming of sports shoe leather, comprising the following steps: in an inert gas atmosphere, a polyol compound, a single-ended dihydroxy polyether with a Y-shaped structure, a diisocyanate, and a catalyst are mixed and reacted once, then a carboxyl-containing hydrophilic chain extender, a small molecule diol chain extender, and N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide are added to carry out a secondary reaction, an organic solvent is added to reduce viscosity, a neutralizer is added to carry out a neutralization reaction, water is added for emulsification, an amine chain extender is added, a tertiary reaction is carried out, and the organic solvent is removed to obtain the water-based polyurethane emulsion for direct coating and foaming of sports shoe leather.

[0031] The above-mentioned diisocyanate, polyol compound, chain extender, catalyst, neutralizer and antioxidant are all dried and dehydrated before use.

[0032] Preferably, the reaction is carried out at 90-95°C for 1.5-2.5 hours.

[0033] Preferably, the secondary reaction is carried out at 60-65° C. for 1.5-2.5 h.

[0034] Preferably, the neutralization reaction is carried out at 20-40°C for 5-15 min.

[0035] Preferably, the reaction is carried out three times at 20-40°C for 1.5-2.5 h.

[0036] The present invention also provides a sports shoe leather, comprising: non-woven fabric and foaming emulsion, wherein the raw materials of the foaming emulsion include: thickener, foaming agent, curing agent and the above-mentioned water-based polyurethane emulsion.

[0037] Preferably, the weight ratio of the aqueous polyurethane emulsion, the thickener, the foaming agent and the curing agent is 100:0.3-0.5:3-5:0.8-1.2.

[0038] Preferably, the viscosity of the foaming emulsion at 25° C. is 15,000-20,000 CPS.

[0039] Preferably, the curing agent is one or more of a polymeric MDI curing agent, a polymeric IPDI curing agent, and a polymeric HDI curing agent.

[0040] The foaming emulsion may further contain fillers, color pastes, etc.; the fillers may be kaolin, etc.; the weight ratio of the aqueous polyurethane emulsion to the filler may be 100:4-6; the amount of the color paste added may be adjusted according to the color requirements of the sports shoe leather.

[0041] The thickener may be an associative waterborne polyurethane thickener, and the foaming agent may be a stearate foaming agent.

[0042] The present invention also provides a method for preparing the sports shoe leather, which comprises the following steps: mixing the raw materials of the foaming emulsion, coating it on the surface of the non-woven fabric, curing and drying it to obtain the sports shoe leather.

[0043] Preferably, the curing and drying procedure is: keeping at 85-95°C for 4-6 minutes, then keeping at 105-115°C for 4-6 minutes, and finally drying at 120-140°C.

[0044] 1. The present invention selects a single-ended bis-hydroxy polyether with a Y-shaped structure and a hydrophilic chain extender containing a carboxyl group to cooperate with each other. When the weight ratio of the two is 0.5-0.9:1, the problem that the emulsion is prone to cracking during the drying process can be avoided, and an appropriate amount of N, N-bis (2-hydroxyethyl) -3-aminopropionyl glycinamide is added as a chain extender to introduce aminopropionyl glycinamide groups, which can form hydrogen bonds between polyurethane molecular chains, improve the crack resistance and adhesion of polyurethane, and avoid the problems of cracking, degumming, and low peel strength of sports shoe leather; and the single-ended bis-hydroxy polyether with a Y-shaped structure, the hydrophilic chain extender containing a carboxyl group and N, N-bis (2-hydroxyethyl) -3-aminopropionyl glycinamide cooperate with each other, which can increase the baking temperature in the preparation process of sports shoe leather and relax the requirements of production operations.

[0045] 2. The present invention selects an amine chain extender with a hydroxyl group to cooperate with N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide, so that the polyurethane molecular chain has a small amount of reactive hydroxyl and amino groups, which can react with the curing agent in the foaming emulsion to increase the crosslinking density of the polyurethane, thereby greatly improving the peel strength and room-temperature folding resistance of the sports shoe leather; and the aminopropionylglycinamide group in N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide can form a urea group after reacting with the curing agent in the foaming emulsion, further improving the strength of hydrogen bond formation, and further improving the crack resistance, peel strength and room-temperature folding resistance.

[0046] The waterborne polyurethane emulsion of the present invention adopts a direct coating foaming process to produce sports shoe leather, so that the sports shoe leather not only has good peeling strength and room temperature folding resistance, but also is not prone to drying cracking during the production and processing process. DETAILED DESCRIPTION

[0047] The technical solution of the present invention is described in detail below through specific embodiments.

[0048] The raw material information is shown in Table 1.

[0049] Table 1 Raw material information

[0050]

[0051] Example 1

[0052] The invention discloses a water-based polyurethane emulsion for direct foaming of sports shoe leather. The raw materials thereof include, by weight: 78 g of HMDI, 20 g of IPDI, 200 g of PTMG-2000, 95 g of XCPP-2000N, 5 g of YmerN120, 7 g of DMPA, 3 g of ethylene glycol, 4.2 g of ethylenediamine, 1.2 g of hydroxyethylethylenediamine, 1 g of N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide, 0.05 g of an organic bismuth catalyst MB20, 0.3 g of an antioxidant I-1010, 5.27 g of a neutralizing agent triethylamine, and 520 g of deionized water.

[0053] The method for preparing the above-mentioned water-based polyurethane emulsion for direct foaming of sports shoe leather comprises the following steps:

[0054] Weigh each raw material by weight, add PTMG-2000, XCPP-2000N, YmerN120, and antioxidant I-1010 into a reaction bottle, dehydrate under reduced pressure at 110-120°C for 1-2h, then cool to 50°C, and then add HMDI and IPDI under nitrogen protection, keep warm at 90-95°C for 2h, and add organic bismuth catalyst MB20 during the reaction;

[0055] Then, DMPA, ethylene glycol, and N,N-di(2-hydroxyethyl)-3-aminopropionylglycinamide were added, and the mixture was kept warm at 60-65° C. for a secondary reaction for 2 hours. After the time was up, samples were taken, and the NCO% was determined by di-n-butylamine titration. When the NCO% was lower than the theoretical value, the reaction was stopped, and the mixture was cooled to 30-40° C.; then, 360 g of acetone was added to reduce the viscosity, and a neutralizing agent, triethylamine, was added, and a neutralization reaction was carried out at 30-40° C. for 10 minutes. Then, deionized water was added under high-speed stirring at 1000-1500 rpm for emulsification and dispersion to obtain an emulsion;

[0056] After adding ethylenediamine and hydroxyethylethylenediamine dropwise into the emulsion, the mixture was stirred at 30-40°C for three times for 2 hours; then, acetone was removed by distillation under reduced pressure to obtain a water-based polyurethane emulsion for direct foaming of sports shoe leather.

[0057] Example 2

[0058] The invention discloses a water-based polyurethane emulsion for direct foaming of sports shoe leather. The raw materials thereof include, by weight: 78 g of HMDI, 20 g of IPDI, 200 g of PTMG-2000, 95 g of XCPP-2000N, 3.2 g of YmerN120, 6 g of DMPA, 3 g of ethylene glycol, 4.2 g of ethylenediamine, 1.2 g of hydroxyethylethylenediamine, 1 g of N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide, 0.05 g of an organic bismuth catalyst MB20, 0.3 g of an antioxidant I-1010, 4.52 g of a neutralizing agent triethylamine, and 520 g of deionized water.

[0059] The preparation method of the above-mentioned water-based polyurethane emulsion for direct foaming of sports shoe leather is the same as that in Example 1.

[0060] Example 3

[0061] The invention discloses a water-based polyurethane emulsion for direct foaming of sports shoe leather. The raw materials thereof include, by weight: 88 g of HMDI, 15 g of IPDI, 200 g of PTMG-2000, 95 g of XCPP-2000N, 5.6 g of YmerN120, 8 g of DMPA, 3 g of ethylene glycol, 4.2 g of ethylenediamine, 1.2 g of hydroxyethylethylenediamine, 1.6 g of N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide, 0.05 g of an organic bismuth catalyst MB20, 0.3 g of an antioxidant I-1010, 4.52 g of a neutralizing agent triethylamine, and 520 g of deionized water.

[0062] The preparation method of the above-mentioned water-based polyurethane emulsion for direct foaming of sports shoe leather is the same as that in Example 1.

[0063] Comparative Example 1

[0064] The amount of YmerN120 is 3 g (ie, the weight ratio of the single-terminal dihydroxy polyether with a Y-shaped structure to the carboxyl-containing hydrophilic chain extender is 0.4:1), and the rest is the same as in Example 1.

[0065] Comparative Example 2

[0066] The amount of YmerN120 is 6 g (ie, the weight ratio of the single-terminal dihydroxy polyether with a Y-shaped structure to the carboxyl-containing hydrophilic chain extender is 1:1), and the rest is the same as in Example 2.

[0067] Comparative Example 3

[0068] It does not contain hydroxyethylethylenediamine, and the rest is the same as in Example 2.

[0069] Comparative Example 4

[0070] It does not contain N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide, and the rest is the same as Example 2.

[0071] Comparative Example 5

[0072] It does not contain hydroxyethylethylenediamine and N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide, and the rest is the same as Example 2.

[0073] Take Examples 1-3 and Comparative Examples 1-5, as well as a conventional foaming aqueous polyurethane emulsion for sports shoe leather purchased from the market (Wanhua Chemical aqueous polyurethane foaming emulsion, solid content of 45%, recorded as Comparative Example 6), and prepare a foaming emulsion according to the same method. The viscosity of the foaming emulsion at 25°C is 15000-20000 CPS; then the foaming emulsion is applied to the surface of the non-woven fabric, the coating gap is controlled at 130 silk, and then kept warm at 90°C for 4-6min, and then kept warm at 110°C for 5min, and finally dried at 130°C to obtain sports shoe leather.

[0074] The formula of the foaming emulsion is: 100 parts of water-based polyurethane emulsion, 0.4 parts of thickener, 4 parts of foaming agent, 5 parts of kaolin, 1 part of polymerized MDI curing agent, and 1 part of color paste.

[0075] According to the synthetic leather industry standard QB / T 1646-2007, the peel strength and room temperature folding resistance of the obtained sports shoe leather were tested. The test results are shown in Table 2.

[0076] Table 2 Test results

[0077] Grouping Surface cracking Peel strength (N / 3CM) Folding resistance at room temperature Example 1 Smooth surface without cracks 100-110 105,000 times Comparative Example 1 There are many cracks on the surface 90-95 98,000 times Example 2 Smooth surface without cracks 110-115 110,000 times Example 3 Smooth surface without cracks 110-115 108,000 times Comparative Example 2 There are some cracks on the surface 95-100 99,000 times Comparative Example 3 Smooth surface without cracks 65-70 55,000 times Comparative Example 4 There are many cracks on the surface 60-65 53,000 times Comparative Example 5 There are many cracks on the surface 50-55 46,000 times Comparative Example 6 Severe surface cracking 55-60 48,000 times

[0078] It can be seen from Table 2 that the aqueous polyurethane emulsion of the present invention adopts a direct coating foaming process to produce sports shoe leather, is not easy to crack during high-temperature drying, has a peel strength greater than 100N / 3CM, and has good folding resistance at room temperature, greater than 100,000 times, meeting the requirements of sports shoe leather.

[0079] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A water-based polyurethane emulsion for direct foaming of sports shoe leather, characterized in that: Its raw materials include: diisocyanate, polyol compound, chain extender, neutralizer, catalyst and water; The chain extenders include: single-ended dihydroxy polyether with a Y-shaped structure, carboxyl-containing hydrophilic chain extenders, small molecule diol chain extenders, amine chain extenders, and N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide.

2. The aqueous polyurethane emulsion for direct foaming of sports shoe leather according to claim 1, characterized in that: The single-ended dihydroxy polyether of the Y-shaped structure is YmerN120; preferably, the carboxyl-containing hydrophilic chain extender is one or both of dimethylol propionic acid and dihydroxybutyric acid.

3. The aqueous polyurethane emulsion for direct foaming of sports shoe leather according to claim 1 or 2, characterized in that: The amine chain extender is one or more of ethylenediamine, isophoronediamine, diethylenetriamine, and hydroxyethylethylenediamine; preferably, the amine chain extender is a mixture of ethylenediamine and hydroxyethylethylenediamine in a weight ratio of 3-4:1; preferably, the polyol compound is one or two of polytetrahydrofuran diol and adipic acid polyester polyol; preferably, the polyol compound is a mixture of polytetrahydrofuran diol and adipic acid polyester polyol in a weight ratio of 2-2.2:

1.

4. The aqueous polyurethane emulsion for direct foaming of sports shoe leather according to any one of claims 1 to 3, characterized in that: The diisocyanate is an aliphatic diisocyanate; preferably, the small molecule diol chain extender is one or more of ethylene glycol, 1,4-butanediol, and neopentyl glycol; preferably, the neutralizer is one or both of triethylamine and triethanolamine.

5. The aqueous polyurethane emulsion for direct foaming of sports shoe leather according to any one of claims 1 to 4, characterized in that: The weight ratio of the single-ended dihydroxy polyether with a Y-shaped structure and the hydrophilic chain extender containing a carboxyl group is 0.5-0.9:1; preferably, the weight ratio of the hydrophilic chain extender containing a carboxyl group, the amine chain extender, N,N-bis(2-hydroxyethyl)-3-aminopropionylglycinamide, and the small molecule diol chain extender is 1:0.6-0.9:0.14-0.2:0.3-0.

5.

6. The aqueous polyurethane emulsion for direct foaming of sports shoe leather according to any one of claims 1 to 5, characterized in that: The weight ratio of diisocyanate to polyol compound is 6-9:17-27; preferably, the weight ratio of diisocyanate to chain extender is 6-9:1-2.1; preferably, the weight ratio of diisocyanate to catalyst is 6-9:0.002-0.005; preferably, the weight ratio of diisocyanate to water is 6-9:30-48; preferably, the weight ratio of diisocyanate to neutralizer is 6-9:0.2-0.

5.

7. A method for preparing the aqueous polyurethane emulsion for direct foaming of sports shoe leather as claimed in any one of claims 1 to 6, characterized in that: The method comprises the following steps: in an inert gas atmosphere, uniformly mixing a polyol compound, a single-ended dihydroxy polyether in a Y-shaped structure, a diisocyanate and a catalyst, carrying out a primary reaction, then adding a carboxyl-containing hydrophilic chain extender, a small molecule diol chain extender and N,N-bis(2-hydroxyethyl)-3-aminopropionyl glycinamide, carrying out a secondary reaction, adding an organic solvent to reduce viscosity, adding a neutralizer, carrying out a neutralization reaction, adding water for emulsification, and then adding an amine chain extender, carrying out a tertiary reaction, removing the organic solvent, and obtaining a water-based polyurethane emulsion for direct foaming of sports shoe leather; preferably, carrying out a primary reaction at 90-95° C. for 1.5-2.5 h; preferably, carrying out a secondary reaction at 60-65° C. for 1.5-2.5 h; preferably, carrying out a neutralization reaction at 20-40° C. for 5-15 min; preferably, carrying out a tertiary reaction at 20-40° C. for 1.5-2.5 h.

8. A sports shoe leather, characterized in that: include: Non-woven fabric and foaming emulsion, wherein the raw materials of the foaming emulsion include: a thickener, a foaming agent, a curing agent and the aqueous polyurethane emulsion according to any one of claims 1-6.

9. The sports shoe leather according to claim 8, characterized in that: The weight ratio of aqueous polyurethane emulsion, thickener, foaming agent and curing agent is 100:0.3-0.5:3-5:0.8-1.2; preferably, the viscosity of the foaming emulsion at 25°C is 15000-20000 CPS; preferably, the curing agent is one or more of polymerized MDI curing agent, polymerized IPDI curing agent and polymerized HDI curing agent.

10. A method for preparing sports shoe leather as claimed in claim 9, characterized in that: The method comprises the following steps: mixing the raw materials of the foaming emulsion, coating the mixture on the surface of the non-woven fabric, curing and drying the mixture to obtain sports shoe leather; preferably, the curing and drying procedure is: keeping the mixture at 85-95°C for 4-6 minutes, keeping the mixture at 105-115°C for 4-6 minutes, and finally drying the mixture at 120-140°C.

Citation Information

Patent Citations

  • Solvent-free polyurethane hot melt adhesive and preparation method thereof

    CN114316875A

  • Waterborne polyurethane surface layer resin for environment-friendly synthetic leather and preparation method of waterborne polyurethane surface layer resin

    CN115785381A

  • Waterborne polyurethane dispersion as well as preparation method and application thereof

    CN116813877A

  • Novel toxoids of elastase of pseudomonas aeruginosa origin

    EP0153710A2

  • Aqueous polyurethane resin dispersion

    US20200369879A1