Rubber composition and preparation method thereof
By using a combination of nitrile rubber and butyl rubber in the PR series speakers, combined with the treatment of additives and fillers, the problems of poor bass sound quality and high impedance peaks of the speakers are solved, and the bass performance and stability of the speakers are significantly improved. .
Patent Information
- Application Number
- CN202411071284.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The speaker rubber cone in the PR series speakers is made of a single nitrile rubber material, resulting in poor bass sound quality, small damping, high impedance peaks, and prone to deflection problems.
A rubber composition is used, including a mixture of nitrile rubber and butyl rubber, which is uniformly blended through an internal mixer, then additives, reinforcing agents, fillers and softeners are added, and then extruded and sheared by an open mixer. Creates a more uniform rubber material.
The bass sound quality of the speaker is improved, the damping is increased, and the impedance peak is reduced from 3000HZ to 2500HZ, effectively solving the deflection problem.
Abstract
Description
Technical Field
[0001] The invention relates to rubber field technology, in particular to a rubber composition and a preparation method thereof. Background Art
[0002] PR series speakers are equipped with high-definition speakers. They are mainly used in conference rooms, classrooms, multi-function halls and other occasions with high sound pressure levels. The product has the following features: 1. The top speaker design technology makes the speaker beautiful in appearance and excellent in performance. 2. The treble adopts a unique wide-angle horn and PET polymer material sound film, which makes the treble sound clear and soft. The bass adopts a high-performance high-temperature resistant voice coil with a unique heat dissipation design magnet structure, which makes the bass speaker stable, reliable and durable. 3. The crossover circuit of the speaker is designed with a treble howling protection device to ensure that the speaker is stable and reliable during use. 4. Convenient hanging. The hanging device designed for this speaker can meet various hanging methods. It is very convenient to fix it on the wall and ceiling, and the speaker angle can be adjusted in all directions.
[0003] At present, the speaker rubber basin in the PR series speakers is made of a single nitrile rubber material, which results in poor bass quality, low damping, impedance peak value up to 3000HZ, and PR deflection problem. Therefore, it is necessary to study a solution to solve the above problems. Summary of the invention
[0004] In view of this, the present invention aims at the deficiencies in the prior art, and its main purpose is to provide a rubber composition and a preparation method thereof, which can effectively solve the problems of the existing PR series speakers whose speaker rubber basins use a single nitrile rubber material, resulting in poor bass quality, low damping and high impedance peak.
[0005] To achieve the above purpose, the present invention adopts the following technical solutions:
[0006] A rubber composition comprises the following raw materials in parts by weight: 80 parts of nitrile rubber and 20 parts of butyl rubber.
[0007] A method for preparing a rubber composition comprises the following steps:
[0008] (1) putting nitrile rubber and butyl rubber into an internal mixer, and forcing the two rubbers to be uniformly melted into one by shearing and kneading in the internal mixer, wherein the mass ratio of nitrile rubber to butyl rubber is 50%;
[0009] (2) After five minutes, open the feed cover of the internal mixer, add the additive and continue to mix until the additive is fully absorbed by the rubber. The weight proportion of the additive is 6%;
[0010] (3) After three minutes, a reinforcing agent, a filler and a softener are added and further kneaded, wherein the total weight of the reinforcing agent, the filler and the softener accounts for 44%;
[0011] (4) When all materials are fully mixed into irregular lumps, the material is discharged when the temperature reaches 115°C;
[0012] (5) Enter the next process of refining, and use the refining machine to extrude, shear, and thin pass three times to make all the materials more fully and evenly dispersed;
[0013] (6) Film packaging.
[0014] Preferably, the auxiliary agent includes an antioxidant and a dispersant;
[0015] Preferably, the reinforcing agent is one or both of carbon black and white carbon black.
[0016] Preferably, the filler is light calcium.
[0017] Compared with the prior art, the present invention has obvious advantages and beneficial effects. Specifically, it can be seen from the above technical solution that:
[0018] By using the rubber composition prepared by the formula and method of the present invention on PR series speakers, the bass sound quality of the PR series speakers can be improved, damping can be increased, and the impedance peak can be reduced from the peak value of 3000HZ of single nitrile rubber to 2500HZ, which can effectively improve the PR deflection problem. DETAILED DESCRIPTION
[0019] The invention discloses a rubber composition, which comprises the following raw materials in parts by weight: 80 parts of nitrile butadiene rubber (NBR) and 20 parts of butyl rubber (IIR).
[0020] The present invention also discloses a method for preparing a rubber composition, comprising the following steps:
[0021] (1) Nitrile rubber (NBR) and butyl rubber (IIR) are put into an internal mixer, and the two rubbers are uniformly melted together through shearing and kneading in the internal mixer, with the mass ratio of nitrile rubber to butyl rubber being 50%.
[0022] (2) After five minutes, open the feed cover of the internal mixer, add the additive and continue to mix, so that the additive is fully absorbed by the rubber, and the weight proportion of the additive is 6%. The additive includes an antioxidant and a dispersant.
[0023] (3) After three minutes, a reinforcing agent, a filler and a softener are added and the kneading is continued. The total weight of the reinforcing agent, the filler and the softener accounts for 44%. The reinforcing agent is one or two of carbon black and white carbon black. The filler is light calcium.
[0024] (4) When all materials are fully mixed into irregular lumps and the temperature reaches 115°C, discharge the material.
[0025] (5) Enter the next process of refining, and use the refining machine to extrude, shear and thin pass three times to make all the materials more fully and evenly dispersed.
[0026] (6) Film packaging.
[0027] The main principle of blending nitrile rubber (NBR) and butyl rubber (IIR) is to utilize the complementarity of their physical and chemical properties to improve the performance limitations of each when used alone. The main specific purpose is: performance complementarity.
[0028] The advantages of nitrile rubber (NBR) are heat resistance, wear resistance and strong adhesion, but poor cold resistance and ozone resistance. The biggest advantage of butyl rubber (IIR) is its low air permeability and low ozone resistance, good shock absorption, and improved processing performance after blending, which increases the fluidity of nitrile rubber (NBR) and reduces mixing heat, giving full play to their respective advantages and making up for their shortcomings.
[0029] After testing and use, the rubber composition prepared by the above formula and method is applied to the PR series speakers, which can improve the bass sound quality of the PR series speakers, increase damping, and reduce the impedance peak from the peak value of 3000HZ of single nitrile rubber to 2500HZ, which can effectively improve the PR deflection problem.
[0030] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.
Claims
1. A rubber composition, characterized in that: The invention comprises the following raw materials in parts by weight: 80 parts of nitrile rubber and 20 parts of butyl rubber.
2. A method for preparing the rubber composition according to claim 1, characterized in that: The following steps are included: (1) putting nitrile rubber and butyl rubber into an internal mixer, and forcibly mixing the two rubbers uniformly into one by shearing and kneading the internal mixer, wherein the mass ratio of nitrile rubber to butyl rubber is 50%; (2) After five minutes, open the feed cover of the mixer, add the additive and continue mixing until the additive is fully absorbed by the rubber. The weight percentage of the additive is 6%. (3) After three minutes, a reinforcing agent, a filler and a softener are added and further kneaded, wherein the total weight proportion of the reinforcing agent, the filler and the softener is 44%; (4) After all materials are fully mixed into irregular lumps, the material is discharged when the temperature reaches 115°C; (5) Enter the next process of refining, and use the refining machine to extrude, shear, and thin pass three times to make all the materials more fully and evenly dispersed; (6) Film packaging.
3. The method for preparing the rubber composition according to claim 2, characterized in that: The auxiliary agent includes an antioxidant and a dispersant.
4. The method for preparing the rubber composition according to claim 2, characterized in that: The reinforcing agent is one or both of carbon black and white carbon black.
5. The method for preparing the rubber composition according to claim 2, characterized in that: The filler is light calcium.