Nano calcium carbonate reinforced flame-retardant polypropylene composite material as well as preparation method and application thereof
Through the combination of modified ammonium polyphosphate and phytic acid and nano-calcium carbonate, the problem in the existing technology that the composite reaction of nano-calcium carbonate and ammonium polyphosphate reduces the flame retardant efficiency is solved, and the mechanical properties of the material are ensured while ensuring Significantly improve the flame retardant performance of polypropylene composite materials.
Patent Information
- Application Number
- CN202411182714.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing technology, the compounding of nano-calcium carbonate and ammonium polyphosphate reacts during the extrusion process, reducing the flame retardant efficiency. Moreover, the flame retardant efficiency of ammonium polyphosphate on polypropylene is low when used alone, making it difficult to improve the mechanical properties of the material while ensuring it. Flame retardant properties.
By using Tris reagent to modify ammonium polyphosphate to form an integrated intumescent flame retardant, and mixing it with modified phytic acid at an appropriate pH value, controlling the ratio of modified ammonium polyphosphate and modified phytic acid to form a modified Polypropylene IFR is used in conjunction with nano-calcium carbonate to improve the flame retardant properties of polypropylene composites.
It effectively improves the flame retardant performance of polypropylene composite materials, while maintaining the mechanical properties of the material, avoiding the adverse reactions between nanometer calcium carbonate and ammonium polyphosphate, and improving the flame retardant efficiency and appearance quality of the product.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a nano-calcium carbonate reinforced flame-retardant polypropylene composite material, a preparation method and application thereof. Background Art
[0002] Polypropylene (PP) is one of the five general-purpose plastics widely used in our daily lives, bringing great convenience to people's lives, such as bumpers and decorative parts in the automotive field. However, PP is composed of flammable elements such as C and O, and is very easy to burn, so it is necessary to make it flame retardant.
[0003] Among the current flame-retardant PP technologies, there are two categories: halogen flame retardant and non-halogen flame retardant. However, halogen flame retardant is gradually being abandoned, mainly because it releases harmful gases during combustion; while among non-halogen flame retardants, nanomaterials and synergistically enhanced intumescent flame retardants (IFR) are the most widely studied in industry and academia.
[0004] Nanomaterials have been widely used in the field of flame retardancy. Nano calcium carbonate is non-metallic and its size is less than 100nm. It has the functions of strengthening and toughening in the field of polymers. However, when compounded with typical IFR, especially with ammonium polyphosphate (APP), it will react during the extrusion process, reducing the flame retardant efficiency and affecting the appearance of the product. At the same time, the flame retardant efficiency of APP for PP is also very low when used alone, and it also needs to be modified. For the above reasons, while using nano calcium carbonate to strengthen and toughen polymers, it is imperative to improve the flame retardant properties of PP composites with IFR. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a nano-calcium carbonate reinforced flame-retardant polypropylene composite material, a preparation method and use thereof, which can improve the flame-retardant properties of the material while ensuring the mechanical properties of the material.
[0006] The embodiment of the present invention provides a nano-calcium carbonate reinforced flame-retardant polypropylene composite material, which is characterized in that it includes the following components in weight: 70-75% polypropylene, 20-25% IFR, and 1-5% nano-calcium carbonate; the IFR includes modified ammonium polyphosphate and modified phytic acid, and the weight ratio of the modified ammonium polyphosphate to the modified phytic acid is 2-4:0.5-1.5.
[0007] Preferably, the composition comprises the following components by weight: 75% polypropylene, 20-22% IFR, and 3-5% nano calcium carbonate; the IFR comprises modified ammonium polyphosphate and modified phytic acid, and the weight ratio of the modified ammonium polyphosphate to the modified phytic acid is 3:1.
[0008] Optionally, the modified ammonium polyphosphate is obtained by reacting an aqueous ammonium polyphosphate solution with a Tris reagent and drying the resultant.
[0009] Optionally, the modified phytic acid is obtained by mixing a phytic acid solution and an ammonia solution and controlling the pH value to be 6-8.
[0010] The embodiment of the present invention provides a method for preparing the nano-calcium carbonate reinforced flame-retardant polypropylene composite material, which comprises uniformly mixing polypropylene, IFR and nano-calcium carbonate, extruding and treating to obtain the nano-calcium carbonate reinforced flame-retardant polypropylene composite material.
[0011] Preferably, the processing temperature during extrusion is 180-200°C.
[0012] Preferably, the preparation method of the IFR is to uniformly mix the modified ammonium polyphosphate and the modified phytic acid in an aqueous solution to obtain the IFR.
[0013] Preferably, the preparation method of the modified ammonium polyphosphate is to add Tris reagent to an aqueous solution of ammonium polyphosphate, mix evenly to make the pH value of the solution be 6-8 (preferably 7), filter, wash, and dry to obtain the modified ammonium polyphosphate.
[0014] Preferably, the preparation method of the modified phytic acid is to mix a phytic acid aqueous solution and ammonia water, and control the pH value to be 6-8 to obtain the modified phytic acid.
[0015] The embodiment of the present invention provides a use of the nano-calcium carbonate reinforced flame-retardant polypropylene composite material, and the nano-calcium carbonate reinforced flame-retardant polypropylene composite material is used to prepare a flame-retardant material.
[0016] The beneficial effects of the present invention are that the present invention mainly utilizes Tris reagent to first modify APP, the purpose of which is: (1) enriching the flame retardant effect of APP, giving it OH functional groups (APP is a gas source and a nitrogen source, and Tris reagent is a carbon source and a nitrogen source), and forming an integrated intumescent flame retardant; (2) giving the APP surface a more reactive and more active negative charge type and density.
[0017] PA reacts with ammonia water to give ammonium groups on the surface of PA, which not only gives PA a positive charge function, but also enriches the flame retardant function of PA (N is a gas source, which releases inert gas during combustion to dilute the concentration of oxygen in the air). However, when modified with ammonia water, the ammonia content should not be too much, and the pH should be controlled at a neutral level, that is, 6-8. If it is excessive, exceeding 8, the flame retardant properties of the composite material will be greatly reduced. This is mainly because ammonium polyphosphate is acidic, and the two will react during the blending process.
[0018] When the modified ammonium polyphosphate and the modified phytic acid of the present invention are used to prepare IFR, the ratio of the two is appropriately controlled at about 3:1. If the content of the modified ammonium polyphosphate is too high, the flame retardant performance of the composite material will be significantly reduced. DETAILED DESCRIPTION
[0019] Example 1 A method for preparing a nano calcium carbonate reinforced flame retardant polypropylene composite material comprises the following steps: Step S1, preparation of IFR: (1) Dissolve 10 g APP in a three-necked flask containing 100 mL deionized water and stir for 30 min. Take an appropriate amount of Tris reagent and slowly add it to the above solution. Continue stirring at 80 °C until the pH value of the solution reaches neutral. Filter, wash and dry to obtain Tris reagent-modified APP (Tris@APP). + The generated APP surface has multiple hydroxyl features, which gives it more dehydration groups and prevents nano-calcium from reacting with it. At the same time, it also gives the APP surface a negative charge, which is beneficial for reacting with positively charged materials.
[0020] (2) Preparation of positively charged materials: An appropriate amount of bio-based material phytic acid (PA) is prepared into a PA aqueous solution with a mass concentration of 30%. During the stirring process, an ammonia aqueous solution is added to adjust the pH value of the above solution to 7, thereby obtaining a positively charged modified PA (N@PA).
[0021] (3) Preparation of IFR: Mix Tris@APP and N@PA in a mass ratio of 3:1 and stir in an aqueous solution to obtain IFR. This gives APP more flame retardant groups. Wash and dry the mixture for later use.
[0022] Step S2, taking 75% of dried polypropylene (PP), 20% of IFR and 5% of nano calcium carbonate according to the weight ratio of the components, mixing them evenly and adding them to an extruder for extrusion, the processing temperature of the extruder is 180-200° C., and then pelletizing and tableting are performed to obtain a nano calcium carbonate reinforced flame retardant polypropylene composite material.
[0023] Example 2 A method for preparing a nano calcium carbonate reinforced flame retardant polypropylene composite material comprises the following steps: Step S1, preparation of IFR: (1) Dissolve 10 g APP in a three-necked flask containing 100 mL deionized water and stir for 30 min. Take an appropriate amount of Tris reagent and slowly add it to the above solution. Continue stirring at 80 °C until the pH value of the solution reaches neutral. Filter, wash and dry to obtain Tris reagent-modified APP (Tris@APP). + The generated APP surface has multiple hydroxyl features, which gives it more dehydration groups and prevents nano-calcium from reacting with it. At the same time, it also gives the APP surface a negative charge, which is beneficial for reacting with positively charged materials.
[0024] (2) Preparation of positively charged materials: An appropriate amount of bio-based material phytic acid (PA) is prepared into a PA aqueous solution with a mass concentration of 30%. During the stirring process, an ammonia aqueous solution is added to adjust the pH value of the above solution to 7, thereby obtaining a positively charged modified PA (N@PA).
[0025] (3) Preparation of IFR: Mix Tris@APP and N@PA in a mass ratio of 3:1 and stir in an aqueous solution to obtain IFR. This gives APP more flame retardant groups. Wash and dry the mixture for later use.
[0026] Step S2: 75% of dried PP, 22% of IFR and 3% of nano calcium carbonate are mixed uniformly and added to an extruder for extrusion at a processing temperature of 180-200° C., followed by pelletizing and tableting to obtain a nano calcium carbonate reinforced flame retardant polypropylene composite material.
[0027] Example 3 A method for preparing a nano calcium carbonate reinforced flame retardant polypropylene composite material comprises the following steps: Step S1, preparation of IFR: (1) Dissolve 10 g APP in a three-necked flask containing 100 mL deionized water and stir for 30 min. Take an appropriate amount of Tris reagent and slowly add it to the above solution. Continue stirring at 80 °C until the pH value of the solution reaches neutral. Filter, wash and dry to obtain Tris reagent-modified APP (Tris@APP). + The generated APP surface has multiple hydroxyl features, which gives it more dehydration groups and prevents nano-calcium from reacting with it. At the same time, it also gives the APP surface a negative charge, which is beneficial for reacting with positively charged materials.
[0028] (2) Preparation of positively charged materials: An appropriate amount of bio-based material phytic acid (PA) is prepared into a 30% PA solution. During the stirring process, an ammonia solution is added to adjust the pH value of the solution to 7, thereby obtaining a positively charged modified PA (N@PA).
[0029] (3) Preparation of IFR: Mix Tris@APP and N@PA in a mass ratio of 3:1 and stir in an aqueous solution to obtain IFR. This gives APP more flame retardant groups. Wash and dry the mixture for later use.
[0030] Step S2, taking 75% of dried PP, 24% of IFR and 1% of nano calcium carbonate according to the weight ratio of the components, mixing them evenly and adding them to an extruder for extrusion, the processing temperature of the extruder is 180-200° C., and then pelletizing and tableting are performed to obtain a nano calcium carbonate reinforced flame retardant polypropylene composite material.
[0031] Comparative Example 1 Compared with Example 1, the Tris@APP in step S1 is replaced with 10 g of APP, and the rest is consistent with Example 1.
[0032] Comparative Example 2 Compared with Example 1, in step S2, the weight ratio of dried PP is 75%, IFR is 20%, and nano-calcium carbonate is 5%, which is replaced by the weight ratio of dried PP is 75% and nano-calcium carbonate is 25%, and the rest is consistent with Example 1.
[0033] Comparative Example 3 Compared with Example 1, in Comparative Example 3, in step S2, the weight ratio of dried PP is 75%, IFR is 20%, and nano calcium carbonate is 5%, which is replaced by the weight ratio of dried PP is 75% and ammonium polyphosphate (APP) is 25%, and the rest is consistent with Example 1.
[0034] Comparative Example 4 This comparative example 4 does not have other fillers, that is, compared with Example 1, in step S2, the weight ratio of the dried PP is 75%, the IFR is 20%, and the nano calcium carbonate is 5%, which is replaced by the weight ratio of the dried PP is 100%, and the rest is consistent with Example 1.
[0035] Comparative Example 5 Compared with Example 1, Comparative Example 5 differs in that: in step S1, (2) the positively charged material is prepared by adding an appropriate amount of bio-based material phytic acid (PA) to a PA aqueous solution with a mass concentration of 30%, and during stirring, an ammonia aqueous solution is added to adjust the pH value of the solution to 10, thereby obtaining a positively charged modified PA (N@PA).
[0036] The other steps are the same as those in Example 1.
[0037] Comparative Example 6 The difference between Comparative Example 6 and Example 1 is that in step S1, (3) IFR is prepared by taking the mass ratio of Tris@APP to N@PA as 10:1.
[0038] The other steps are the same as those in Example 1.
[0039] The nano-calcium carbonate reinforced flame-retardant polypropylene composite materials obtained in the above Examples 1-3 and Comparative Examples 1-6 were subjected to performance tests, respectively. The performance tests included: (1) Mechanical properties test: The test shall be carried out in accordance with the test method disclosed in GB / T1040-2006 “Determination of tensile properties of plastics”.
[0040] (2) Flame retardant performance test: The test was carried out according to the test method disclosed in GB / T 2406-2009 "Plastics Combustion Performance Test Method Oxygen Index Method".
[0041] The measurement is carried out in accordance with the test method disclosed in GB / T 2408-20218 "Horizontal and vertical methods for determination of combustion performance of plastics".
[0042] The measurement is carried out according to the test method disclosed in ISO5660-1 "Combustion heat release rate test".
[0043] The performance test results are shown in Table 1.
[0044] Table 1: Performance test of calcium carbonate reinforced flame retardant polypropylene composites
[0045] From the above performance test results, compared with adding unmodified APP, or adding only nano-calcium carbonate, or adding only unmodified ammonium polyphosphate, or adding excessive ammonia water to make its pH value 10, or controlling the excessive amount of modified APP to make the mass ratio of Tris@APP to N@PA 10:1, the composite material of the embodiment of the present invention can effectively improve the flame retardant properties while maintaining the mechanical properties.
[0046] A person skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of protection of the present application is limited to these examples. In line with the concept of the present application, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of different aspects of one or more embodiments of the present application as described above, which are not provided in detail for the sake of simplicity.
[0047] One or more embodiments of the present application are intended to cover all such substitutions, modifications and variations that fall within the broad scope of the present application. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of one or more embodiments of the present application should be included in the protection scope of the present application.
Claims
1. A nano calcium carbonate reinforced flame retardant polypropylene composite material, characterized in that: The invention comprises the following components by weight: 70-75% polypropylene, 20-25% IFR and 1-5% nano calcium carbonate; the IFR comprises modified ammonium polyphosphate and modified phytic acid, and the weight ratio of the modified ammonium polyphosphate to the modified phytic acid is 2-4:0.5-1.
5.
2. The nano-calcium carbonate reinforced flame-retardant polypropylene composite material according to claim 1, characterized in that: The invention comprises the following components by weight: 75% polypropylene, 20-22% IFR and 3-5% nano calcium carbonate; the IFR comprises modified ammonium polyphosphate and modified phytic acid, and the weight ratio of the modified ammonium polyphosphate to the modified phytic acid is 3:
1.
3. The nano calcium carbonate reinforced flame retardant polypropylene composite material according to claim 1 or 2, characterized in that: The modified ammonium polyphosphate is obtained by reacting an ammonium polyphosphate aqueous solution with a Tris reagent and drying the resultant.
4. The nano-calcium carbonate reinforced flame-retardant polypropylene composite material according to claim 1 or 2, characterized in that: The modified phytic acid is obtained by mixing a phytic acid solution and an ammonia solution and controlling the pH value to be 6-8.
5. A method for preparing the nano-calcium carbonate reinforced flame-retardant polypropylene composite material according to any one of claims 1 to 4, characterized in that: The polypropylene, IFR and nano calcium carbonate are uniformly mixed, extruded and processed to obtain a nano calcium carbonate reinforced flame retardant polypropylene composite material.
6. The preparation method according to claim 5, characterized in that: The processing temperature during the extrusion is 180-200°C.
7. The preparation method according to claim 5 or 6, characterized in that: The preparation method of the IFR is to uniformly mix modified ammonium polyphosphate and modified phytic acid in an aqueous solution to obtain the IFR.
8. The preparation method according to claim 7, characterized in that: The preparation method of the modified ammonium polyphosphate comprises the following steps: adding Tris reagent to an ammonium polyphosphate aqueous solution, mixing uniformly to make the pH value of the solution be 6-8, filtering, washing, and drying to obtain the modified ammonium polyphosphate.
9. The preparation method according to claim 7, characterized in that: The preparation method of the modified phytic acid is as follows: mixing a phytic acid aqueous solution and ammonia water, and controlling the pH value to be 6-8 to obtain the modified phytic acid.
10. Use of the nano-calcium carbonate reinforced flame-retardant polypropylene composite material according to any one of claims 1 to 4, characterized in that: The nano calcium carbonate reinforced flame retardant polypropylene composite material is used for preparing flame retardant materials.