Impact-resistant ethylene propylene diene monomer and application thereof in sealing product
By blending multi-arm maleimide flame retardant with EPDM rubber and modified nano-silicon nitride and vulcanizing to form a cross-linked network structure, the flame retardant performance of EPDM rubber in sealing products is solved. Low and flammable problems, improved mechanical properties and sealing effect.
Patent Information
- Application Number
- CN202410759753.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing EPDM rubber has problems with low flame retardancy, flammability, and reduced physical properties in sealing products. It also has poor compatibility with other materials, making it difficult to achieve uniform dispersion and co-vulcanization.
The multi-arm maleimide flame retardant is blended with components such as EPDM rubber and modified nano-silicon nitride, and is vulcanized to form a cross-linked network structure to improve the flame retardant and mechanical properties.
The flame retardant and mechanical properties of EPDM rubber are significantly improved, forming a dense cross-linked network structure, hindering the penetration of gases and liquids, and broadening its application in sealing products.
Smart Images

Figure BDA0004890690460000051 
Figure BDA0004890690460000061 
Figure BDA0004890690460000062
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber materials, in particular to an impact-resistant ethylene propylene diene monomer rubber and application thereof in sealing products. Background Art
[0002] Ethylene propylene diene monomer (EPDM) is a saturated rubber with excellent heat resistance, weather resistance and electrical properties, and is moderately priced and has mature technology. It is the preferred material for automobiles, ships, railways, and electrical equipment, and is currently the most widely used sealing material; rubber sealing products used in mobile equipment such as automobiles are high-end products in the sealing field, and have high requirements for weather resistance and other aspects. They have always used imported EPDM materials; although EPDM itself has good heat resistance, chemical resistance, water resistance, etc., it is an organic polymer material. During use, it will cause the physical and mechanical properties to gradually deteriorate due to the combined effects of external environmental factors such as light, heat, oxygen and corrosive media, and will cause cracking, hardening, softening, powdering and other phenomena, and the mechanical properties will be significantly reduced; therefore, the preparation of an impact-resistant EPDM material to broaden its application in sealing products has become a hot topic of research.
[0003] At present, the use function of EPDM rubber sealing materials in China is limited to sealing, and other factors such as flame retardancy and environmental protection have not been taken into consideration; EPDM, like most organic polymer materials, has a low limiting oxygen index and is easy to burn. It is easy to cause fire directly or indirectly during use. In the existing technology, metal hydroxides such as magnesium hydroxide and aluminum hydroxide are mostly used to prepare low-smoke halogen-free flame retardant rubber composite materials. However, filling a large amount of micron flame retardants will cause a serious decline in the physical properties of the rubber material, and there is a phenomenon that the flame retardant is not environmentally friendly or the environmentally friendly is not flame retardant; in addition, when EPDM rubber is blended, it has poor adhesion with other materials and a slow vulcanization speed. Therefore, the key to rubber modification is not only to ensure good compatibility and uniform dispersion between the components, but also to achieve co-vulcanization between the components.
[0004] The invention aims to synthesize a multi-arm maleimide flame retardant which can be co-crosslinked with EPDM rubber, improve the mechanical properties and flame retardant properties of the rubber, is halogen-free and environmentally friendly, and broadens its application in sealing products. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art, provide an impact-resistant EPDM rubber and its application in sealing products, improve the flame retardant and mechanical properties of the existing EPDM rubber, and broaden its further application in sealing products.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] An impact-resistant EPDM rubber comprises the following components in parts by weight: 100 parts of EPDM rubber, 10-20 parts of carbon black, 3-15 parts of modified nano silicon nitride, 2-10 parts of multi-arm maleimide flame retardant, 2-5 parts of zinc oxide, 3-7 parts of stearic acid, 0.5-1 parts of dicumyl peroxide, 1-3 parts of sulfur and 0.8-1.5 parts of accelerator M.
[0008] The preparation method of impact-resistant EPDM rubber is as follows: EPDM rubber and modified nano silicon nitride are mixed in an internal mixer at a temperature of 110-130°C and a rotation speed of 150-200r / min until the rollers are covered, carbon black, multi-arm maleimide flame retardant, zinc oxide, stearic acid, diisopropylbenzene peroxide, accelerator M and sulfur are added in sequence, mixed for 10-20 minutes, discharged, and then pressed into thin sheets through a double-roll open mill, left at room temperature for 16-32 hours, the thin sheets are placed in a mold, and placed on a flat vulcanizer for vulcanization to obtain impact-resistant EPDM rubber.
[0009] Preferably, the vulcanization temperature is 150-170° C., the vulcanization pressure is 10-20 MPa, and the vulcanization time is 5-15 min.
[0010] Preferably, the preparation method of the multi-arm maleimide flame retardant is:
[0011] Step (1), under a nitrogen atmosphere, add 4,6-dichloro-1,3,5-triazine ring-2-amine, 4-nitrophenylboric acid, potassium carbonate and toluene to a reaction flask, stir evenly, add tetrakis(triphenylphosphine)palladium, stir to react, after the reaction is completed, cool to room temperature, filter, recrystallize from ethanol, and dry to obtain a structural formula of Intermediate 1.
[0012] Step (2), under nitrogen atmosphere, add ethyl dichlorophosphate and acetonitrile to a reaction flask, stir evenly, add intermediate 1 and triethylamine, react at 35-50° C. for 5-10 h, filter, wash with ethanol, and dry to obtain a product having the structural formula: Intermediate 2.
[0013] Step (3), under nitrogen atmosphere, add intermediate 2 and ethanol to the reaction flask, heat to 50-65°C, add 30-40% ammonium chloride solution and iron powder under stirring, continue to react for 2-5h, filter, wash with ethyl acetate, concentrate and dry to obtain a compound with the structural formula Intermediate 3.
[0014] Step (4), under nitrogen atmosphere, add intermediate 3 and N-methylpyrrolidone to the reaction flask, stir evenly, add maleic anhydride, react at 160-180°C for 3-6h, cool to room temperature, filter and dry to obtain the structural formula Multi-arm maleimide flame retardant.
[0015] Preferably, in step (1), the molar ratio of 4,6-dichloro-1,3,5-triazine-2-amine, 4-nitrophenylboric acid, potassium carbonate and tetrakis(triphenylphosphine)palladium is 1:(2.05-2.2):(2.1-2.3):(0.15-0.25).
[0016] Preferably, in step (1), the reaction temperature is 80-100° C. and the reaction time is 12-24 h.
[0017] Preferably, in step (2), the molar ratio of ethyl dichlorophosphate, intermediate 1, and triethylamine is 1:(2-2.15):(2.3-2.5).
[0018] Preferably, the molar ratio of the intermediate 2, the ammonium chloride solution and the iron powder in step (3) is 1:(10-15):(6-9).
[0019] Preferably, the molar ratio of intermediate 3 to maleic anhydride in step (4) is 1:(4.5-6).
[0020] Preferably, impact-resistant EPDM rubber is used in sealing products.
[0021] By adopting the above technical solution, the beneficial effects of the present invention are:
[0022] The invention uses 4,6-dichloro-1,3,5-triazine ring-2-amine and 4-nitrophenylboric acid as raw materials, obtains intermediate 1 under the catalytic action of tetrakis(triphenylphosphine)palladium, then undergoes substitution reaction with ethyl dichlorophosphate to obtain intermediate 2, then reduces the nitro group to obtain intermediate 3, and then reacts with maleic anhydride to obtain multi-arm maleimide flame retardant, and finally blends with ethylene propylene diene monomer rubber, modified nano silicon nitride and the like for extrusion and vulcanization molding to obtain impact-resistant ethylene propylene diene monomer rubber.
[0023] The triazine structure in the multi-arm maleimide flame retardant has an excellent carbon-forming effect. It decomposes under high temperature and releases nitrogen, which promotes the formation of a foam carbon protective layer and effectively prevents the material from further burning. At the same time, organic phosphorus decomposes under heat to generate phosphoric acid and pyrophosphoric acid with strong dehydration effect, which can form a solid phase layer on the surface of the material to isolate air and heat. The ammonia generated by its decomposition can also isolate air, and phosphoric acid catalysis promotes the formation of carbon. The triazine carbon former and organic phosphorus synergistically flame retardant, forming a dense expanded carbon layer during the combustion process, and promptly taking away the heat and flammable small molecules generated by the combustion. In addition, the maleimide group has a highly active double bond functional group. During the mixing and vulcanization process with EPDM rubber, the active double bond opens and forms a "bridge bond" cross-linking with EPDM rubber to form a cross-linked network structure, which promotes carbonization, thereby stopping the combustion of the material and improving the flame retardant properties of the rubber material.
[0024] The multiple maleimide groups in the multi-arm maleimide flame retardant have highly active double bond functional groups. During the vulcanization process of mixing with EPDM rubber, the active double bonds are opened to form a "bridge bond" cross-linked network structure, which enhances the ability to resist external stress; the modified nano-silicon nitride has good compatibility with the EPDM rubber system, improves the interface between nano-silicon nitride and EPDM rubber, and forms a relatively uniform dispersion system between the two, which plays a significant reinforcing role, thereby exerting the characteristics of inorganic nanoparticles and improving the impact resistance of the rubber; at the same time, EPDM rubber contains a dense cross-linked network structure, which hinders the penetration of gas and liquid into the interior of the material, broadening its further application in sealing products. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Preparation of modified nano silicon nitride: Add 10 g of nano silicon nitride and 100 mL of ethanol to a reaction flask, stir evenly, then add 0.5 g of zinc methacrylate and 0.1 g of initiator azobisisobutyronitrile, reflux at 60 °C for 2.5 h, concentrate and dry, take out and sieve, place in a Soxhlet extractor, extract with ethanol for 72 h to obtain modified nano silicon nitride.
[0027] Example 1
[0028] (1) Under nitrogen atmosphere, 18 mmol of 4,6-dichloro-1,3,5-triazine-2-amine, 38.7 mmol of 4-nitrophenylboric acid, 37.8 mmol of potassium carbonate and 155 mL of toluene were added to a reaction flask, stirred evenly, and then 3.6 mmol of tetrakis(triphenylphosphine)palladium was added. The mixture was reacted at 90° C. for 16 h, cooled to room temperature, filtered, recrystallized from ethanol, and dried to obtain intermediate 1. The preparation reaction formula is as follows:
[0029]
[0030] (2) Under nitrogen atmosphere, 15 mmol of ethyl dichlorophosphate and 180 mL of acetonitrile were added to a reaction flask, stirred evenly, and then 31 mmol of intermediate 1 and 39 mmol of triethylamine were added. The mixture was reacted at 45° C. for 8 h, filtered, washed with ethanol, and dried to obtain intermediate 2. The preparation reaction formula is as follows:
[0031]
[0032] (3) Under nitrogen atmosphere, 12 mmol of intermediate 2 and 162 mL of ethanol were added to a reaction flask, heated to 55° C., 165 mmol of 35% ammonium chloride solution and 90 mmol of iron powder were added under stirring, and the reaction was continued for 4 h. The mixture was filtered, washed with ethyl acetate, and concentrated to dryness to obtain intermediate 3. The preparation reaction formula is as follows:
[0033]
[0034] (4) Under nitrogen atmosphere, 10 mmol of intermediate 3 and 250 mL of N-methylpyrrolidone were added to the reaction flask, and after stirring, 50 mmol of maleic anhydride was added, and the mixture was reacted at 170° C. for 5 h, cooled to room temperature, filtered and dried to obtain a multi-arm maleimide flame retardant. The preparation reaction formula is as follows:
[0035]
[0036] (5) 100 g of EPDM rubber and 3 g of modified nano silicon nitride were mixed in an internal mixer at a temperature of 120 ° C and a rotation speed of 180 r / min until the rollers were wrapped. 15 g of carbon black, 2 g of multi-arm maleimide flame retardant, 3.5 g of zinc oxide, 6 g of stearic acid, 0.8 g of diisopropylbenzene peroxide, 1 g of accelerator M and 2 g of sulfur were added in sequence. The mixture was mixed for 15 min, discharged, and then pressed into a thin sheet through a double-roll open mill. The thin sheet was left at room temperature for 24 h. The thin sheet was placed in a mold and placed on a flat vulcanizer for vulcanization at a vulcanization temperature of 160 ° C, a vulcanization pressure of 18 MPa, and a vulcanization time of 10 min to obtain an impact-resistant EPDM rubber.
[0037] Example 2
[0038] (1) Under nitrogen atmosphere, 40 mmol of 4,6-dichloro-1,3,5-triazine-2-amine, 82 mmol of 4-nitrophenylboric acid, 84 mmol of potassium carbonate and 200 mL of toluene were added to a reaction flask. After stirring evenly, 6 mmol of tetrakis(triphenylphosphine)palladium was added. The mixture was reacted at 100° C. for 12 h. The mixture was cooled to room temperature, filtered, recrystallized from ethanol and dried to obtain intermediate 1.
[0039] (2) Under nitrogen atmosphere, 35 mmol of ethyl dichlorophosphate and 350 mL of acetonitrile were added to a reaction flask. After stirring, 70 mmol of intermediate 1 and 80.5 mmol of triethylamine were added. The mixture was reacted at 50° C. for 5 h, filtered, washed with ethanol, and dried to obtain intermediate 2.
[0040] (3) Under nitrogen atmosphere, 28 mmol of intermediate 2 and 420 mL of ethanol were added to a reaction flask, heated to 65° C., 280 mmol of 40% ammonium chloride solution and 168 mmol of iron powder were added under stirring, and the reaction was continued for 3 h. The mixture was filtered, washed with ethyl acetate, and concentrated to dryness to obtain intermediate 3.
[0041] (4) Under nitrogen atmosphere, 24 mmol of intermediate 3 and 480 mL of N-methylpyrrolidone were added to a reaction flask. After stirring evenly, 108 mmol of maleic anhydride was added. The mixture was reacted at 180° C. for 3 h. The mixture was cooled to room temperature, filtered and dried to obtain a multi-arm maleimide flame retardant.
[0042] (5) 100 g of EPDM rubber and 6 g of modified nano silicon nitride were mixed in an internal mixer at a temperature of 130 ° C and a rotation speed of 200 r / min until the rollers were wrapped. 10 g of carbon black, 4 g of multi-arm maleimide flame retardant, 4 g of zinc oxide, 3 g of stearic acid, 1 g of diisopropylbenzene peroxide, 1.5 g of accelerator M and 3 g of sulfur were added in sequence. The mixture was mixed for 20 min, discharged, and then pressed into a thin sheet through a double-roll open mill. The thin sheet was left at room temperature for 32 h. The thin sheet was placed in a mold and placed on a flat vulcanizer for vulcanization at a vulcanization temperature of 170 ° C, a vulcanization pressure of 20 MPa, and a vulcanization time of 5 min to obtain an impact-resistant EPDM rubber.
[0043] Example 3
[0044] (1) Under nitrogen atmosphere, 25 mmol of 4,6-dichloro-1,3,5-triazine-2-amine, 55 mmol of 4-nitrophenylboric acid, 57.5 mmol of potassium carbonate and 250 mL of toluene were added to a reaction flask. After stirring, 6.25 mmol of tetrakis(triphenylphosphine)palladium was added. The mixture was reacted at 80° C. for 24 h. The mixture was cooled to room temperature, filtered, recrystallized from ethanol and dried to obtain intermediate 1.
[0045] (2) Under nitrogen atmosphere, 20 mmol of ethyl dichlorophosphate and 200 mL of acetonitrile were added to a reaction flask. After stirring, 40 mmol of intermediate 1 and 46 mmol of triethylamine were added. The mixture was reacted at 35° C. for 10 h. The mixture was filtered, washed with ethanol, and dried to obtain intermediate 2.
[0046] (3) Under nitrogen atmosphere, 18 mmol of intermediate 2 and 360 mL of ethanol were added to a reaction flask, heated to 50°C, and 270 mmol of 30% ammonium chloride solution and 162 mmol of iron powder were added under stirring. The reaction was continued for 5 h, filtered, washed with ethyl acetate, and concentrated to dryness to obtain intermediate 3.
[0047] (4) Under nitrogen atmosphere, 15 mmol of intermediate 3 and 450 mL of N-methylpyrrolidone were added to a reaction flask, and after stirring, 90 mmol of maleic anhydride was added. The mixture was reacted at 160° C. for 6 h, cooled to room temperature, filtered and dried to obtain a multi-arm maleimide flame retardant.
[0048] (5) 100 g of EPDM rubber and 9 g of modified nano silicon nitride were mixed in an internal mixer at a temperature of 110 ° C and a rotation speed of 150 r / min until the rollers were wrapped. 20 g of carbon black, 6 g of multi-arm maleimide flame retardant, 5 g of zinc oxide, 7 g of stearic acid, 0.5 g of diisopropylbenzene peroxide, 0.8 g of accelerator M and 1 g of sulfur were added in sequence. The mixture was mixed for 10 min, discharged, and then pressed into a thin sheet through a double-roll open mill. The thin sheet was left at room temperature for 16 h. The thin sheet was placed in a mold and placed on a flat vulcanizer for vulcanization at a vulcanization temperature of 150 ° C, a vulcanization pressure of 10 MPa, and a vulcanization time of 15 min to obtain impact-resistant EPDM rubber.
[0049] Example 4
[0050] (1) Under nitrogen atmosphere, 30 mmol of 4,6-dichloro-1,3,5-triazine-2-amine, 63 mmol of 4-nitrophenylboric acid, 65 mmol of potassium carbonate and 270 mL of toluene were added to a reaction flask. After stirring evenly, 6.6 mmol of tetrakis(triphenylphosphine)palladium was added. The mixture was reacted at 85° C. for 18 h. The mixture was cooled to room temperature, filtered, recrystallized from ethanol and dried to obtain intermediate 1.
[0051] (2) Under nitrogen atmosphere, 25 mmol of ethyl dichlorophosphate and 350 mL of acetonitrile were added to a reaction flask. After stirring, 52 mmol of intermediate 1 and 60 mmol of triethylamine were added. The mixture was reacted at 40° C. for 9 h. The mixture was filtered, washed with ethanol, and dried to obtain intermediate 2.
[0052] (3) Under nitrogen atmosphere, 20 mmol of intermediate 2 and 370 mL of ethanol were added to a reaction flask, heated to 60°C, and 280 mmol of 35% ammonium chloride solution and 170 mmol of iron powder were added under stirring. The reaction was continued for 4 h, filtered, washed with ethyl acetate, and concentrated to dryness to obtain intermediate 3.
[0053] (4) Under nitrogen atmosphere, 16 mmol of intermediate 3 and 400 mL of N-methylpyrrolidone were added to a reaction flask. After stirring evenly, 88 mmol of maleic anhydride was added. The mixture was reacted at 175° C. for 5 h. The mixture was cooled to room temperature, filtered and dried to obtain a multi-arm maleimide flame retardant.
[0054] (5) 100 g of EPDM rubber and 12 g of modified nano silicon nitride were mixed in an internal mixer at a temperature of 125 ° C and a rotation speed of 160 r / min until the rollers were wrapped. 18 g of carbon black, 8 g of multi-arm maleimide flame retardant, 3 g of zinc oxide, 5 g of stearic acid, 0.9 g of diisopropylbenzene peroxide, 1.2 g of accelerator M and 2 g of sulfur were added in sequence. The mixture was mixed for 20 min, discharged, and then pressed into a thin sheet through a double-roll open mill. The thin sheet was left at room temperature for 24 h. The thin sheet was placed in a mold and placed on a flat vulcanizer for vulcanization at a vulcanization temperature of 165 ° C, a vulcanization pressure of 12 MPa, and a vulcanization time of 10 min to obtain an impact-resistant EPDM rubber.
[0055] Example 5
[0056] (1) Under nitrogen atmosphere, 12 mmol of 4,6-dichloro-1,3,5-triazine-2-amine, 26 mmol of 4-nitrophenylboric acid, 27 mmol of potassium carbonate and 78 mL of toluene were added to a reaction flask. After stirring, 2.65 mmol of tetrakis(triphenylphosphine)palladium was added. The mixture was reacted at 95° C. for 15 h. The mixture was cooled to room temperature, filtered, recrystallized from ethanol and dried to obtain intermediate 1.
[0057] (2) Under nitrogen atmosphere, 9 mmol of ethyl dichlorophosphate and 100 mL of acetonitrile were added to a reaction flask. After stirring, 18.5 mmol of intermediate 1 and 21.6 mmol of triethylamine were added. The mixture was reacted at 45° C. for 9 h. The mixture was filtered, washed with ethanol, and dried to obtain intermediate 2.
[0058] (3) Under nitrogen atmosphere, 5 mmol of intermediate 2 and 90 mL of ethanol were added to a reaction flask, heated to 60°C, and 75 mmol of 40% ammonium chloride solution and 42 mmol of iron powder were added under stirring. The reaction was continued for 5 h, filtered, washed with ethyl acetate, and concentrated to dryness to obtain intermediate 3.
[0059] (4) Under nitrogen atmosphere, 3 mmol of intermediate 3 and 70 mL of N-methylpyrrolidone were added to a reaction flask. After stirring evenly, 16.5 mmol of maleic anhydride was added. The mixture was reacted at 170° C. for 5 h. The mixture was cooled to room temperature, filtered and dried to obtain a multi-arm maleimide flame retardant.
[0060] (5) 100 g of EPDM rubber and 15 g of modified nano silicon nitride were mixed in an internal mixer at a temperature of 120 ° C and a rotation speed of 200 r / min until the rollers were wrapped. 15 g of carbon black, 10 g of multi-arm maleimide flame retardant, 5 g of zinc oxide, 4 g of stearic acid, 0.9 g of diisopropylbenzene peroxide, 1.2 g of accelerator M and 2.5 g of sulfur were added in sequence. The mixture was mixed for 16 min, discharged, and then pressed into a thin sheet through a double-roll open mill. The thin sheet was left at room temperature for 24 h, and then placed in a mold and placed on a flat vulcanizer for vulcanization at a vulcanization temperature of 165 ° C, a vulcanization pressure of 18 MPa, and a vulcanization time of 12 min to obtain an impact-resistant EPDM rubber.
[0061] Comparative Example 1
[0062] 100g of EPDM rubber and 3g of modified nano-silicon nitride were mixed in an internal mixer at a temperature of 120°C and a rotation speed of 180r / min until the rollers were wrapped. 15g of carbon black, 3.5g of zinc oxide, 6g of stearic acid, 0.8g of diisopropylbenzene peroxide, 1g of accelerator M and 2g of sulfur were added in sequence. The mixture was mixed for 15min, discharged, and then pressed into a sheet through a double-roll open mill. The sheet was left at room temperature for 24h, and the sheet was placed in a mold and vulcanized on a flat vulcanizer at a vulcanization temperature of 160°C, a vulcanization pressure of 18MPa, and a vulcanization time of 10min to obtain modified EPDM rubber.
[0063] Comparative Example 2
[0064] 100g of EPDM rubber and nano-silicon nitride were mixed in an internal mixer at a temperature of 120°C and a speed of 180r / min until the rollers were wrapped. 15g of carbon black, 2g of multi-arm maleimide flame retardant, 3.5g of zinc oxide, 6g of stearic acid, 0.8g of diisopropylbenzene peroxide, 1g of accelerator M and 2g of sulfur were added in sequence. The mixture was mixed for 15min, discharged, and then pressed into a thin sheet through a double-roll open mill. The thin sheet was left at room temperature for 24h, placed in a mold, and placed on a flat vulcanizer for vulcanization at a vulcanization temperature of 160°C, a vulcanization pressure of 18MPa, and a vulcanization time of 10min to obtain a modified EPDM rubber.
[0065] Comparative Example 3
[0066] 100g of EPDM rubber was mixed in an internal mixer at a temperature of 120°C and a speed of 180r / min until the rollers were wrapped. 15g of carbon black, 3.5g of zinc oxide, 6g of stearic acid, 0.8g of diisopropylbenzene peroxide, 1g of accelerator M and 2g of sulfur were added in sequence. The mixture was mixed for 15min, discharged, and then pressed into a sheet through a double-roll mill. The sheet was left at room temperature for 24h. The sheet was placed in a mold and vulcanized on a flat vulcanizer at a vulcanization temperature of 160°C, a vulcanization pressure of 18MPa, and a vulcanization time of 10min to obtain a modified EPDM rubber.
[0067] Vertical combustion performance test: The test was conducted using a vertical combustion tester in accordance with GB / T 2408-2008 standard, with a sample size of 130mm×13mm×3mm.
[0068] Limiting oxygen index test: The test is carried out using an oxygen index meter in accordance with GB / T 2406.1-2008 standard, and the sample size is 100mm×7mm×3mm.
[0069] Table 1 Flame retardant performance test
[0070]
[0071] From the test results in the above table, it can be seen that with the increase of the content of multi-arm maleimide flame retardant, the flame retardant performance of EPDM rubber gradually increases. The limiting oxygen index of implementation 5 is 32.5%, and the vertical combustion grade is V-0, which belongs to the level of flame-retardant materials. This is because the triazine structure in the multi-arm maleimide flame retardant has an excellent carbonizing effect, which absorbs heat and decomposes at high temperatures, releasing nitrogen, promoting the formation of a foam carbon protective layer, and effectively preventing the material from further burning; at the same time, organic phosphorus is thermally decomposed to generate phosphoric acid and pyrophosphoric acid with strong dehydration effect, which can form on the surface of the material. The solid phase layer isolates air and heat, and the ammonia generated by its decomposition can also isolate air. Phosphoric acid catalysis promotes the formation of carbon; triazine carbon formers and organic phosphorus synergistically flame retardant, forming a dense expanded carbon layer during the combustion process, which promptly takes away the heat and flammable small molecules generated by the combustion; in addition, the maleimide group has a highly active double bond functional group. During the mixing and vulcanization process with EPDM rubber, the active double bond opens and forms a "bridge bond" cross-linking with EPDM rubber to form a cross-linked network structure, which promotes carbonization, thereby stopping the combustion of the material and further improving the flame retardant properties of the rubber material.
[0072] Comparative Example 1 and Comparative Example 3 do not contain flame retardants and have no flame retardant effect; Comparative Example 2 contains flame retardants and has good flame retardant properties.
[0073] Mechanical properties test: The test was carried out using an electronic tensile testing machine in accordance with GB / T 528-1998, with a tensile speed of 200 mm / min.
[0074] Table 2 Mechanical properties test
[0075] Tensile strength(MPa) Tear strength (kN / m) Example 1 23.2 34.1 Example 2 24.5 37.3 Example 3 25.3 42.5 Example 4 26.8 50.2 Example 5 26.0 47.4 Comparative Example 1 22.6 33.5 Comparative Example 2 21.4 31.8 Comparative Example 3 20.1 30.2
[0076] It can be seen from the test results in the above table that with the increase of the content of multi-arm maleimide flame retardant and modified nano silicon nitride, the mechanical properties of EPDM rubber are gradually enhanced, wherein the tensile strength in Example 4 is 26.8MPa, and the tear strength is 50.2kN / m. This is because, on the one hand, the multiple maleimide groups in the multi-arm maleimide flame retardant have double bond functional groups with higher activity. During the mixing and vulcanization process with EPDM rubber, the active double bonds are opened to form a "bridge bond" cross-linked network structure, which enhances the ability to resist external stress; on the other hand, the modified nano silicon nitride has good compatibility with the EPDM rubber system, improves the interface between nano silicon nitride and EPDM rubber, forms a relatively uniform dispersion system between the two, plays a significant reinforcing role, and then exerts the characteristics of inorganic nanoparticles to improve the impact resistance of the rubber; in Comparative Example 2, the nano silicon nitride is not modified, and its compatibility with the EPDM rubber matrix is poor, resulting in poor mechanical properties.
[0077] Liquid permeability test: An electric waterproof tester was used to test the liquid permeability of the material. The prepared EPDM rubber was cut into circular specimens with a diameter of 35 mm and kept under a pressure of 0.3 MPa (equivalent to a 30 m water column) for 24 hours. The water absorption quality was tested after 24 hours. The water absorption rate of the specimen was calculated based on the change in mass before and after water absorption. Water absorption rate = (m2-m1) / S×100%, where m1 is the mass of the specimen before water absorption (g), m2 is the mass of the specimen after water absorption (g), and S is the area of the specimen (m 2 ).
[0078] Gas permeability performance test: The gas permeability coefficient of the material was determined according to GB / T 1038-2000. The prepared EPDM rubber was cut into circular specimens with a diameter of 5 cm. The thickness was averaged by 5-point testing. The experimental gas was nitrogen, the experimental temperature was 40°C, and the degassing time was 12 h.
[0079] Table 3 Sealing performance test
[0080]
[0081]
[0082] It can be seen from the test results in the above table that the water absorption rate and air permeability coefficient of the EPDM rubber prepared by the present invention are significantly reduced within the same period of time, and the material has good liquid and gas barrier properties and a good sealing effect; this is because the prepared EPDM rubber contains a dense cross-linked network structure, which hinders the penetration of gas and liquid into the interior of the material, thereby broadening its further application in sealing products.
[0083] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. An impact-resistant EPDM rubber, characterized in that: The EPDM rubber comprises the following components in parts by weight: 100 parts of EPDM rubber, 10-20 parts of carbon black, 3-15 parts of modified nano silicon nitride, 2-10 parts of multi-arm maleimide flame retardant, 2-5 parts of zinc oxide, 3-7 parts of stearic acid, 0.5-1 parts of dicumyl peroxide, 1-3 parts of sulfur and 0.8-1.5 parts of accelerator M; The preparation method of impact-resistant EPDM rubber is as follows: EPDM rubber and modified nano silicon nitride are mixed in an internal mixer at a temperature of 110-130°C and a rotation speed of 150-200r / min until the rollers are covered, carbon black, multi-arm maleimide flame retardant, zinc oxide, stearic acid, diisopropylbenzene peroxide, accelerator M and sulfur are added in sequence, mixed for 10-20 minutes, discharged, and then pressed into thin sheets through a double-roll open mill, left at room temperature for 16-32 hours, the thin sheets are placed in a mold, and placed on a flat vulcanizer for vulcanization to obtain impact-resistant EPDM rubber.
2. The impact-resistant EPDM rubber according to claim 1, characterized in that: The vulcanization temperature is 150-170° C., the vulcanization pressure is 10-20 MPa, and the vulcanization time is 5-15 min.
3. The impact-resistant EPDM rubber according to claim 1, characterized in that: The preparation method of the multi-arm maleimide flame retardant is: Step (1), under a nitrogen atmosphere, add 4,6-dichloro-1,3,5-triazine ring-2-amine, 4-nitrophenylboric acid, potassium carbonate and toluene to a reaction flask, stir evenly, add tetrakis(triphenylphosphine)palladium, stir to react, after the reaction is completed, cool to room temperature, filter, recrystallize from ethanol, and dry to obtain a structural formula of Intermediate 1; Step (2), under nitrogen atmosphere, add ethyl dichlorophosphate and acetonitrile to a reaction flask, stir evenly, add intermediate 1 and triethylamine, react at 35-50° C. for 5-10 h, filter, wash with ethanol, and dry to obtain a product having the structural formula: Intermediate 2; Step (3), under nitrogen atmosphere, add intermediate 2 and ethanol to the reaction flask, heat to 50-65°C, add 30-40% ammonium chloride solution and iron powder under stirring, continue to react for 2-5h, filter, wash with ethyl acetate, concentrate and dry to obtain a compound with the structural formula Intermediate 3; Step (4), under nitrogen atmosphere, add intermediate 3 and N-methylpyrrolidone to the reaction flask, stir evenly, add maleic anhydride, react at 160-180°C for 3-6h, cool to room temperature, filter and dry to obtain the structural formula Multi-arm maleimide flame retardant.
4. The impact-resistant EPDM rubber according to claim 3, characterized in that: In the step (1), the molar ratio of 4,6-dichloro-1,3,5-triazine ring-2-amine, 4-nitrophenylboric acid, potassium carbonate and tetrakis(triphenylphosphine)palladium is 1:(2.05-2.2):(2.1-2.3):(0.15-0.25).
5. The impact-resistant EPDM rubber according to claim 3, characterized in that: In the step (1), the reaction temperature is 80-100° C. and the reaction time is 12-24 h.
6. The impact-resistant EPDM rubber according to claim 3, characterized in that: In the step (2), the molar ratio of ethyl dichlorophosphate, intermediate 1 and triethylamine is 1:(2-2.15):(2.3-2.5).
7. The impact-resistant EPDM rubber according to claim 3, characterized in that: The molar ratio of the intermediate 2, the ammonium chloride solution and the iron powder in the step (3) is 1:(10-15):(6-9).
8. The impact-resistant EPDM rubber according to claim 3, characterized in that: The molar ratio of the intermediate 3 to maleic anhydride in the step (4) is 1:(4.5-6).
9. Use of the impact-resistant EPDM rubber according to any one of claims 1 to 8 in sealing products.
Citation Information
Patent Citations
Zinc polymethacrylate coating modified nano nitride powder and use thereof
CN101148491A
Flame-retardant insulating rubber and preparation method thereof
CN110498975A
Modified polyvinylidene fluoride lithium ion battery diaphragm and preparation method thereof
CN117691301A
Multimode degradable hydrogels for controlled release of cargo substances
WO2015168090A1
Rubber composite, processing method, applications, manufacturing method for the applications
WO2018130195A1