Antistatic PVC plastic and preparation method thereof

By introducing modified carbon black and imidazole bromide ionic liquid into PVC materials, the problem of static electricity accumulation in PVC materials is solved, the antistatic performance is significantly improved, and it is suitable for places where static electricity is easy to accumulate.

CN118791809AInactive Publication Date: 2024-10-18DONGGUAN ANSHUYI POLYMER MATERIAL TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411055471.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

PVC materials are prone to static electricity accumulation during processing and use, leading to static electricity hazards, especially in places such as micro device production workshops, laboratories, and operating rooms, causing serious losses.

Method used

An antistatic PVC plastic is used, which includes PVC resin, plasticizer, modified carbon black as an antistatic agent and stearate, and reacts with the carbon black surface through hydrolysis of the silane coupling agent, and the photoinitiator promotes 1-ethylene The base imidazole is grafted, and the imidazole bromide ionic liquid is formed through the reaction of 2,2,6,6-tetramethylpiperidine-oxide and chloroacetyl chloride. The synergistic effect of carbon black and ionic liquid gives the material excellent resistance to Electrostatic properties.

Benefits of technology

Significantly improves the antistatic properties of PVC materials. Through the compatibility of modified carbon black and PVC matrix, it reduces static electricity hazards and is suitable for special places where static electricity is easy to accumulate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004976258730000091
    Figure BDA0004976258730000091
Patent Text Reader

Abstract

The invention discloses an antistatic PVC plastic and a preparation method thereof, and belongs to the technical field of antistatic materials, the antistatic PVC plastic comprises the following raw materials by weight: 80-100 parts of PVC resin, 15-35 parts of a plasticizer, 3-8 parts of an antistatic agent, 4-6 parts of a heat stabilizer, and 1-3 parts of stearate; pVC is used as a matrix, the plastic is endowed with excellent antistatic performance by adding the antistatic agent, the antistatic agent can endow the matrix with excellent antistatic performance through the synergistic effect of carbon black and ionic liquid, and a 2, 2, 6, 6-tetramethylpiperidine-nitrogen-oxide structure introduced into the antistatic agent has good compatibility with the PVC matrix, so that the antistatic performance of the plastic is improved. Furthermore, the compatibility of the antistatic agent and a matrix can be improved, and good antistatic performance is exerted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of antistatic materials, and in particular to an antistatic PVC plastic and a preparation method thereof. Background Art

[0002] Polyvinyl chloride (PVC) is formed by the polymerization of vinyl chloride monomers and is a thermoplastic plastic whose current output is second only to polyethylene. Its application areas are very broad, ranging from electrical insulation materials in the industrial and agricultural industries, building frames, interior decoration, agricultural rain shelters, etc. to daily necessities. However, due to the presence of polar groups, PVC has a high resistivity, which is prone to static electricity accumulation during processing and use, causing static electricity hazards and affecting normal use. Especially in special places, such as: micro-device manufacturing workshops, laboratories, operating rooms, etc., the static electricity hazards generated by devices made of PVC will cause serious losses. Summary of the invention

[0003] In order to solve the above technical problems, the present invention provides an antistatic PVC plastic and a preparation method thereof.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] An antistatic PVC plastic comprises the following raw materials in parts by weight: 80-100 parts of PVC resin, 15-35 parts of plasticizer, 3-8 parts of antistatic agent, 4-6 parts of heat stabilizer, and 1-3 parts of stearate;

[0006] The antistatic agent is prepared by the following steps:

[0007] Step S1, mixing KH-590, ethanol and acetic acid and stirring them magnetically for 30 minutes, then adding carbon black, stirring for 30 minutes, heating to 70-80°C, and reacting for 4-6 hours. After the reaction is completed, filtering, washing and drying are performed to obtain modified carbon black, and the dosage ratio of KH-590, ethanol, acetic acid and carbon black is controlled to be 0.05-0.08g:30-35mL:1-1.2mL:1g;

[0008] In step S1, the silane coupling agent KH-590 is hydrolyzed and condensed with the hydroxyl groups on the surface of carbon black to be grafted onto the surface of carbon black;

[0009] Step S2, adding modified carbon black and 1-vinylimidazole to dichloromethane, stirring at a uniform speed and adding a photoinitiator (2,2-dimethoxy-2-phenylacetophenone), placing under a 300W ultraviolet lamp for irradiation and reaction for 1 hour, and obtaining modified carbon black after the reaction is completed, controlling the amount ratio of modified carbon black, 1-vinylimidazole and dichloromethane to be 0.5-0.8g: 0.02-0.05g: 50mL, and the amount of the photoinitiator to be 0.3-0.5% of the weight of the modified carbon black;

[0010] In step S2, under the action of a photoinitiator, the thiol group on the surface of the carbon black reacts with the carbon-carbon double bond on 1-vinylimidazole, thereby grafting 1-vinylimidazole on the surface of the carbon black;

[0011] Step S3, adding 2,2,6,6-tetramethylpiperidine-nitrogen-oxide and chloroacetylphthalide to dichloromethane, stirring at a uniform speed in an ice-water bath and reacting for 12 hours, filtering after the reaction, washing with deionized water and then rotary evaporating to obtain an intermediate, wherein the amount ratio of 2,2,6,6-tetramethylpiperidine-nitrogen-oxide, chloroacetylphthalide and dichloromethane is controlled to be 0.15-0.2g:10-12g:10-15mL;

[0012] In step S3, 2,2,6,6-tetramethylpiperidine-nitrogen-oxide is reacted with chloroacetyl chloride to obtain an intermediate;

[0013] Step S4, adding the prepared intermediate and modified carbon black to acetonitrile, heating to 75-80°C, stirring at a uniform speed and reacting for 24 hours, filtering after the reaction is completed to obtain an antistatic agent, and controlling the weight ratio of modified carbon black, intermediate and acetonitrile to be 1:0.2-0.5:10.

[0014] In step S4, the chlorine on the intermediate reacts with the imidazole group on the modified carbon black to form an imidazole bromide ionic liquid. Through the synergistic effect of carbon black and the ionic liquid, the substrate can be endowed with excellent antistatic properties. In addition, the 2,2,6,6-tetramethylpiperidine-nitrogen-oxide structure introduced in the antistatic agent has good compatibility with the PVC substrate, thereby improving the compatibility of the antistatic agent with the substrate and exerting good antistatic properties.

[0015] Furthermore, the stearate is barium stearate.

[0016] A method for preparing antistatic PVC plastic comprises the following steps:

[0017] After mixing the raw materials, stir them at a speed of 500-800 r / min for 2-2.5 minutes to obtain a mixed material, which is then sent to a twin-screw extruder for extrusion and granulation to obtain an antistatic PVC plastic.

[0018] The temperature of each section of the twin-screw extruder is 1#120℃, 2#130℃, 3#150℃, 4#160℃, 5#160℃, 6#150℃, 7#145℃, and the die head is 140℃.

[0019] Beneficial effects of the present invention:

[0020] The invention prepares an antistatic PVC plastic. The PVC is used as a matrix and an antistatic agent is added to give the plastic excellent antistatic performance. In the preparation process, the antistatic agent is firstly hydrolyzed by a silane coupling agent KH-590 and then condensed with a hydroxyl group on a carbon black surface and then grafted on the carbon black surface. Then, under the action of a photoinitiator, the thiol group on the surface of the modified carbon black reacts with a carbon-carbon double bond on 1-vinyl imidazole, and then 1-vinyl imidazole is grafted on the surface of the carbon black. Then, 2,2,6,6-tetramethylpiperidine-nitrogen-oxide reacts with chloroacetyl chloride to obtain an intermediate. Finally, the chlorine on the intermediate reacts with an imidazole group on the modified carbon black to form an imidazole bromide ionic liquid. The synergistic effect of the carbon black and the ionic liquid can give the matrix excellent antistatic performance. Moreover, the 2,2,6,6-tetramethylpiperidine-nitrogen-oxide structure introduced in the antistatic agent has good compatibility with the PVC matrix, thereby improving the compatibility of the antistatic agent with the matrix and exerting good antistatic performance. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] An antistatic PVC plastic comprises the following raw materials in parts by weight: 80 parts of PVC resin, 15 parts of plasticizer DOP, 3 parts of antistatic agent, 4 parts of aluminum salt composite stabilizer, and 1 part of barium stearate;

[0024] A method for preparing antistatic PVC plastic comprises the following steps:

[0025] The raw materials were mixed and stirred at a speed of 500 r / min for 2 minutes to obtain a mixture, which was then sent to a twin-screw extruder for extrusion and granulation to obtain an antistatic PVC plastic.

[0026] The temperature of each section of the twin-screw extruder is 1#120℃, 2#130℃, 3#150℃, 4#160℃, 5#160℃, 6#150℃, 7#145℃, and the die head is 140℃.

[0027] The antistatic agent is prepared by the following steps:

[0028] Step S1, mixing KH-590, ethanol and acetic acid and stirring them magnetically for 30 minutes, then adding carbon black, stirring for 30 minutes, heating to 70°C, and reacting for 4 hours. After the reaction is completed, filtering, washing and drying are performed to obtain modified carbon black, and the dosage ratio of KH-590, ethanol, acetic acid and carbon black is controlled to be 0.05g:30mL:1mL:1g;

[0029] Step S2, adding modified carbon black and 1-vinylimidazole to dichloromethane, stirring at a uniform speed and adding a photoinitiator 2,2-dimethoxy-2-phenylacetophenone, placing under a 300W ultraviolet lamp for irradiation and reaction for 1 hour, and obtaining modified carbon black after the reaction is completed, and controlling the amount ratio of modified carbon black, 1-vinylimidazole and dichloromethane to be 0.5g:0.02g:50mL, and the amount of the photoinitiator to be 0.3% of the weight of the modified carbon black;

[0030] Step S3, adding 2,2,6,6-tetramethylpiperidine-nitrogen-oxide and chloroacetylphthalide to dichloromethane, stirring at a uniform speed in an ice-water bath and reacting for 12 hours, filtering after the reaction, washing with deionized water and then rotary evaporating to obtain an intermediate, wherein the amount ratio of 2,2,6,6-tetramethylpiperidine-nitrogen-oxide, chloroacetylphthalide and dichloromethane is controlled to be 0.15g:10g:10mL;

[0031] Step S4, adding the prepared intermediate and modified carbon black to acetonitrile, heating to 75°C, stirring at a uniform speed and reacting for 24 hours, filtering after the reaction is completed to obtain an antistatic agent, and controlling the weight ratio of modified carbon black, intermediate and acetonitrile to be 1:0.2:10.

[0032] Example 2

[0033] An antistatic PVC plastic comprises the following raw materials in parts by weight: 90 parts of PVC resin, 20 parts of plasticizer DOP, 5 parts of antistatic agent, 5 parts of aluminum salt composite stabilizer, and 2 parts of barium stearate;

[0034] A method for preparing antistatic PVC plastic comprises the following steps:

[0035] The raw materials were mixed and stirred at a speed of 600 r / min for 2.2 minutes to obtain a mixture, which was then sent to a twin-screw extruder for extrusion and granulation to obtain an antistatic PVC plastic.

[0036] The temperature of each section of the twin-screw extruder is 1#120℃, 2#130℃, 3#150℃, 4#160℃, 5#160℃, 6#150℃, 7#145℃, and the die head is 140℃.

[0037] The antistatic agent is prepared by the following steps:

[0038] Step S1, mixing KH-590, ethanol and acetic acid and stirring magnetically for 30 minutes, then adding carbon black, stirring for 30 minutes, heating to 70°C, and reacting for 4 hours. After the reaction is completed, filtering, washing and drying are performed to obtain modified carbon black, and the dosage ratio of KH-590, ethanol, acetic acid and carbon black is controlled to be 0.06g:32mL:1.1mL:1g;

[0039] Step S2, adding modified carbon black and 1-vinylimidazole to dichloromethane, stirring at a uniform speed and adding a photoinitiator 2,2-dimethoxy-2-phenylacetophenone, placing under a 300W ultraviolet lamp for irradiation and reaction for 1 hour, and obtaining modified carbon black after the reaction is completed, and controlling the amount ratio of modified carbon black, 1-vinylimidazole and dichloromethane to be 0.6g:0.04g:50mL, and the amount of the photoinitiator to be 0.4% of the weight of the modified carbon black;

[0040] Step S3, adding 2,2,6,6-tetramethylpiperidine-nitrogen-oxide and chloroacetylphthalide to dichloromethane, stirring at a uniform speed in an ice-water bath and reacting for 12 hours, filtering after the reaction, washing with deionized water and then rotary evaporating to obtain an intermediate, wherein the amount ratio of 2,2,6,6-tetramethylpiperidine-nitrogen-oxide, chloroacetylphthalide and dichloromethane is controlled to be 0.16g:10g:12mL;

[0041] Step S4, adding the prepared intermediate and modified carbon black to acetonitrile, heating to 78°C, stirring at a uniform speed and reacting for 24 hours, filtering after the reaction is completed to obtain an antistatic agent, and controlling the weight ratio of modified carbon black, intermediate and acetonitrile to be 1:0.3:10.

[0042] Example 3

[0043] An antistatic PVC plastic comprises the following raw materials in parts by weight: 90 parts of PVC resin, 32 parts of plasticizer DOP, 6 parts of antistatic agent, 5 parts of aluminum salt composite stabilizer, and 2 parts of barium stearate;

[0044] A method for preparing antistatic PVC plastic comprises the following steps:

[0045] The raw materials were mixed and stirred at a speed of 800 r / min for 2.5 minutes to obtain a mixture, which was then sent to a twin-screw extruder for extrusion and granulation to obtain an antistatic PVC plastic.

[0046] The temperature of each section of the twin-screw extruder is 1#120℃, 2#130℃, 3#150℃, 4#160℃, 5#160℃, 6#150℃, 7#145℃, and the die head is 140℃.

[0047] The antistatic agent is prepared by the following steps:

[0048] Step S1, mixing KH-590, ethanol and acetic acid and stirring them magnetically for 30 minutes, then adding carbon black, stirring for 30 minutes, heating to 80°C, and reacting for 6 hours. After the reaction is completed, filtering, washing and drying are performed to obtain modified carbon black, and the dosage ratio of KH-590, ethanol, acetic acid and carbon black is controlled to be 0.07g:35mL:1.1mL:1g;

[0049] Step S2, adding modified carbon black and 1-vinylimidazole to dichloromethane, stirring at a uniform speed and adding a photoinitiator 2,2-dimethoxy-2-phenylacetophenone, placing under a 300W ultraviolet lamp for irradiation and reaction for 1 hour, and obtaining modified carbon black after the reaction is completed, wherein the amount ratio of modified carbon black, 1-vinylimidazole and dichloromethane is controlled to be 0.7g:0.04g:50mL, and the amount of the photoinitiator is 0.3-0.5% of the weight of the modified carbon black;

[0050] Step S3, adding 2,2,6,6-tetramethylpiperidine-nitrogen-oxide and chloroacetylphthalide to dichloromethane, stirring at a uniform speed in an ice-water bath and reacting for 12 hours, filtering after the reaction, washing with deionized water and then rotary evaporating to obtain an intermediate, wherein the amount ratio of 2,2,6,6-tetramethylpiperidine-nitrogen-oxide, chloroacetylphthalide and dichloromethane is controlled to be 0.19 g:12 g:15 mL;

[0051] Step S4, adding the prepared intermediate and modified carbon black to acetonitrile, heating to 80°C, stirring at a uniform speed and reacting for 24 hours, filtering after the reaction is completed to obtain an antistatic agent, and controlling the weight ratio of modified carbon black, intermediate and acetonitrile to be 1:0.5:10.

[0052] Example 4

[0053] An antistatic PVC plastic comprises the following raw materials in parts by weight: 100 parts of PVC resin, 35 parts of plasticizer DOP, 8 parts of antistatic agent, 6 parts of aluminum salt composite stabilizer, and 3 parts of barium stearate;

[0054] A method for preparing antistatic PVC plastic comprises the following steps:

[0055] The raw materials were mixed and stirred at a speed of 800 r / min for 2.5 minutes to obtain a mixture, which was then sent to a twin-screw extruder for extrusion and granulation to obtain an antistatic PVC plastic.

[0056] The temperature of each section of the twin-screw extruder is 1#120℃, 2#130℃, 3#150℃, 4#160℃, 5#160℃, 6#150℃, 7#145℃, and the die head is 140℃.

[0057] The antistatic agent is prepared by the following steps:

[0058] Step S1, mixing KH-590, ethanol and acetic acid and stirring them magnetically for 30 minutes, then adding carbon black, stirring for 30 minutes, heating to 80°C, and reacting for 6 hours. After the reaction is completed, filtering, washing and drying are performed to obtain modified carbon black, and the dosage ratio of KH-590, ethanol, acetic acid and carbon black is controlled to be 0.08g:35mL:1.2mL:1g;

[0059] Step S2, adding modified carbon black and 1-vinylimidazole to dichloromethane, stirring at a uniform speed and adding a photoinitiator 2,2-dimethoxy-2-phenylacetophenone, placing under a 300W ultraviolet lamp for irradiation and reaction for 1 hour, and obtaining modified carbon black after the reaction is completed, and controlling the amount ratio of modified carbon black, 1-vinylimidazole and dichloromethane to be 0.8g:0.05g:50mL, and the amount of the photoinitiator to be 0.5% of the weight of the modified carbon black;

[0060] Step S3, adding 2,2,6,6-tetramethylpiperidine-nitrogen-oxide and chloroacetylphthalide to dichloromethane, stirring at a uniform speed in an ice-water bath and reacting for 12 hours, filtering after the reaction, washing with deionized water and then rotary evaporating to obtain an intermediate, wherein the amount ratio of 2,2,6,6-tetramethylpiperidine-nitrogen-oxide, chloroacetylphthalide and dichloromethane is controlled to be 0.2g:12g:15mL;

[0061] Step S4, adding the prepared intermediate and modified carbon black to acetonitrile, heating to 80°C, stirring at a uniform speed and reacting for 24 hours, filtering after the reaction is completed to obtain an antistatic agent, and controlling the weight ratio of modified carbon black, intermediate and acetonitrile to be 1:0.5:10.

[0062] Comparative Example 1

[0063] Compared with Example 1, this comparative example uses carbon black as an antistatic agent, and the rest is the same as Example 1.

[0064] Comparative Example 2

[0065] This comparative example is an antistatic PVC plastic produced by a certain company on the market.

[0066] The properties of the PVC plastics prepared in Examples 1-4 and Comparative Examples 1-2 were tested, and the results are shown in Table 1 below:

[0067] Table 1

[0068]

[0069] It can be seen from Table 1 above that the PVC plastics prepared in Examples 1-4 of the present invention have excellent mechanical properties. The antistatic agent based on carbon black is added. By modifying the carbon black, the compatibility of the carbon black and the PVC material is improved. The PVC plastics have excellent mechanical properties and improved antistatic properties. In addition, the synergistic effect of carbon black and ionic liquid can give the matrix excellent antistatic properties.

[0070] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. An antistatic PVC plastic, characterized in that: The method comprises the following raw materials in parts by weight: 80-100 parts of PVC resin, 15-35 parts of plasticizer, 3-8 parts of antistatic agent, 4-6 parts of heat stabilizer, and 1-3 parts of stearate; The antistatic agent is prepared by the following steps: Step S1, mixing KH-590, ethanol and acetic acid, and magnetically stirring for 30 minutes, then adding carbon black, continuing to stir for 30 minutes, heating to 70-80°C, and continuing to react for 4-6 hours. After the reaction is completed, filtering, washing and drying are performed to obtain modified carbon black; Step S2, adding the modified carbon black and 1-vinyl imidazole into dichloromethane, stirring at a uniform speed and adding a photoinitiator, placing under a 300 W ultraviolet lamp for irradiation for 1 hour, and obtaining the modified carbon black after the reaction is completed; Step S3, adding 2,2,6,6-tetramethylpiperidine-nitrogen-oxide and chloroacetyl chloride to dichloromethane, stirring at a uniform speed in an ice-water bath and reacting for 12 hours, filtering after the reaction, washing with deionized water and rotary evaporating to obtain an intermediate; Step S4, adding the obtained intermediate and modified carbon black into acetonitrile, heating to 75-80° C., stirring at a uniform speed and reacting for 24 hours, filtering after the reaction is completed, and obtaining an antistatic agent.

2. The antistatic PVC plastic according to claim 1, characterized in that: In step S1, the dosage ratio of KH-590, ethanol, acetic acid and carbon black is controlled to be 0.05-0.08 g: 30-35 mL: 1-1.2 mL: 1 g.

3. The antistatic PVC plastic according to claim 1, characterized in that: In step S2, the dosage ratio of modified carbon black, 1-vinylimidazole and dichloromethane is controlled to be 0.5-0.8 g: 0.02-0.05 g: 50 mL, and the dosage of the photoinitiator is 0.3-0.5% of the weight of the modified carbon black.

4. The antistatic PVC plastic according to claim 1, characterized in that: In step S3, the dosage ratio of 2,2,6,6-tetramethylpiperidine-nitrogen-oxide, chloroacetyl chloride and dichloromethane is controlled to be 0.15-0.2 g: 10-12 g: 10-15 mL.

5. The antistatic PVC plastic according to claim 1, characterized in that: In step S4, the weight ratio of modified carbon black, intermediate and acetonitrile is controlled to be 1:0.2-0.5:

10.

6. The antistatic PVC plastic according to claim 1, characterized in that: The stearate is barium stearate.

7. The method for preparing an antistatic PVC plastic according to claim 1, characterized in that: The steps include: The raw materials are mixed and stirred at a speed of 500-800 r / min for 2-2.5 minutes to obtain a mixed material, which is then sent to a twin-screw extruder for extrusion and granulation to obtain an antistatic PVC plastic.

Citation Information

Cited By

  • Preparation method, product and application of antistatic pre-dispersion for PVC (polyvinyl chloride) film

    CN119529582A

  • A method for preparing an antistatic predispersant for PVC film, the product and its application

    CN119529582B