High heat resistant and high impact resistant pMMA composition

By using a core-shell impact modifier with a particle size of 150-300 nm in a hydrophobic high Tg copolymer, the lack of heat resistance and impact resistance of existing impact-modified acrylic compositions in high-performance applications is solved solve the problem and achieve high impact resistance, water mist resistance and melt fluidity improvement. It is suitable for applications such as automotive LEDs and mobile phone front films.

CN118791817APending Publication Date: 2024-10-18TRINSEO EURO GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410420149.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-04-09
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing commercial impact-modified acrylic compositions lack high heat resistance, high impact resistance, water mist resistance and sufficient melt fluidity in high-performance applications, and cannot meet the high-performance needs of automotive LEDs, mobile phone front films, etc. .

Method used

A composition containing a hydrophobic acrylic copolymer and a core-shell impact modifier was developed. By incorporating a core-shell impact modifier with a particle size of 150-300 nm into the hydrophobic high Tg copolymer, Improves the impact resistance and water mist resistance of the composition and optimizes its melt flow.

Benefits of technology

It achieves high impact resistance, excellent water mist resistance, sufficient melt fluidity and long-term weather resistance. It is suitable for high-performance applications such as automotive LEDs and mobile phone front films, and significantly improves the performance of the composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004782155970000051
    Figure BDA0004782155970000051
  • Figure BDA0004782155970000052
    Figure BDA0004782155970000052
  • Figure BDA0004782155970000161
    Figure BDA0004782155970000161
Patent Text Reader

Abstract

An impact-modified hydrophobic acrylic composition comprising (a) a hydrophobic acrylic copolymer having (i) monomeric units selected from the group consisting of tert-butylcyclohexyl methacrylate, 3, 3, 5-trimethylcyclohexyl (meth) acrylate, and mixtures thereof, (ii) methyl methacrylate monomeric units, and (iii) optionally, optionally, an acrylic monomer selected from the group consisting of tert-butylcyclohexyl methacrylate, 3, 3, 5-trimethylcyclohexyl (meth) acrylate, and mixtures thereof, and optionally, an acrylic monomer selected from the group consisting of tert-butylcyclohexyl methacrylate, 3, 3, 5-trimethylcyclohexyl (meth) acrylate, and mixtures thereof. Other monomer units capable of copolymerizing with methyl methacrylate; (b) optionally, another (meth) acrylic copolymer; (c) one or more core-shell impact modifiers wherein the core-shell impact modifiers have a volume average particle size of from 70 nm to 350 nm wherein the impact-modified hydrophobic acrylic composition has a melt flow rate of greater than 1.0 / 10 minutes at 230 DEG C at 3.8 kg; and wherein the notched Izod impact strength of the impact modified hydrophobic acrylic composition is greater than 4.5 kJ / m < 2 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to impact modified hydrophobic acrylic copolymer compositions. Background Art

[0002] Thermoplastic polymers and copolymers, especially (meth)acrylic polymers, have excellent characteristics such as transparency, mechanical properties and processability, and are widely used in various fields such as automobile parts, electrical parts, industrial parts, optical materials, various parts for home appliances, aesthetic parts, groceries, etc.

[0003] High Tg acrylic polymers can be used in applications requiring high optical clarity and high heat resistance, such as automotive front interior lenses, thin-walled parts, lighting tubes, optical protection / retardation films in electronic devices, solar panels / films, mobile phone back covers, pMMA / PC front films for mobile phones and tablets, home appliances, composite materials, etc.

[0004] The impact resistance of acrylic resins can be improved by incorporating high levels of impact modifiers. However, current commercial impact-modified acrylic compositions do not have the combination of high heat resistance, high impact resistance, water spray resistance, sufficient melt flow and weather resistance required for high-performance applications such as automotive LED front / rear signature lighting tubes, automotive LED grille lighting, automotive LED headlight covers, optical protective films and / or moisture-proof films in emblems, automotive black trim / pillars, pMMA / PC front films for mobile phones and tablets, surface protection layers for co-extruded products / 3D complex profiles, railings / covers, etc. Summary of the invention

[0005] According to a first aspect of the present invention, a product comprising a reactive impact-modified hydrophobic acrylic composition is disclosed. The composition comprises 40 wt % to 95 wt %, preferably 50 wt % to 90 wt %, more preferably 50 wt % to 80 wt %, most preferably 55 wt % to 70 wt % of a hydrophobic acrylic copolymer based on the weight of the hydrophobic polymer plus the impact modifier. The hydrophobic acrylic copolymer may be characterized by having a Tg of 111° C. to 140° C., preferably 113° C. to 135° C., preferably 115° C. to 130° C., more preferably 116° C. to 125° C. The hydrophobic acrylic copolymer may be further characterized by

[0006] 1) 0.1 to 20% by weight, preferably 0.3 to 10% by weight, more preferably 0.5 to 5% by weight of monomer units selected from tert-butylcyclohexyl methacrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate and mixtures thereof;

[0007] 2) 50 to 80 wt% of methyl methacrylate monomer units;

[0008] 3) optionally 0% to 49.9% by weight of other monomer units copolymerizable with methyl methacrylate;

[0009] Each of the foregoing percentages is based on the total monomer units in the hydrophobic acrylic copolymer.

[0010] The composition further comprises 5 to 60 wt %, preferably 10 to 50 wt %, more preferably 20 to 50 wt %, most preferably 30 to 45 wt % of one or more core-shell impact modifiers. The core-shell impact modifier has a volume average particle size of 70 nm to 350 nm, preferably 100-350 nm, preferably 150-300, more preferably 200-250 nm; wherein the Tg of the shell layer is greater than 105° C., preferably greater than 107° C. (Cb). Optionally, the composition further comprises other (meth)acrylic copolymers.

[0011] The impact-modified hydrophobic acrylic composition has a melt flow rate of greater than 1.0 g / 10 min at 230° C. under 3.8 kg, preferably greater than 1.2 g / 10 min, and more preferably greater than 1.5 g / 10 min; and wherein the impact-modified hydrophobic acrylic composition has a notched Izod impact strength of greater than 4.5 kJ / m 2 , preferably greater than 5.4 kJ / m 2 , and more preferably greater than 6.4 kJ / m 2 .

[0012] According to another embodiment, an article made from the impact-modified hydrophobic acrylic composition of the present invention is disclosed. Exemplary articles include automotive LED headlight covers, automotive LED front / rear signature lighting tubes, optical films, moisture-proof films, digital printing films, weather-resistant surface protection layers, surface protection layers for cover panels / rails, automobiles, electronic devices, medical, digital printing, laser cutting, architecture and construction, lighting tubes, thin-walled parts, optical lenses, extruded films, (co)extruded sheets / profiles, thermoformable sheets, cast sheets, composite materials, medical devices and LED / OLED displays. DETAILED DESCRIPTION

[0013] The inventors have now developed and optimized an impact-modified acrylic composition that incorporates a selected core-shell acrylic impact modifier with a particle size diameter of 150-300 nm into a hydrophobic high-heat pMMA copolymer. The resulting composition has high impact resistance, excellent water mist resistance, sufficiently high melt flowability, and excellent long-term weather resistance. The new hydrophobic pMMA impact-resistant composition can be used for automotive LED front / rear signature lighting tubes, automotive LED headlight covers, automotive LED grille lighting, LED front thick lenses, automotive black trim / pillars, window profiles, trim / railings, coating materials / surface protection layers, co-extruded sheets, medical devices, pMMA / PC front films for mobile phones and tablets, electronic components, etc.

[0014] As used herein, "copolymer" means a polymer having two or more different monomer units, including copolymers and polymers having three or more different monomers, such as terpolymers and tetrapolymers. Therefore, the term "copolymer, terpolymer and tetrapolymer" covers any polymer having more than one type of comonomer. "Polymer" is used to mean homopolymers and copolymers. The polymer may be linear, branched, star-shaped, comb-shaped, block or any other structure. The polymer may be homogeneous, heterogeneous, and may have a gradient distribution of comonomer units. All cited documents are incorporated herein by reference. As used herein, unless otherwise described, percentages shall mean weight percentages. Molecular weight is the weight average molecular weight measured by gel permeation chromatography (GPC) using polymethyl methacrylate standards. In the case where the polymer contains some crosslinking and GPC cannot be applied due to the insoluble polymer fraction, the weight average molecular weight is determined using the soluble fraction / gel fraction or soluble fraction molecular weight after extraction from the gel.

[0015] As used herein, "hydrophobic" means that the pMMA copolymer contains at least 0.2 weight percent of tert-butylcyclohexyl (meth)acrylate and / or 3,3,5-trimethylcyclohexyl (meth)acrylate hydrophobic monomer units.

[0016] As used herein, "(meth)acrylic" or "(meth)acrylate" means both acrylate and methacrylate.

[0017] In one embodiment, the hydrophobic copolymer of the present invention passes the 85°C / 85%RH test. In another embodiment, the hydrophobic copolymer of the present invention passes the -40°C to 80°C / 85%RH humidity freeze cycle test.

[0018] Hydrophobic high Tg copolymers or terpolymers

[0019] "High Tg monomer" refers to a monomer that, when polymerized, produces a polymer having a Tg greater than 116° C., and more preferably greater than 120° C., and more preferably greater than 130° C. Examples of useful hydrophobic high Tg monomers include, but are not limited to, tert-butylcyclohexyl methacrylate, and 3,3,5-trimethylcyclohexyl (meth)acrylate, and isomeric blends thereof.

[0020] The hydrophobic high Tg monomer is polymerized with methyl methacrylate and optionally other acrylic monomers to form the hydrophobic high Tg copolymers and terpolymers of the compositions of the present invention. The compositions of the present invention contain 40 to 95 wt%, preferably 50 to 90 wt%, and more preferably 50 to 80 wt%, and more preferably 55 to 70 wt% of the hydrophobic high Tg copolymer or terpolymer.

[0021] The hydrophobic high Tg copolymer or terpolymer contains 0.1 wt% to 20 wt%, preferably 0.3 wt% to 10 wt%, and more preferably 0.5 wt% to 5 wt% of the hydrophobic monomer.

[0022] tert-Butyl cyclohexyl methacrylate

[0023] The structural formula of tert-butyl cyclohexyl (meth)acrylate is as follows:

[0024]

[0025] tert-Butylcyclohexyl methacrylate tert-Butylcyclohexyl acrylate

[0026] The monomer is a mixture of cis-form and trans-form, with a trans / cis ratio between 30 / 70 and 97 / 3, preferably between 40 / 60 and 80 / 20, and more preferably between 50 / 50 and 75 / 25.

[0027] 3,3,5-Trimethylcyclohexyl (meth)acrylate

[0028] The structural formula of 3,3,5-trimethylcyclohexyl (meth)acrylate is as follows:

[0029] The monomer is a mixture of cis- and trans-forms.

[0030]

[0031] 3,3,5-Trimethylcyclohexyl methacrylate 3,3,5-Trimethylcyclohexyl acrylate

[0032] The content of tert-butyl cyclohexyl methacrylate or 3,3,5-trimethylcyclohexyl methacrylate in the final copolymer is generally in the range of 0.2-20 wt % based on the total monomer units in the copolymer, and more preferably 0.5 to 10 wt %. It has been found that as little as 1 wt %, and even 0.5 wt % of tert-butyl cyclohexyl methacrylate provides a copolymer with hydrophobic characteristics. In certain embodiments, the Tg of the copolymer is from 116° C. to 140° C.

[0033] Acrylic Monomer, MMA

[0034] One or more hydrophobic high Tg monomers are copolymerized with one or more other monomers. In a preferred embodiment of the present invention, the copolymer contains at least 50 wt% methyl methacrylate monomer units, preferably at least 70 wt% and more preferably at least 80 wt% methyl methacrylate monomer units constituting the copolymer.

[0035] In addition to the hydrophobic high Tg monomer and methyl methacrylate, the copolymer of the present invention may also contain 0 wt % to 49.5 wt % of other acrylate and methacrylate monomers or other ethylenically unsaturated monomers, including but not limited to styrene, alpha methyl styrene, acrylonitrile, and a low level of crosslinking agent may also be present in the monomer mixture. Suitable acrylate and methacrylate comonomers include but are not limited to methyl acrylate, ethyl acrylate and ethyl methacrylate, butyl acrylate and butyl methacrylate, isooctyl methacrylate and isooctyl acrylate, lauryl acrylate and lauryl methacrylate, octadecyl acrylate and octadecyl methacrylate, isobornyl acrylate and isobornyl methacrylate, methoxyethyl acrylate and methoxymethylacrylate, 2-ethoxyethyl acrylate and 2-ethoxyethyl methacrylate, and dimethylaminoethyl acrylate and dimethylaminoethyl methacrylate monomers. (Meth) acrylic acid, such as methacrylic acid and acrylic acid, can be used in the monomer mixture. In addition to carboxyl functional groups, other functional groups can also be added to the high molecular weight acrylic processing aid via functional comonomers, including epoxy (such as glycidyl methacrylate), hydroxyl and anhydride functional groups. Functional monomer units (monomer units with functional groups) can be present in up to 70 wt %, preferably up to 50 wt % of the acrylic polymer.

[0036] In a preferred embodiment, the acrylic copolymer has a high Tg of greater than 115°C, more preferably greater than 120°C, greater than 125°C, greater than 130°C, greater than 135°C, and even greater than 140°C. In addition to tert-butylcyclohexyl methacrylate and 3,3,5-trimethylcyclohexyl (meth)acrylate, other high Tg monomers may optionally be present in an amount of 0% to 25% by weight, and more preferably 0% to 10% by weight. The other high Tg monomers may be hydrophilic, hydrophobic, or neutral in character, and include, but are not limited to, methacrylic acid, acrylic acid, itaconic acid, alpha methylstyrene, maleic anhydride, maleimide, isobornyl methacrylate, norbornyl methacrylate, tert-butyl methacrylate, cyclohexyl methacrylate, acrylamide, and methacrylamide.

[0037] In one embodiment, a terpolymer of MMA / methacrylic acid and 3,3,5-trimethylcyclohexyl (meth)acrylate provides a useful terpolymer.

[0038] In one embodiment, the hydrophobic effect of tert-butylcyclohexyl methacrylate and / or 3,3,5-trimethylcyclohexyl (meth)acrylate was found to be strong enough to overcome the hydrophilic effect of the hydrophilic comonomer used at lower levels, resulting in an overall hydrophobic copolymer.

[0039] The weight average molecular weight of the hydrophobic high heat pMMA copolymer in the polymer blend is above 70,000 g / mol, preferably above 80,000 g / mol, more preferably above 90,000 g / mol. Increasing the molecular weight of the hydrophobic pMMA copolymer can increase chemical resistance.

[0040] The hydrophobic copolymer of the present invention can be obtained by melt polymerization (including but not limited to solution polymerization, emulsion polymerization and suspension polymerization).

[0041] The glass transition temperature (Tg) values ​​of pure pMMA copolymers are in the range of 114° C. to 140° C., preferably 115° C. to 135° C., more preferably 115° C. to 130° C., and most preferably 117° C. to 125° C. The weight average molecular weight of pure pMMA copolymers is in the range of 60,000 g / mol to 120,000 g / mol, preferably 65,000 g / mol to 110,000 g / mol.

[0042] Impact modifier

[0043] The impact modifier used in embodiments of the present invention may be a core-shell impact modifier. In a preferred embodiment, the core-shell impact modifier has an acrylic shell.

[0044] Preferred core-shell impact modifiers have a hard core. The volume average particle size of the core-shell impact modifier is 70nm to 350nm, preferably 100nm to 350nm, preferably 150nm to 300nm, more preferably 200nm to 250nm. In one embodiment, the shell contains some longer chain acrylic monomer units, making the shell slightly hydrophobic. The hydrophobic shell increases the compatibility of the core-shell impact modifier with the hydrophobic acrylic copolymer. Useful longer chain monomer units in the shell include butyl (meth) acrylate, C6 to C (meth) acrylic acid, and C6 to C7 esters. 16 Esters, and even low levels of tert-butylcyclohexyl(meth)acrylate and / or 3,3,5-trimethylcyclohexyl(meth)acrylate.

[0045] In a preferred embodiment, the core-shell impact modifier of the present invention consists of more than 45 wt%, preferably more than 50 wt%, of rubber having a Tg below 0°C, preferably below -10°C, more preferably below -20°C.

[0046] The compositions of the present invention contain 5 to 60 wt %, preferably 10 to 50 wt %, preferably 20 to 50 wt %, more preferably 25 to 50 wt %, and most preferably 30 to 45 wt % of one or more core-shell impact modifiers, and corresponding 40 to 95 wt %, 50 to 90 wt %, 50 to 80 wt %, 50 to 75 wt %, and 55 to 70 wt % of the hydrophobic acrylic copolymer, based on the total weight of the impact modifier and copolymer. Since the impact modifier of the present invention is more effective, lower loadings can be used.

[0047] The melt flow rate value of the hydrophobic impact pMMA copolymer is higher than 0.7 g / 10 min at 230°C / 3.8kg, preferably higher than 1.0 g / 10 min, more preferably higher than 1.2 g / 10 min, and more preferably higher than 1.5 g / 10 min. The Vicat softening temperature of the impact copolymer resin is detected at 10N to be at least 110°C, preferably higher than 112°C, and more preferably higher than 114°C. The water haze Δ value of the 3.2 mm molded plaque is controlled to be less than 14%, preferably less than 10%, and more preferably less than 8% after an exposure time of 168 hours in a 70°C water bath immersion test. The water haze gain value of the impact-modified hydrophobic acrylic copolymer is less than 8.0%, preferably less than 6.0%, more preferably less than 4.0%, and even less than 2.0%. The notched Izod impact strength is greater than 4 kJ / m 2 , preferably greater than 5kJ / m 2 , and more preferably greater than 6.4 kJ / m 2The impact-modified hydrophobic acrylic composition has a light transmittance retention of 86%, preferably higher than 90%, more preferably higher than 94%, and even higher than 96% after 168 hours in a 70° C. water bath immersion test.

[0048] additive

[0049] The compositions of the present invention can be blended with typical additives used in thermoplastics. These include, but are not limited to, fillers, surface modification additives, processing aids, fibers, lubricants, matting agents, heat stabilizers, flame retardants, synergists, matting agents, plasticizers, fillers, colorants, pigments, antioxidants, antistatic agents, surfactants, toners, refractive index matching additives, additives with specific light diffraction, light absorption or light reflection properties, or dispersing aids.

[0050] Examples of matting agents include, but are not limited to, cross-linked polymer particles of various geometric shapes. The amount of fillers and additives included in the polymer composition may vary from about 0.01% to about 70% of the combined weight of the polymer, additives, and fillers. Typically, amounts of about 5% to about 45%, about 10% to about 40% are included.

[0051] In one embodiment, selected antioxidants can be used to improve the thermal stability of the composition at high temperatures (e.g., 255-275° C.) and reduce yellowing at high temperatures. The loading of the antioxidant in the final composition is at a level of about 50ppm to 3500ppm, preferably about 100ppm to about 2500ppm based on the total weight of the composition. Non-limiting examples of useful antioxidants include sterically hindered phenols, organic phosphites, hindered amine light stabilizers (HALS), benzotriazoles, triazines, benzophenones, and cyanoacrylates. For example, the copolymer may include 100 to 2000ppm by weight or 2500ppm by weight of an antioxidant, which includes at least one of hydroxyphenylbenzotriazole, sterically hindered phenols, organic phosphites, hindered amines, and combinations thereof. These antioxidants are used to improve the thermal stability of the resin at high temperatures, such as 255° C. to 275° C., and reduce yellowing at high temperatures. The loading level of antioxidant in the final resin formulation ranges from 100 ppm to 2000 ppm by weight, or from 150 ppm to 1900 ppm, or from 200 ppm to 1800 ppm, or from 150 ppm to 1500 ppm, or from 100 ppm to 1000 ppm by weight.

[0052] Blends with other polymers

[0053] Other compatible polymers can be optionally blended with the copolymers of the present invention to form alloys. For example, other poly(meth)acrylate copolymers, such as poly(methyl(meth)acrylate) / ethyl(meth)acrylate) copolymers; poly(methyl methacrylate) / methyl acrylate copolymers, polyvinylidene fluoride, poly(styrene-acrylonitrile) (SAN), acrylonitrile-styrene-acrylate (ASA) copolymers, copolymers of ethylenediamine fluoride and hexafluoropropylene; polylactic acid; and combinations thereof can be blended with the polymer composition. The alloy blend can contain any level, such as 1-99%, of other compatible polymers, depending on the desired final properties.

[0054] In a preferred embodiment, the further poly(meth)acrylate is 0.5-20 wt%, preferably 5-15 wt% of a hydrophobic copolymer / terpolymer containing butyl methacrylate (BMA) / MMA having a weight average molecular weight in the range of 30,000-50,000 g / mol as measured in GPC.

[0055] In another preferred embodiment, the poly(meth)acrylate copolymer used in the alloy is a high molecular weight copolymer having a weight average molecular weight above 70,000 g / mol, preferably above 80,000 g / mol, more preferably above 90,000 g / mol, more preferably above 100,000 g / mol. Increasing the molecular weight leads to an increase in chemical resistance.

[0056] characteristic

[0057] The impact-modified hydrophobic acrylic compositions of the present invention provide many improvements over the prior art, as seen in the examples. These include one or more of the following improvements:

[0058] - Water spray resistance;

[0059] -Transmittance retention rate;

[0060] -YI displacement;

[0061] - surface hardness;

[0062] - Vicat heat resistance; and

[0063] -Melt fluidity.

[0064] application

[0065] The compositions of the present invention are thermoplastic and, in certain embodiments, can be readily formed into sheets, films, light pipes, and lenses.

[0066] The properties of the composition of the present invention provide a high performance impact modified polymer, making the polymer particularly suitable for automotive LED logo lighting tubes, automotive headlight covers, optical films, moisture barrier films, digital printing films and surface protection layers, such as, for example, decks / railings. The composition of the present invention can also be used in other applications requiring one or more of high light transmittance, low haze, high heat resistance, high impact resistance, high dimensional stability, high water spray resistance and sufficiently high melt flow.

[0067] Other uses of the impact-modified acrylic composition of the present invention include, but are not limited to, automotive, electronic equipment, medical, digital printing, laser cutting, building and construction, lighting tubes, thin-walled parts, optical lenses, extruded films, (co)extruded sheets / profiles, thermoformable sheets, cast sheets, composites, medical devices, etc. The high heat resistant acrylic film of the present invention is also used in LED / OLED displays.

[0068] In this specification, the embodiments have been described in a manner that enables a clear and concise description to be written, but it is intended and should be understood that the embodiments can be variously combined or separated without departing from the present invention. For example, it should be understood that all preferred features described herein are applicable to all aspects of the present invention described herein.

[0069] Non-limiting aspects of the invention are summarized below.

[0070] Example

[0071] Test Method :

[0072] Injection molding samples : In the following tests involving injection molded samples or plaques, the plaque sample dimensions were molded as 45 mm (width) x 67 mm (length) x 3.2 mm (thickness).

[0073] Melt Flow Rate (MFR) Measurement The melt flow rate of the polymer was measured using an Instron Ceast MF30 device. The mold temperature was controlled at 230°C and the load cell weight was 3.8 kg. The dried pellets were placed below T g Annealing is performed at a temperature of about 20°C for more than 8 hours.

[0074] Gel Permeation Chromatography (GPC): Polymer molecular weight measurements were performed using a Waters Alliance 2695 and a Waters DifferentialRefractometer 2410. The columns were based on two PL Gel mixed C columns and a guard column (7.8 mm ID x 30 cm, 5 μm). THF (HPLC grade) was chosen as the solvent. The temperature was controlled at 35°C. Ten poly(methyl methacrylate) standards were used in the calibration, with Mp (peak molecular weight) ranges from 550 g / mol to 1,677,000 g / mol.

[0075] NMR : Samples were prepared for use by dissolving approximately 200 mg of pellet in approximately 4 ml of CDCl3 in separate 10 mm NMR tubes. 13 C NMR. Before and after MAA derivatization, the spectrometers were operated at 25 °C on a Bruker AVIII HD 500 (11.07 T) spectrometer with a 5 mm 1 H / 19 F / 13 C TXO probe acquisition 1 H spectra. Acquired on a Bruker AV 400 (9.4T) using a 10 mm BBO probe at 50 °C 13 C spectrum.

[0076] Differential Scanning Calorimetry (DSC): The glass transition temperature of the acrylic polymer was measured during the second heating using a TA Instruments Q2000DSC in N2 at a heating rate of 10°C / min. The first heating was used to heat the sample to 170°C at a heating rate of 10°C / min, and then the sample was cooled to 0°C at a cooling rate of 10°C / min. The sample weight was controlled at 5-10 mg.

[0077] Thermogravimetric analysis (TGA): The thermal decomposition temperature of acrylic polymer was measured using TA Instruments Q5000 TGA in N2 at a heating rate of 10°C / min. The sample weight was controlled at 5-10 mg. The sample was pre-dried in a vacuum oven at 100°C overnight.

[0078] Total light transmittance : Total light transmittance was measured from film and / or plaque samples in transmission mode using a Perkin Elmer Lambda 950 with a 150 mm integrating sphere. The selected UV / Vis wavelength range was 200 nm to 800 nm in the UV / Vis region.

[0079] Haze : Optical haze of transparent film and / or plaque samples was measured using BYK HazeGard Plus according to ASTM method D1003.

[0080] Refractive Index : The refractive index of the polymer film was measured at three different wavelengths, 402 nm, 518 nm and 636.5 nm, using an optical prism coupler Metricon 2010 from Metricon Inc, while the refractive index was calculated at a selected wavelength of 589 nm.

[0081] Tensile strength and elongation : After 23°C / 48 hours preconditioning, tensile strength, modulus and elongation of tensile bars were evaluated using ASTM D638 method using Instron Model 4202 at a crosshead speed of 5 mm / min. The tensile length was 152.4 mm and the width was 12.7 mm. The sample thickness was 3.175 mm.

[0082] Notched Izod impact : Notched Izod impact strength or impact resistance is measured using ASTM D256 method using a 1.0 J impact hammer at 23°C / 50% relative humidity. Notched Izod bars were injection molded with dimensions of 10.2 mm (width) x 100 mm (length) x 3.2 mm (thickness).

[0083] Vicat softening temperature : Samples were tested in an Instron HV6M using ASTM method D1525 at 10 N and 50 N forces. Sample heating rate was controlled at a rate of 50 °C / hour. Injection molded samples were annealed at about 20 °C below Tg for 16 hours and stored in a drying oven before testing.

[0084] Water mist : The injection molded plaque samples were immersed in a DI water bath at a selected temperature (such as 70°C). The plaque sample size was molded to be 45mm (width) x 67mm (length) x 3.2mm (thickness). Water haze was measured using BYK HazeGard, while light transmittance was measured using Color-i after gently wiping off the water on the sample surface with a soft, dry paper towel. The sample needed to be completely cooled to ambient temperature at least 1.5 hours after being removed from the water bath.

[0085] Yellowness Index : Yellowness Index (YI) was measured using Color-i at 23°C / 50%RH according to ASTM E313 method from 3.2 mm injection molded plaques.

[0086] Surface hardness : Surface hardness is measured by Rockwell hardness on the M scale after annealing the plaque sample at a selected temperature (about 20°C below its glass transition temperature). 。

[0087] Average particle diameter: The core-shell impact modifier dispersed in a dilute solution (0.1-0.2 wt%) was spin coated onto a Si wafer substrate and dried at 70°C for 1 hour. A thin layer of iridium was coated on the modifier sample using an ion beam coater (model IBSe) from Southbay Technologies and the sample was imaged at various magnifications using a Hitachi SU8010 field emission SEM. Particle size analysis was performed using custom software. The average diameter of the impact modifier particles was determined based on more than 200 individual particles and the median diameter in the SEM images.

[0088] Example 1. Hydrophobic Acrylic Copolymer Synthesis Example

[0089] (pMMA copolymer MW2204 containing 1.0% t-butylcyclohexyl methacrylate, Tg = about 116°C). This example demonstrates the preparation of a high molecular weight copolymer of methyl methacrylate and t-butylcyclohexyl methacrylate (having a 72% trans / 28% cis isomer ratio). 9858.5 parts of methyl methacrylate and 100 parts of t-butylcyclohexyl methacrylate were charged to a reaction vessel at approximately 0°C under N2 with a mechanical stirring speed of 100 rpm. In addition, a 1% t-butylcyclohexyl methacrylate mixture was added to the reaction vessel. The mixture was stirred at 100 rpm for 2 h. 531 (from Arkema) was used as an initiator in an amount of 2.0 parts, while 38.5 parts of n-dodecyl mercaptan (n-DDM from Aldrich) was used as a chain transfer agent, and 1.0 parts of di-tert-dodecyl disulfide (DtDDS from Arkoma) was used. The polymerization reaction took place at 160°C for 7 hours. When the conversion rate reached more than 50%, the residual monomers were removed by the exhaust system. The resulting polymer was passed through a single screw extruder at a die temperature of 240°C and a barrel temperature of 225-245°C. The melt stream passed through a water bath before pelletization. The copolymer was then pelletized into 3-4 mm long resin pellets and dried in a drying oven at 100°C for 8 hours. The melt flow rate of this polymer was measured at 230°C under 3.8 kg and was 5.41 g / 10 minutes. The refractive index of the resulting polymer was measured at 589 nm and was 1.491.

[0090] use 1 H NMR confirmed that the resulting polymer had a composition of pMMA / tert-butylcyclohexyl methacrylate (99.06 / 0.94 w / w). 13The syndiotacticity of the copolymer was measured by NMR from a chemical shift of 44.5ppm as 52%, while the isotacticity and atacticity were measured from 45.5ppm and 45.0ppm as 7% and 41%. The glass transition temperature of the resin was measured to be 116°C in N2 at a heating rate of 10°C / min using DSC. After the sample was annealed at 95°C for 16 hours, the Vicat softening temperatures were detected to be 116°C and 112°C at 10N and 50N. The weight average molecular weight Mw of the resin was measured using GPC to be 78,500g / mol, and the Mw / Mn (polydispersity) value was 1.9. The transmittance of a 3.2mm plate was measured at 560nm using a Lambda 950 with a 150mm integrating sphere to be 92.3%, and the haze was measured to be 0.4% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the tested sample was 3.2 GPa, while the tensile strength was 75 MPa and the tensile elongation was 10%.

[0091] Example 2. Hydrophobic Acrylic Copolymer Synthesis Example (pMMA Copolymer MW2208 with 1.0% t-butylcyclohexyl methacrylate, Tg = ~116°C). This example demonstrates the preparation of a high molecular weight copolymer of methyl methacrylate and t-butylcyclohexyl methacrylate (having a 67% trans / 33% cis isomer ratio). 9857.4 parts of methyl methacrylate and 100 parts of t-butylcyclohexyl methacrylate were charged to a reaction vessel at approximately 0°C under N2 with a mechanical stirring speed of 100 rpm. In addition, a 1% t-butylcyclohexyl methacrylate was added to the reaction vessel. 531 (from Arkema) was used as an initiator in an amount of 2.1 parts, while 39.5 parts of n-dodecyl mercaptan (n-DDM from Aldrich) was used as a chain transfer agent, and 1.0 parts of di-tert-dodecyl disulfide (DtDDS from Arkoma) was used. The polymerization reaction took place at 160°C for 7 hours. When the conversion rate reached more than 50%, the residual monomers were removed by the exhaust system. The resulting polymer was passed through a single screw extruder at a die temperature of 240°C and a barrel temperature of 230-245°C. The melt stream passed through a water bath before pelletization. The copolymer was then pelletized into 3-4 mm long resin pellets and dried in a drying oven at 100°C for 8 hours. The melt flow rate of this polymer was measured at 230°C under 3.8 kg and was 6.23 g / 10 minutes. The refractive index of the resulting polymer was measured at 589 nm and was 1.491.

[0092] use 1 H NMR confirmed that the resulting polymer had a composition of pMMA / tert-butylcyclohexyl methacrylate (99.0 / 1.0 w / w). 13The syndiotacticity of the copolymer was measured by NMR from a chemical shift of 44.5ppm as 51%, while the isotacticity and atacticity were measured from 45.5ppm and 45.0ppm as 7% and 42%. The glass transition temperature of the resin was measured to be 116°C in N2 at a heating rate of 10°C / min using DSC. After the sample was annealed at 100°C for 16 hours, the Vicat softening temperatures were detected to be 117°C and 113°C at 10N and 50N. The weight average molecular weight Mw of the resin was measured using GPC to be 75,500g / mol, and the Mw / Mn (polydispersity) value was 2.1. The transmittance of a 3.2mm plate was measured at 560nm using a Lambda 950 with a 150mm integrating sphere to be 92.2%, and the haze was measured to be 0.4% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the tested sample was 3.2 GPa, while the tensile strength was 70 MPa and the tensile elongation was 7%.

[0093] Example 3.

[0094] This example demonstrates the preparation of a copolymer of methyl methacrylate and tert-butyl cyclohexyl methacrylate (SR218A from Sartomer, containing 72% trans / 28% cis isomers) MW2204 at 99.06 / 0.94 with a commercial core-shell acrylic impact modifier (M212 from Kaneka at 48%). A high Tg hydrophobic acrylic resin (MW2204, Tg=116°C) prepared by Trinseo was compounded with a core-shell impact modifier (M212 from Kaneka) having a particle size of 215 nm using a 27 mm intermeshing co-rotating twin screw extruder (from Leistritz) at a compounding rate of 25 lbs / hr at a die temperature of 210°C and a barrel temperature of 210-230°C to form an impact acrylic resin. UV stabilizers were also added to the formulation by pre-blending during compounding. The compounded acrylic pellets were cut through a water bath at ambient temperature and dried at 100°C.

[0095] The melt flow rate of the resulting polymer was measured at 230°C under 3.8kg to be 1.06 g / 10 min. The glass transition temperature of the resin was measured to be 113°C in N2 using DSC at a heating rate of 10°C / min. After the sample was annealed at 95°C for 16 hours, the Vicat softening temperatures were detected to be 110°C and 95°C at 10N and 50N. The transmittance of a 3.2 mm molded plaque was measured at 560nm using a Lambda 950 to be 90.0%, while the haze was measured to be 1.8% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the test sample was 1.61 GPa, while the tensile strength was 38 MPa, and the elongation was 72%. The notched Izod impact strength was measured to be 6.6 kJ / m at 23°C. 2 The Rockwell superficial hardness (M) was measured at 21 after the sample was annealed. The water haze gain value was measured to be 7.0% after 168 hours in a 70°C water bath immersion test, while the light transmittance was measured to be 86.5% (and the light transmittance retention was 96.1%) and the YI was 6.6 (compared to the initial YI of 2.0).

[0096] Table 1

[0097]

[0098] Example 4 .

[0099] This example demonstrates the preparation of a 99.0 / 1.0 copolymer of methyl methacrylate and tert-butyl cyclohexyl methacrylate (SR218A from Sartomer, containing 67% trans / 33% cis isomers) MW2208 with a commercial core-shell acrylic impact modifier (48% M210 from Kaneka). A high Tg hydrophobic acrylic resin (MW2208, Tg=116°C) prepared by Trinseo was compounded with a core-shell impact modifier (M210 from Kaneka) having a particle size of 250 nm using a 27 mm co-rotating twin screw extruder (from Leistritz) at a die temperature of 210°C and a barrel temperature of 220-240°C at a compounding rate of 25 lbs / hr to form an impact acrylic resin. UV stabilizers were also added to the formulation by pre-blending during compounding. The compounded acrylic pellets were cut through a water bath at ambient temperature and dried at 100°C.

[0100] The melt flow rate of the resulting polymer was measured at 230°C under 3.8kg to be 0.89 g / 10 min. The glass transition temperature of the resin was measured to be 115°C in N2 at a heating rate of 10°C / min using DSC. After the sample was annealed at 95°C for 16 hours, the Vicat softening temperatures were detected to be 114°C and 97°C at 10N and 50N. The transmittance of a 3.2 mm molded plaque was measured at 560nm using a Lambda 950 to be 90.5%, while the haze was measured to be 1.2% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the test sample was 1.39 GPa, while the tensile strength was 36 MPa, and the elongation was 92%. The notched Izod impact strength was measured to be 7.3 kJ / m at 23°C. 2 The Rockwell Surface Hardness (M) was measured at 21 after the sample was annealed. The water haze gain value was measured to be 4.8% after 168 hours in a 70°C water bath immersion test, while the light transmittance was measured to be 85.1% (and the light transmittance retention was 94.0%) and the YI was 9.1 (compared to the initial YI of 2.5).

[0101] Table 2

[0102] Example 4 supplier Quantity (portions) Acrylic MW2208 Trinseo 5160 Core-shell impact modifier (M210) Kaneka 4800 UV Blend 10 (Contains Tinuvin 234) Trinseo 40

[0103] Example 5 .

[0104] This example demonstrates the preparation of a 99.0 / 1.0 copolymer of methyl methacrylate and tert-butyl cyclohexyl methacrylate (SR218A from Sartomer, containing 67% trans / 33% cis isomers) MW2208 with a commercial core-shell acrylic impact modifier (40% M210 from Kaneka). The extruder was extruded using a 27 mm co-rotating twin screw extruder (from Sartomer) at a die temperature of 210°C and a barrel temperature of 220-240°C. Leistritz ) A high Tg hydrophobic acrylic resin (MW2208, Tg=116°C) prepared by Trinseo was compounded with a core-shell impact modifier (M210 from Kaneka) with a particle size of 250 nm at a compounding speed of 25 lbs / hr to form an impact acrylic resin. A UV stabilizer was also added to the formulation by pre-blending during compounding. The compounded acrylic pellets were cut through a water bath at ambient temperature and dried at 100°C.

[0105] The melt flow rate of the obtained polymer measured at 230°C under 3.8 kg is 1.4Grams / 10 minutes. The glass transition temperature of the resin was measured to be 115°C in N2 using DSC at a heating rate of 10°C / min. After the sample was annealed at 95°C for 16 hours, the Vicat softening temperatures of 115°C and 103°C were detected at 10N and 50N. The transmittance of a 3.2 mm molded plaque was measured to be 90.3% at 560nm using a Lambda 950, while the haze was measured to be 2.1% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the test sample was 1.55 GPa, while the tensile strength was 38 MPa, and the elongation was 85%. The notched cantilever impact resistance / impact strength was measured to be 6.7 kJ / m at 23°C. 2 The Rockwell Surface Hardness (M) was measured at 37 after annealing. The water haze gain value was measured after 168 hours in a 70°C water bath immersion test to be 4.9%, while the light transmittance was 86.3% (and the light transmittance retention was 95.6%) and the YI was 5.9 (compared to the initial YI of 2.3) 。

[0106] Table 3

[0107]

[0108] Example 6 .

[0109] This example demonstrates the preparation of a copolymer of methyl methacrylate and tert-butyl cyclohexyl methacrylate (SR218A from Sartomer, containing 72% trans / 28% cis isomers) MW2204 at 99.06 / 0.94 with a commercial core-shell acrylic impact modifier (M212 from Kaneka at 40%). A high Tg hydrophobic acrylic resin (MW2204, Tg = 116°C) prepared by Trinseo was compounded with a core-shell impact modifier (M212 from Kaneka) having a particle size of 215 nm using a 27 mm co-rotating twin screw extruder (from Leistritz) at a compounding rate of 25 lbs / hr at a die temperature of 210°C and a barrel temperature of 220-240°C to form an impact acrylic resin. UV stabilizers were also added to the formulation by pre-blending during compounding. The compounded acrylic pellets were cut through a water bath at ambient temperature and dried at 100°C.

[0110] The melt flow rate of the resulting polymer was measured at 230°C under 3.8kg to be 1.77 g / 10 min. The glass transition temperature of the resin was measured to be 114°C in N2 at a heating rate of 10°C / min using DSC. After the sample was annealed at 95°C for 16 hours, the Vicat softening temperatures were detected to be 114°C and 102°C at 10N and 50N. The transmittance of a 3.2 mm molded plaque was measured at 560nm using a Lambda 950 to be 90.0%, while the haze was measured to be 1.8% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the test sample was 1.6 GPa, while the tensile strength was 38 MPa, and the elongation was 85%. The notched cantilever impact resistance / impact strength was measured to be 6.6 kJ / m at ambient temperature. 2 The Rockwell superficial hardness (M) was measured at 42 after the sample was annealed. The water haze gain value was measured to be 7.0% after 168 hours in a 70°C water bath immersion test, while the light transmittance was measured to be 85.6% (and the light transmittance retention was 95.1%) and the YI was 3.8 (compared to the initial YI of 1.1).

[0111] Table 4

[0112]

[0113] Example 7 .

[0114] This example demonstrates the preparation of a copolymer of methyl methacrylate and tert-butyl cyclohexyl methacrylate (SR218A from Sartomer, containing 72% trans / 28% cis isomers) MW2204, 99.06 / 0.94, with a commercial core-shell acrylic impact modifier (M210 from Kaneka at 35%). A high Tg hydrophobic acrylic resin (MW2204, Tg=116°C) prepared by Trinseo was compounded with a core-shell impact modifier (M210 from Kaneka) having a particle size of 250 nm using a 27 mm co-rotating twin screw extruder (from Leistritz) at a die temperature of 210°C and a barrel temperature of 220-240°C at a compounding rate of 25 lbs / hr to form an impact acrylic resin. A UV stabilizer was also added to the formulation by pre-blending during compounding. The compounded acrylic pellets were cut through a water bath at ambient temperature and dried at 100°C.

[0115] The melt flow rate of the resulting polymer was measured at 230°C under 3.8kg to be 1.51 g / 10 min. The glass transition temperature of the resin was measured to be 115°C in N2 at a heating rate of 10°C / min using DSC. After the sample was annealed at 95°C for 16 hours, the Vicat softening temperatures were detected to be 115°C and 104°C at 10N and 50N. The transmittance of a 3.2 mm molded plaque was measured at 560nm using a Lambda 950 to be 90.3%, while the haze was measured to be 1.9% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the test sample was 1.72 GPa, while the tensile strength was 42 MPa, and the elongation was 82%. The notched cantilever impact resistance / impact strength was measured to be 6.9 kJ / m at 23°C. 2 The Rockwell surface hardness (M) was measured at 45 after annealing. The water haze gain value was 6.3% after 168 hours of immersion test in a 70°C water bath. , The light transmittance was also measured to be 87.5% (and the light transmittance retention was 96.9%) and the YI was 4.1 (compared to an initial YI of 1.7).

[0116] Table 5

[0117]

[0118] Example 8 .

[0119] This example demonstrates the preparation of a copolymer of methyl methacrylate and tert-butyl cyclohexyl methacrylate (SR218A from Sartomer, containing 72% trans / 28% cis isomers) MW2204, 99.06 / 0.94, with a commercial core-shell acrylic impact modifier (M212 from Kaneka at 35%). A high Tg hydrophobic acrylic resin (MW2204, Tg = 116°C) prepared by Trinseo was compounded with a core-shell impact modifier (M212 from Kaneka) having a particle size of 215 nm using a 27 mm co-rotating twin screw extruder (from Leistritz) at a compounding rate of 25 lbs / hr at a die temperature of 210°C and a barrel temperature of 220-240°C to form an impact acrylic resin. UV stabilizers were also added to the formulation by pre-blending during compounding. The compounded acrylic pellets were cut through a water bath at ambient temperature and dried at 100°C.

[0120] The melt flow rate of the resulting polymer was measured at 230°C under 3.8kg to be 1.91 g / 10 min. The glass transition temperature of the resin was measured to be 116°C in N2 using DSC at a heating rate of 10°C / min. After the sample was annealed at 95°C for 16 hours, the Vicat softening temperatures were detected to be 116°C and 106°C at 10N and 50N. The transmittance of a 3.2 mm molded plaque was measured at 560nm using a Lambda 950 to be 90.6%, while the haze was measured using a haze meter (Haze Gard Plus from BYK) to be 2.1%. The tensile modulus of the test sample was 2.03 GPa, while the tensile strength was 50 MPa, and the elongation was 51%. The notched cantilever impact resistance / impact strength was measured to be 6.0 kJ / m at 23°C. 2 The Rockwell surface hardness (M) was measured at 55 after annealing. The water haze gain value was 4.2% after 168 hours of immersion test in a 70°C water bath. , The light transmittance was also measured to be 88.1% (and the light transmittance retention was 97.2%) and the YI was 2.3 (compared to an initial YI of 1.3).

[0121] Table 6

[0122]

[0123] Example 9 .

[0124] This example demonstrates the preparation of a copolymer of 99.06 / 0.94 methyl methacrylate and tert-butyl cyclohexyl methacrylate (SR218A from Sartomer, containing 72% trans / 28% cis isomers) MW2204 with a commercial core-shell acrylic impact modifier (30% M210 from Kaneka). A high Tg hydrophobic acrylic resin (MW2204, Tg = 116°C) prepared by Trinseo was mixed with B60 (from Dow Chemical) and a core-shell impact modifier (M210 from Kaneka) with a particle size of 250 nm were compounded to form an impact resistant acrylic resin. A 27 mm co-rotating twin screw extruder (from Leistritz) was used at a die temperature of 210° C. and a barrel temperature of 210-230° C. at a speed of 25 lbs / hour during compounding. UV stabilizers were also added to the formulation by pre-blending during compounding. The compounded acrylic pellets were cut through a water bath at ambient temperature and dried at 100° C.

[0125] The melt flow rate of the resulting polymer was measured at 230°C under 3.8kg to be 3.09 g / 10 min. The glass transition temperature of the resin was measured to be 114°C in N2 at a heating rate of 10°C / min using DSC. After the sample was annealed at 95°C for 16 hours, the Vicat softening temperatures were detected to be 113°C and 103°C at 10N and 50N. The transmittance of a 3.2 mm molded plaque was measured at 560nm using a Lambda 950 to be 91.3%, while the haze was measured to be 1.4% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the test sample was 1.86 GPa, while the tensile strength was 44 MPa, and the elongation was 49%. The notched cantilever impact resistance / impact strength was measured to be 4.9 kJ / m at 23°C. 2 The Rockwell superficial hardness (M) was measured at 50 after the sample was annealed. The water haze gain value was measured to be 3.7% after 168 hours in a 70°C water bath immersion test, while the light transmittance was measured to be 88.2% (and the light transmittance retention was 96.6%) and the YI was 3.7 (compared to the initial YI of 1.6).

[0126] Table 7

[0127]

[0128] Example 10 .

[0129] This example demonstrates the preparation of a copolymer of methyl methacrylate and tert-butyl cyclohexyl methacrylate (SR218A from Sartomer, containing 72% trans / 28% cis isomers) MW2204 at 99.06 / 0.94 with a commercial core-shell acrylic impact modifier (30% M212 from Kaneka). A high Tg hydrophobic acrylic resin (MW2204, Tg = 116°C) prepared by Trinseo was compounded with a core-shell impact modifier (M210 from Kaneka) having a particle size of 215 nm using a 27 mm co-rotating twin screw extruder (from Leistritz) at a compounding rate of 25 lbs / hr at a die temperature of 210°C and a barrel temperature of 210-230°C to form an impact acrylic resin. UV stabilizers were also added to the formulation by pre-blending during compounding. The compounded acrylic pellets were cut through a water bath at ambient temperature and dried at 100°C.

[0130] The melt flow rate of the resulting polymer was measured at 230°C under 3.8kg to be 2.37 g / 10 min. The glass transition temperature of the resin was measured to be 116°C in N2 using DSC at a heating rate of 10°C / min. After the sample was annealed at 95°C for 16 hours, the Vicat softening temperatures were detected to be 116°C and 107°C at 10N and 50N. The transmittance of a 3.2 mm molded plaque was measured at 560nm using a Lambda 950 to be 90.4%, while the haze was measured to be 2.3% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the test sample was 2.12 GPa, while the tensile strength was 50 MPa, and the elongation was 46%. The notched cantilever impact resistance / impact strength was measured to be 4.7 kJ / m at 23°C. 2 The Rockwell surface hardness (M) was measured at 62 after the sample was annealed. The water haze gain value was 2.3% after 168 hours of immersion test in a 70°C water bath. , The light transmittance was also measured to be 88.0% (and the light transmittance retention was 97.3%) and the YI was 1.9 (compared to an initial YI of 1.2).

[0131] Table 8

[0132]

[0133] Embodiment 11 .

[0134] This example demonstrates the preparation of a copolymer of methyl methacrylate and tert-butyl cyclohexyl methacrylate (SR218A from Sartomer, containing 72% trans / 28% cis isomers) MW2204, 99.06 / 0.94, with a commercial core-shell acrylic impact modifier (25% M210 from Kaneka). A high Tg hydrophobic acrylic resin (MW2204, Tg=116°C) prepared by Trinseo was compounded with a core-shell impact modifier (M210 from Kaneka) having a particle size of 250 nm using a 27 mm co-rotating twin screw extruder (from Leistritz) at a die temperature of 210°C and a barrel temperature of 220-240°C at a compounding rate of 25 lbs / hr to form an impact acrylic resin. UV stabilizers were also added to the formulation by pre-blending during compounding. The compounded acrylic pellets were cut through a water bath at ambient temperature and dried at 100°C.

[0135] The melt flow rate of the resulting polymer was measured at 230°C under 3.8kg to be 2.08 g / 10 min. The glass transition temperature of the resin was measured to be 117°C in N2 using DSC at a heating rate of 10°C / min. After the sample was annealed at 95°C for 16 hours, the Vicat softening temperatures were detected to be 117°C and 109°C at 10N and 50N. The transmittance of a 3.2 mm molded plaque was measured at 560nm using a Lambda 950 to be 90.7%, while the haze was measured using a haze meter (Haze Gard Plus from BYK) to be 1.8%. The tensile modulus of the test sample was 1.93 GPa, while the tensile strength was 48 MPa, and the elongation was 79%. The notched cantilever impact resistance / impact strength was measured to be 5.8 kJ / m at 23°C. 2 The Rockwell surface hardness (M) was measured at 68 after the sample was annealed. The water haze gain value was 3.4% after 168 hours of immersion test in a 70°C water bath. , The light transmittance was also measured to be 88.5% (and the light transmittance retention was 97.6%) and the YI was 2.4 (compared to an initial YI of 1.2).

[0136] Table 9

[0137]

[0138] Example 12 .

[0139] This example demonstrates the preparation of a copolymer of 99.06 / 0.94 methyl methacrylate and tert-butyl cyclohexyl methacrylate (SR218A from Sartomer, containing 72% trans / 28% cis isomers) MW2204 with a commercial core-shell acrylic impact modifier (35% M210 from Kaneka). A high Tg hydrophobic acrylic resin (MW2204, Tg = 116°C) prepared by Trinseo was mixed with B60 (from Dow Chemical) and a core-shell impact modifier (M210 from Kaneka) with a particle size of 250 nm were compounded to form an impact resistant acrylic resin. A 27 mm co-rotating twin screw extruder (from Leistritz) was used at a die temperature of 210° C. and a barrel temperature of 210-230° C. at a speed of 25 lbs / hour during compounding. UV stabilizers were also added to the formulation by pre-blending during compounding. The compounded acrylic pellets were cut through a water bath at ambient temperature and dried at 100° C.

[0140] The melt flow rate of the resulting polymer was measured at 230°C under 3.8kg to be 2.57 g / 10 min. The glass transition temperature of the resin was measured to be 111°C in N2 at a heating rate of 10°C / min using DSC. After the sample was annealed at 95°C for 16 hours, the Vicat softening temperatures were detected to be 111°C and 98°C at 10N and 50N. The transmittance of a 3.2 mm molded plaque was measured at 560nm using a Lambda 950 to be 90.1%, while the haze was measured to be 1.8% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the test sample was 1.70 GPa, while the tensile strength was 42 MPa, and the elongation was 80%. The notched cantilever impact resistance / impact strength was measured to be 5.4 kJ / m at 23°C. 2 The Rockwell surface hardness (M) was measured at 39 after the sample was annealed. The water haze gain value was 5.2% after 168 hours of immersion test in a 70°C water bath. , The light transmittance was also measured to be 85.2% (and the light transmittance retention was 94.6%) and the YI was 7.0 (compared to an initial YI of 1.9).

[0141] Table 10

[0142]

[0143] Comparative Example 1 .

[0144] A 27 mm co-rotating twin-screw extruder (from Leistritz ) at a line speed of 25 lbs / hr V920 acrylic copolymer resin (from Trinseo) was compounded with a core-shell impact modifier (48 wt.% MPD91 from Trinseo) with a particle size of 300 nm to form an impact acrylic resin. UV stabilizer ( 234) was added to the formulation. The compounded acrylic pellets were cut through a water bath at ambient temperature and dried at 85°C.

[0145] The melt flow rate of the resulting polymer was measured at 230°C under 3.8kg to be 1.14 g / 10 min. The glass transition temperature of the resin was measured to be 106°C in N2 using DSC at a heating rate of 10°C / min. After the sample was annealed at 85°C for 16 hours, the Vicat softening temperatures were detected to be 105°C and 98°C at 10N and 50N. The transmittance of a 3.2 mm molded plaque was measured at 560nm using a Lambda 950 to be 90.5%, while the haze was measured to be 1.5% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the test sample was 1.83 GPa, while the tensile strength was 42 MPa, and the elongation was 70%. The notched Izod impact strength was measured to be 5.7 kJ / m at 23°C / 50% RH. 2 The Rockwell surface hardness (M) was measured to be 46 after the sample was annealed. The water haze gain value was measured to be 60% after 168 hours in a 70°C water bath immersion test, while the light transmittance was measured to be 57.5% (and the light transmittance retention was 63.5%) and the YI was 15.5.4 (compared to the initial YI of 0.2).

[0146] Comparison Table 1

[0147]

[0148] Comparative Example 2 .

[0149] This example demonstrates the preparation of a 99.0 / 1.0 copolymer of methyl methacrylate and tert-butyl cyclohexyl methacrylate (SR218A from Sartomer, containing 62% trans / 38% cis isomers) MW2009 with a core-shell acrylic impact modifier (45% MPD85T from Kaneka). The glass transition temperature of the resin was 117°C using DSC at a heating rate of 10°C / min in N2. The weight average molecular weight Mw of the resin was 81,500 g / mol using GPC, and the Mw / Mn (polydispersity) value was 1.9. A high Tg hydrophobic acrylic resin (MW2009, Tg=117°C) prepared by Trinseo was compounded with a core-shell impact modifier (MPD85T) having a particle size of 300 nm using a 27 mm co-rotating twin screw extruder (from Leistritz) at a compounding speed of 25 lbs / hour at a die temperature of 210°C and a barrel temperature of 210-230°C to form an impact acrylic resin. A UV stabilizer was also added to the formulation by pre-blending during compounding. The compounded acrylic pellets were cut through a water bath at ambient temperature and dried at 100°C.

[0150] The melt flow rate of the polymer was measured at 230°C under 3.8 kg and was 0.85 g / 10 min. The DSC was heated at a rate of 10°C / min under N 2 The glass transition temperature of the resin was measured as 117℃ . After the sample was annealed at 95°C for 16 hours, the Vicat softening temperatures of 115°C and 105°C were detected at 10N and 50N. The transmittance of the 3.2 mm molded plaque was measured at 560nm using a Lambda 950 and the haze was measured to be 1.3% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the test sample was 1.82 GPa, while the tensile strength was 42 MPa and the elongation was 54%. The notched cantilever impact resistance / impact strength was measured at 23°C and was 5.5 kJ / m 2 The Rockwell Surface Hardness (M) was measured at 50 after the sample was annealed. The water haze gain value was measured to be 15.9% after 168 hours in a 70°C water bath immersion test, while the light transmittance was measured to be 77.0% (and the light transmittance retention was 84.4%) and the YI was 13.9 (compared to the initial YI of 3.2).

[0151] Comparison Table 2

[0152]

[0153] Comparative Example 3.

[0154] Measured at 230°C under 3.8 kg from Rohm The melt flow rate of Resist AG-100 polymer is 1.45 g / 10 min. The glass transition temperature of the resin was measured to be 111°C in N2 using DSC at a heating rate of 10°C / min. AG-100 consists of 32 wt% of an acrylic core-shell impact modifier with a particle size of 290-300 nm in a pMMA / MA (98.5 / 1.5) copolymer. After the sample was annealed at 90°C for 16 hours, Vicat softening temperatures of 111°C and 101°C were detected at 10N and 50N. The transmittance of a 3.2 mm molded plaque was measured at 560nm using a Lambda 950 to be 90.5%, while the haze was measured to be 1.5% using a haze meter (Haze Gard Plus from BYK). The tensile modulus of the test sample was 1.99 GPa, while the tensile strength was 46 MPa, and the elongation was 81%. The notched cantilever beam impact resistance / impact strength measured at 23°C is 6.0 kJ / m 2The Rockwell superficial hardness (M) was measured at 56 after the sample was annealed. The water haze gain value was measured to be 34.3% after 168 hours in a 70°C water bath immersion test, while the light transmittance was measured to be 72.6% (and the light transmittance retention was 80.2%) and the YI was 9.4 (compared to the initial YI of -0.1).

[0155] Embodiment overview: As can be seen from the examples, the impact-modified acrylic composition of the present invention provides much higher water spray resistance, higher heat resistance, higher impact resistance and / or higher surface hardness than commercially available impact-modified commercial products.

Claims

1. An impact-modified hydrophobic acrylic composition comprising: a) 40 to 95 wt%, preferably 50 to 90 wt%, more preferably 50 to 80 wt%, and most preferably 55 to 70 wt% of a hydrophobic acrylic copolymer based on the weight of the hydrophobic polymer plus the impact modifier, wherein the hydrophobic acrylic copolymer comprises: 1) 0.1 to 20% by weight, preferably 0.3 to 10% by weight, more preferably 0.5 to 5% by weight of monomer units selected from tert-butylcyclohexyl methacrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate and mixtures thereof; 2) 50 to 80 wt% of methyl methacrylate monomer units; 3) optionally 0% to 49.9% by weight of other monomer units copolymerizable with methyl methacrylate; The percentages are based on the total monomer units in the hydrophobic acrylic copolymer, wherein the copolymer has a Tg of 111°C to 140°C, preferably 113°C to 135°C, preferably 115°C to 130°C, and more preferably 116°C to 125°C; b) optionally other (meth)acrylic copolymers; c) 5 to 60 wt %, preferably 10 to 50 wt %, more preferably 20 to 50 wt %, and most preferably Preferably 30 wt% to 45 wt% of one or more core-shell impact modifiers, wherein the core-shell impact modifier has a volume average particle size of 70 nm to 350 nm, preferably 100 nm to 350 nm, preferably 150-300 nm, more preferably 200-250 nm; in, The Tg of the shell layer is greater than 105°C, preferably greater than 107°C; wherein said percentages of said polymers a), b) and c) in said impact-modified hydrophobic acrylic composition total 100%; wherein the melt flow rate of the impact-modified hydrophobic acrylic composition is greater than 0.7 g / 10 min at 230° C. under 3.8 kg, preferably greater than 1.0 g / 10 min, more preferably greater than 1.2 g / 10 min, and more preferably greater than 1.5 g / 10 min; and wherein the notched Izod impact strength of the impact-modified hydrophobic acrylic composition is greater than 4.5 kJ / m 2 , preferably greater than 5.4 kJ / m 2 , and more preferably greater than 6.4 kJ / m 2 .

2. The impact-modified hydrophobic acrylic composition of claim 1, wherein the impact-modified hydrophobic acrylic composition has a water haze gain value of less than 8.0%, preferably less than 6.0%, more preferably less than 4.0%, and even less than 2.0% after 168 hours in a 70°C water bath immersion test.

3. The impact-modified hydrophobic acrylic composition according to claim 1 or 2, wherein the impact-modified hydrophobic acrylic composition has a light transmittance retention of 86%, preferably higher than 90%, more preferably higher than 94%, and even higher than 96% after 168 hours under a 70°C water bath immersion test.

4. The impact modified hydrophobic acrylic composition of any one of claims 1 to 3, wherein the other acrylic composition further comprises 5-20% of a hydrophobic copolymer / terpolymer containing butyl methacrylate (BMA) / MMA having a weight average molecular weight in the range of 30,000-50,000 g / mol as measured in GPC.

5. The impact-modified hydrophobic acrylic composition of any one of claims 1 to 4, wherein the core-shell impact modifier consists of more than 45 wt%, preferably more than 50 wt%, of rubber having a Tg below 0°C, preferably below -10°C, more preferably below -20°C.

6. The impact modified hydrophobic acrylic composition of any one of claims 1 to 5, wherein the tert-butylcyclohexyl(meth)acrylate and / or 3,3,5-trimethylcyclohexyl(meth)acrylate monomer units have a trans / cis ratio of 30 / 70 to 97 / 3, more preferably 40 / 60 to 80 / 20, and most preferably 50 / 50 to 75 / 25.

7. The impact modified hydrophobic acrylic composition of any one of claims 1 to 6, wherein the optional other monomer units copolymerizable with methyl methacrylate are selected from the group consisting of styrene, alpha methyl styrene, acrylonitrile, methyl acrylate, ethyl acrylate and ethyl methacrylate, butyl acrylate and butyl methacrylate, isooctyl methacrylate and isooctyl acrylate, lauryl acrylate and lauryl methacrylate, octadecyl acrylate and octadecyl methacrylate, isobornyl acrylate and isobornyl methacrylate, methoxyethyl acrylate and methoxymethylacrylate, 2-ethoxyethyl acrylate and 2-ethoxyethyl methacrylate and dimethylaminoethyl acrylate and methacrylate monomers, (meth)acrylic acid, methacrylic acid, acrylic acid and mixtures thereof.

8. The impact modified hydrophobic acrylic composition of any one of claims 1 to 7, wherein the optional other monomer units copolymerizable with methyl methacrylate comprise 0.01 wt% to 25 wt% of a high Tg comonomer selected from the group consisting of methacrylic acid, acrylic acid, itaconic acid, alpha methylstyrene, maleic anhydride, maleimide, isobornyl methacrylate, norbornyl methacrylate, t-butyl methacrylate, cyclohexyl methacrylate, acrylamide and methacrylamide, and mixtures thereof.

9. The impact modified hydrophobic acrylic composition of any one of claims 1 to 8, wherein the hydrophobic acrylic copolymer has a weight average molecular weight of 55,000 to 250,000 g / mol, preferably 70,000 to 200,000 g / mol, more preferably greater than 80,000 to 160,000 g / mol.

10. The impact modified hydrophobic acrylic composition of any one of claims 1 to 9, wherein the composition is optically clear, having a TWLT of at least 89%, preferably at least 90%, and more preferably at least 91%; and an optical haze of less than 4%, preferably less than 3%, and most preferably less than 2% as measured on a 3.2 mm thick plaque using ASTM method D1003.

11. The impact-modified hydrophobic acrylic composition according to any one of claims 1 to 10, wherein the acrylic composition has a refractive index of 1.47 to 1.50 at a wavelength of 589 nm.

12. The impact modified hydrophobic acrylic composition of any one of claims 1 to 11, wherein the acrylic composition further comprises effective amounts of fillers, surface modification additives, processing aids, fibers, lubricants, matting agents, heat stabilizers, flame retardants, synergists, matting agents, plasticizers, fillers, colorants, pigments, antioxidants, antistatic agents, surfactants, toners, refractive index matching additives; additives having specific light diffraction, light absorption or light reflection properties; antioxidants and dispersing aids.

13. The impact modified hydrophobic acrylic composition of claim 12, wherein the antioxidant is present in an amount of 50 ppm to 3500 ppm based on the weight of the polymer solids.

14. An article comprising the impact modified hydrophobic acrylic composition of claims 1 to 13, wherein the article is selected from the group consisting of automotive LED grille lighting, automotive LED headlight covers, automotive LED front / rear signature lighting tubes, optical protective films, moisture barrier films, digital printing films, weather resistant surface protection layers, surface protection layers for decking / railings, automotive, electronic devices, medical, digital printing, laser cutting, building and construction, lighting tubes, thin wall parts, optical lenses, extruded films, (co)extruded sheets / profiles, thermoformable sheets, cast sheets, composites, medical devices and LED / OLED displays.