Biomass-based stress hardening polymer and preparation process thereof

Through the multiple hydrogen bonding of biomass-based polymers and flexible small molecule chain extenders, combined with gelatin and agar colloids, the problem of unstable and non-degradable performance of existing impact-resistant materials is solved, and the stress relief of biomass-based polymers is achieved. Hardening and dynamic response meet environmental requirements and special application needs.

CN118791864APending Publication Date: 2024-10-18HUNAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411224210.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing impact-resistant materials have unstable performance, non-degradability and cold flow problems during application, making it difficult to meet environmental protection requirements and the needs of special occasions.

Method used

Using biomass-based polymers, through the melt blending of linear polymers and biomass colloids, multiple hydrogen bonding units and flexible small molecule chain extenders are introduced to form I and II type molecular structures, combined with gelatin and agar colloids to achieve stress Hardening and dynamic response.

Benefits of technology

The material's non-Newtonian fluid characteristics, excellent energy dissipation and impact resistance are achieved, broadening the application range, and achieving degradation under composting conditions, avoiding cold flow problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_5
    Figure SMS_5
  • Figure SMS_7
    Figure SMS_7
  • Figure SMS_9
    Figure SMS_9
Patent Text Reader

Abstract

The invention relates to a biomass-based stress hardening polymer and a preparation process thereof, the biomass-based stress hardening polymer is prepared by blending a linear polymer A and a biomass colloid, and the linear polymer A is obtained by polymerizing a hydroxyl-terminated biopolyester oligomer, an isocyanate-terminated caprolactone oligomer, a multi-hydrogen-bond interaction biomass unit and a flexible micromolecule chain extender; the stress hardening polymer has good strength and toughness, has an obvious hardening characteristic in a rapid stretching process, and can resist rapid stretching and a relatively large impact effect; meanwhile, the polymer has thermoplasticity, can be easily prepared into different shapes and can be applied to the fields of human body protection, impact resistance of functional materials and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a biomass-based polymer, in particular to a biomass-based polymer capable of producing stress hardening effect through multiple hydrogen bonding and nonlinear change of macromolecular modulus. Background Art

[0002] Flexibility, high functionality and protection can greatly expand the application range of materials. In the field of material protection, a non-Newtonian fluid has recently emerged, which is soft under normal conditions but exhibits excellent impact resistance under high-speed deformation or large shear force, and is widely used in protection and functional fields.

[0003] The earliest materials of this type were shear thickening fluids, such as starch aqueous solutions and magnetic fluids. When the starch reaches a certain volume fraction, the mixed liquid exhibits very good impact resistance due to the hydraulic aggregation of particles under stress, and can withstand people running on it without falling. However, due to the large amount of solvent, it is easy to volatilize and produce performance instability. Subsequently, in order to further expand its application, solid or semi-solid non-Newtonian fluids were gradually developed, typically a mixture of hydroxy silicone oil and polyboric acid based on boron-oxygen bonds. Since the relaxation time of the binding-dispersion of the BO bond in the polymer is shorter than the movement time of the macromolecule when it is stressed or sheared, a large amount of energy is dissipated and converted into heat, thereby realizing this hardening behavior under high stress-strain and realizing intelligent impact resistance. Although this polymer has attractive performance, it has significant cold flow and is prone to deformation, and is still not suitable for applications in some special occasions. In recent years, research on achieving this special hardening through other dynamic bond combinations has gradually emerged. In this field, some biological tissues provide references, such as the echinoderms sea cucumber, which can reversibly change the hardness of their internal dermis in response to external dermal stimuli and thus exhibit stimulus-responsive and mechanical adaptive properties. The realization of this characteristic of sea cucumbers is based on the hard collagen fibrils enhancing the soft matrix stiffness, and this regulatory mechanism is achieved by the adjacent fibrils through transient regulatory interactions. In order to imitate and realize this special function, some polymers with non-strong bonds such as reversible hydrogen bonds and metal ligands have been constructed, and their good energy dissipation and impact resistance have been confirmed. For example, Yu Wei et al. introduced 2-ureido-4-pyridone as a multi-hydrogen bond biomass unit into the polyurethane structure to achieve non-Newtonian fluid behavior (J. Am. Chem. Soc. 2021, 143, 1162-1170), and the patent (202310456261.3) introduced oligomeric polyamide as a rigid unit into the elastomer, and the developed polymer also has good impact resistance.

[0004] Although the performance has been gradually achieved, the developed polymers are not degradable, and the performance of the materials still needs to be explored. With the improvement of environmental protection requirements for materials, the development of degradable special functional materials will undoubtedly be more attractive. In order to achieve better performance and degradability, the present invention uses biomass as the main raw material to construct a light and soft material that can achieve dynamic response and has non-Newtonian fluid properties, which can achieve excellent energy dissipation and impact resistance, thereby greatly broadening the application range of such materials. Summary of the invention

[0005] The purpose of the present invention is to develop a functional impact-resistant material which takes biomass-based materials as main raw materials and has the nonlinear mechanical property of stress hardening.

[0006] The objective of the present invention is achieved through the following technical solutions: A biomass-based stress-hardening polymer, which is formed by melt blending a linear polymer A and a biomass colloid with a mass ratio of 10% to 20% of the linear polymer A; the linear polymer A is polymerized by a terminal hydroxyl biopolyester oligomer, an isocyanate-terminated caprolactone oligomer, a multi-hydrogen-bonded biomass unit, and a flexible small molecule chain extender, and its molecular structure contains the following two molecular structure forms I and II, and the two forms exist in the polymer in any proportion; I: ZR n Z; II: Z(R a TR b )Z; n, a, b are the degrees of polymerization of each chain segment; n=5-15, a+b=10-20; Where R=

[0007] In the molecular structure formula, A is the main chain of biopolyester excluding the terminal hydroxyl group, B is the main chain of caprolactone oligomer excluding the terminal isocyanate group, T is the main chain of flexible small molecule chain extender excluding the terminal hydroxyl and amine groups; Z is the main chain of multiple hydrogen bond biomass units excluding the terminal reactive hydroxyl group.

[0008] Furthermore, the polymerization degrees of A and B are determined by the raw materials.

[0009] Further, the preparation process of the linear polymer A is as follows: a hydroxyl-terminated biopolyester oligomer and an isocyanate-terminated caprolactone oligomer are prepared as raw materials with a molar ratio of hydroxyl content to isocyanate content of 1:2-2.5, the two are put into a reactor filled with nitrogen, and reacted at 70-100°C for 0.5-1 hour to obtain a prepolymer 1; then 5-10 times the mass of the two reactants of N, N-dimethylformamide are added to dissolve the prepolymer A, and after stirring and dissolving completely, multiple hydrogen bonding biomass units are added, and the reaction is fully reacted at 60-90°C for 1-2 hours, and then a soft The reaction was continued at 60-90°C for 1-2 hours, the mixture after the reaction was introduced into a polytetrafluoroethylene mold, and the mixture was placed in a vacuum oven at 70-90°C for 12-24 hours to complete the reaction, and the crude polymer obtained by the reaction was dissolved in tetrahydrofuran, and precipitated with hexane to obtain a purified polymer A; wherein the molar number of the added multiple hydrogen bonding biomass unit is between 30% and 60% of the terminal isocyanate caprolactone oligomer, and the molar number of the added flexible small molecule chain extender is between 5% and 15% of the terminal isocyanate caprolactone oligomer.

[0010] Furthermore, the degree of polymerization and molecular structure are generated during the polymerization process and are affected by temperature, feed, etc., and also have a certain degree of randomness.

[0011] Furthermore, the hydroxyl-terminated bio-polyester oligomer may be one of hydroxyl-terminated polycaprolactone, hydroxyl-terminated polylactic acid, and hydroxyl-terminated (lactic acid-caprolactone) copolymer, with a molecular weight between 4000-20000 and a molecular weight distribution between 1.2-2.5.

[0012] Furthermore, the above-mentioned terminal hydroxyl biopolyester oligomer can be obtained by hydroxyl-terminated during the synthesis process of the biopolyester oligomer. For example, the terminal hydroxyl (lactic acid-caprolactone) copolymer can be prepared by referring to the literature: Fan Guodong, et al., Materials Guide, 2011, 25(8): 38-41.; the terminal hydroxyl polycaprolactone oligomer can be prepared by referring to the literature: Liu Ting, et al., Polyurethane Industry, 2015, 30(05): 10-13.

[0013] Furthermore, the above-mentioned terminal hydroxyl bio-polyester oligomers can be purchased as commercial products, and can be customized from, for example, Guangzhou Carbon Water Technology Co., Ltd.

[0014] Furthermore, the isocyanate-terminated caprolactone oligomer is an isocyanate-terminated product of a polycaprolactone oligomer, has an average functionality between 1.4 and 1.8, and has an oligomer molecular weight between 2000 and 6000.

[0015] Furthermore, the preparation of the isocyanate-terminated caprolactone oligomer can be obtained by using commercially available polycaprolactone diol of a certain molecular weight as a raw material, dissolving it in DMSO or DMF, and then adding an excess of diisocyanate substances such as MDI or HDI to cap it.

[0016] Furthermore, the multiple hydrogen bonding biomass unit is one of 5-hydroxymethyl uracil and 6-thio-2-hydroxypurine, and its molecular structure is as follows: 5-Hydroxymethyluracil: ; 6-Thio-2-hydroxypurine: .

[0017] Furthermore, the flexible small molecule chain extender is a terminal hydroxyl or terminal amine small molecule with a functionality of 2, and can be a small molecule diol, a diamine such as ethylene glycol, ethylenediamine, or a linear oligomer with a terminal hydroxyl or amine group, such as oligobutylene glycol, with a molecular weight between 100-1000, preferably between 200-600.

[0018] Furthermore, the biomass colloid is gelatin, agar gel or a mixture of the two in any proportion.

[0019] Furthermore, the soft-hard transition degree and impact resistance degree of the stress-hardening polymer from normal state to stress impact can be achieved by increasing the proportion of multiple hydrogen-bonded biomass units, but increasing a single component will also affect other properties of the material.

[0020] Furthermore, the present invention mainly uses biomass as raw material to achieve stress hardening of polymers, which is achieved through the following beneficial effects: first, multiple hydrogen bonding units are introduced into the macromolecular chain, which will produce dynamic hydrogen bonding during the stretching process, thereby achieving hardening; second, gelatin and agar components are added through blending, both of which are composed of amino acids. On the one hand, the macromolecule itself has a helical structure, which will increase the modulus during the stretching process. On the other hand, its molecular chain itself has a large number of carboxyl groups and amine groups, which will also produce hydrogen bonding with the hydrogen bonding units in the polymer, thereby dynamically strengthening the hardening effect.

[0021] Furthermore, the prepared polymer has no cold flow property and can be stored stably.

[0022] Furthermore, the original mechanical properties of the stress-hardening polymer can be adjusted by adjusting the ratio of reactants. When the thickness of the standard spline, i.e. the dumbbell spline, is 5 mm, the tensile strength at 5 mm / min is between 0.2-0.8 MPa, and the tensile strength at 50 mm / min is between 3.5-6.7 MPa; when the material with a thickness of 10 mm is compressed at a compression rate of 5 mm / min, the strength is 6-12 MPa when compressed to 60% deformation, and when the compression rate is 50 mm / min, the strength is 32-45 MPa when compressed to 60% deformation.

[0023] Furthermore, the stress hardening polymer has a storage modulus G' between 5*10 3 -4*10 4 Under 100Hz frequency scanning, its storage modulus G' is between 5*10 6 -2*10 7 between.

[0024] Furthermore, when measured by a falling ball impact tester, the energy dissipation rate of the 5 mm thick material is between 75-100% when the impact energy is between 0-1000 J / m, and the energy dissipation rate is between 55-75% when the impact energy is between 1000-2000 J / m; it can ultimately withstand 2000-3000 J / m energy without breaking; at the same time, the impact energy absorbed by the material is directly related to its thickness.

[0025] Furthermore, the stress-hardening polymer can be degraded within 3-5 weeks under composting conditions. DETAILED DESCRIPTION

[0026] The embodiments of the present application will be described in detail below in conjunction with examples, but those skilled in the art will understand that the following examples are only used to illustrate the present application and should not be construed as limiting the scope of the present application. Example 1

[0027] A biomass-based stress-hardening polymer is prepared by melt blending a linear polymer A and a biomass colloid of 10% to 20% by mass; the linear polymer A is polymerized by a terminal hydroxyl biopolyester oligomer, an isocyanate-terminated caprolactone oligomer, a multi-hydrogen-bonded biomass unit, and a flexible small molecule chain extender, and its molecular structure contains the following two molecular structure forms, I and II, wherein the molar ratio of type I to type II is about 35:65; I: ZR n Z; II: Z(R a TR b )Z; n, a, b are the degrees of polymerization of each chain segment; n=12, a+b=20; Where R=

[0028] In the molecular structure formula, A is the main chain of biopolyester except the terminal hydroxyl group, B is the main chain of caprolactone oligomer except the terminal isocyanate group, T is the main chain of flexible small molecule chain extender except the terminal hydroxyl group and amine group; Z is the main chain of biomass unit with multiple hydrogen bonds except the terminal reactive hydroxyl group; The preparation process of the linear polymer A is as follows: a terminal hydroxyl biopolyester oligomer and a terminal isocyanate caprolactone oligomer are prepared as raw materials with a molar ratio of hydroxyl content and isocyanate content of the two respectively measured to be 1:2.2, the two are put into a reactor filled with nitrogen, and reacted at 80°C for 0.6 hours to obtain a prepolymer A; then N, N-dimethylformamide is added in an amount of 8 times the sum of the masses of the two reactants to dissolve the prepolymer A, and after the prepolymer A is completely dissolved, a multi-hydrogen bond biomass unit is added, and the reaction is fully carried out at 70°C for 1.5 hours, and then A flexible small molecule chain extender is added, and the reaction is continued at 70°C for 1.5 hours. The reaction mixture is introduced into a polytetrafluoroethylene mold, and placed in a vacuum oven at 80°C for 16 hours to complete the reaction. Finally, the crude polymer is dissolved in tetrahydrofuran and precipitated with hexane to obtain a purified polymer; wherein the molar number of the added multiple hydrogen bonding biomass unit is 45% of the terminal isocyanate caprolactone oligomer, and the molar number of the added flexible small molecule chain extender is between 12% of the terminal isocyanate caprolactone oligomer.

[0029] The terminal hydroxyl biopolyester oligomer is terminal hydroxyl polylactic acid, with a molecular weight between 5500 and 12000 and a molecular weight distribution of 2.1.

[0030] The isocyanate-terminated caprolactone oligomer is an isocyanate-terminated product of a polycaprolactone oligomer, has an average functionality of 1.6, and an average molecular weight of 3,200.

[0031] The multiple hydrogen bonding biomass unit is 5-hydroxymethyl uracil, and its molecular structure is as follows:

[0032] The flexible small molecule chain extender is ethylenediamine.

[0033] The biomass colloid is gelatin.

[0034] The properties of the stress hardening polymer are as follows: (1) Tensile test was performed on dumbbell-shaped specimens with a thickness of 5 mm; When stretched at a speed of 5 mm / min, the tensile strength is 0.42 MPa, and when stretched at a speed of 50 mm / min, the tensile strength is 4.6 MPa; (2) Compression test was performed on a 100mm*100mm*10mm block sample; When the compression rate is 5 mm / min, the strength is 8.4 MPa when compressed to 60% deformation. When the compression rate is 50 mm / min, the strength is 37.3 MPa when compressed to 60% deformation.

[0035] (3) Impact test was performed on block samples of 100mm*100mm*5mm; When the impact energy is 1000J / m, the energy dissipation rate is 96%, and when the impact energy is 2000J / m, the energy dissipation rate is 70%; the maximum impact energy that can be resisted is about 2200J / m; (4) When the sample thickness is 10 mm, the maximum impact energy it can withstand is approximately 4100 J / m.

[0036] (5) The stress-hardening polymer was measured for its rheological properties by a rotational rheometer. Under a 0.1% strain and 1 Hz frequency scan, its storage modulus G' was approximately 8.2*10 3 , under 100Hz frequency scanning, its storage modulus G' is 9.5*10 6 .

[0037] The stress-hardening polymer can be degraded within 3.5 weeks under composting conditions.

[0038] Example 2 A biomass-based stress-hardening polymer is prepared by melt blending a linear polymer A and a biomass colloid of 10% to 20% by mass; the linear polymer A is polymerized by a terminal hydroxyl biopolyester oligomer, a terminal isocyanate caprolactone oligomer, a multi-hydrogen-bonded biomass unit, and a flexible small molecule chain extender, and its molecular structure contains the following two molecular structure forms, I and II, wherein the molar ratio of type I to type II is about 42:58; I: ZR n Z; II: Z(R a TR b )Z; n, a, b are the degrees of polymerization of each segment; n=10, a+b=16; Where R=

[0039] In the molecular structure formula, A is the main chain of biopolyester except the terminal hydroxyl group, B is the main chain of caprolactone oligomer except the terminal isocyanate group, T is the main chain of flexible small molecule chain extender except the terminal hydroxyl group and amine group; Z is the main chain of biomass unit with multiple hydrogen bonds except the terminal reactive hydroxyl group; The preparation process of the linear polymer A is as follows: a terminal hydroxyl biopolyester oligomer and a terminal isocyanate caprolactone oligomer are prepared as raw materials with a molar ratio of hydroxyl content and isocyanate content of the two being 1:2.4, and the two are put into a reactor filled with nitrogen, and reacted at 90°C for 3.5 hours to obtain a prepolymer A; then, N,N-dimethylformamide is added in an amount of 6 times the mass of the two reactants to dissolve the prepolymer A, and after the prepolymer A is completely dissolved, a multi-hydrogen bond biomass unit is added, and the reaction is fully reacted at 80°C for 0.8 hours. A flexible small molecule chain extender is then added, and the reaction is continued at 80°C for 1.2 hours. The mixture after the reaction is introduced into a polytetrafluoroethylene mold, and placed in a vacuum oven at 80°C for 20 hours to complete the reaction. Finally, the crude polymer is dissolved in tetrahydrofuran and then precipitated with hexane to obtain a purified polymer; wherein the molar number of the added multiple hydrogen bonding biomass unit is 50% of the terminal isocyanate caprolactone oligomer, and the molar number of the added flexible small molecule chain extender is between 6% of the terminal isocyanate caprolactone oligomer.

[0040] The terminal hydroxyl biopolyester oligomer is terminal hydroxyl polycaprolactone, the molecular weight of which is between 4500 and 8000, and the molecular weight distribution is 1.8.

[0041] The isocyanate-terminated caprolactone oligomer is an isocyanate-terminated product of a polycaprolactone oligomer, has an average functionality of 1.6, and an average molecular weight of 3,200.

[0042] The multiple hydrogen bonding biomass unit is 6-thio-2-hydroxypurine, and its molecular structure is as follows:

[0043] The flexible small molecule chain extender is hydroxy-terminated oligobutylene glycol with a molecular weight of 860.

[0044] The biomass colloid is agar colloid.

[0045] The properties of the stress hardening polymer are as follows: (1) Tensile test was performed on dumbbell-shaped specimens with a thickness of 5 mm; When stretched at a speed of 5 mm / min, the tensile strength is 0.42 MPa, and when stretched at a speed of 50 mm / min, the tensile strength is 5.3 MPa; (2) Compression test was performed on a 100mm*100mm*10mm block sample; When the compression rate is 5 mm / min, the strength is 7.1 MPa when compressed to 60% deformation. When the compression rate is 50 mm / min, the strength is 39.7 MPa when compressed to 60% deformation.

[0046] (3) Impact test was performed on block samples of 100mm*100mm*5mm; When the impact energy is 1000J / m, the energy dissipation rate is 94%, and when the impact energy is 2000J / m, the energy dissipation rate is 67%; the maximum impact energy that can be resisted is about 2700J / m; (4) When the sample thickness is 10 mm, the maximum impact energy it can withstand is approximately 4300 J / m.

[0047] (5) The stress-hardening polymer was measured for its rheological properties by a rotational rheometer. Under a 0.1% strain and 1 Hz frequency scan, its storage modulus G' was approximately 2.1*10 4 , under 100Hz frequency scanning, its storage modulus G' is 1.1*10 7 .

[0048] The stress-hardening polymer can be degraded within 4 weeks under composting conditions.

[0049] Example 3 A biomass-based stress-hardening polymer is prepared by melt blending a linear polymer A and a biomass colloid of 10% to 20% by mass; the linear polymer A is polymerized by a terminal hydroxyl biopolyester oligomer, an isocyanate-terminated caprolactone oligomer, a multi-hydrogen-bonded biomass unit, and a flexible small molecule chain extender, and its molecular structure contains the following two molecular structure forms, I and II, wherein the molar ratio of type I to type II is about 62:38; I: ZR n Z; II: Z(R a TR b )Z; n, a, b are the degrees of polymerization of each chain segment; n=8, a+b=18; Where R=

[0050] In the molecular structure formula, A is the main chain of biopolyester excluding the terminal hydroxyl group, B is the main chain of caprolactone oligomer excluding the terminal isocyanate group, T is the main chain of flexible small molecule chain extender excluding the terminal hydroxyl and amine groups; Z is the main chain of multiple hydrogen bond biomass units excluding the terminal reactive hydroxyl group.

[0051] The synthesis process of the linear polymer chain A is as follows: adding a terminal hydroxyl biopolyester oligomer and a terminal isocyanate caprolactone oligomer in a ratio of 1:2.3 of the measured hydroxyl content to isocyanate content into a nitrogen-filled reactor, reacting at 80°C for 0.5 hours to obtain a prepolymer A; then adding N,N-dimethylformamide 10 times the mass of the prepolymer A to dissolve the prepolymer 1, adding a multi-hydrogen bond biomass unit after the dissolution is complete, fully reacting at 85°C for 1.5 hours, and then adding a flexible small component The reaction was continued at 85°C for 1.5 hours, the reaction mixture was introduced into a polytetrafluoroethylene mold, and it was placed in a vacuum oven at 85°C for 16 hours to complete the reaction, and finally the crude polymer was dissolved in tetrahydrofuran and precipitated with hexane to obtain a purified polymer; wherein the molar number of the added multiple hydrogen bonding biomass unit is 35% of the terminal isocyanate caprolactone oligomer, and the molar number of the added flexible small molecule chain extender is between 14% of the terminal isocyanate caprolactone oligomer.

[0052] The terminal hydroxyl biopolyester oligomer is a terminal hydroxyl (lactic acid-caprolactone) copolymer, with a molecular weight between 6000 and 12000 and a molecular weight distribution of 1.5.

[0053] The isocyanate-terminated caprolactone oligomer is an isocyanate-terminated product of a polycaprolactone oligomer, has an average functionality of 1.7, and an average molecular weight of 4,300.

[0054] The biomass colloid is gelatin.

[0055] The multiple hydrogen bonding biomass unit is 5-hydroxymethyl uracil, and its molecular structure is as follows:

[0056] The flexible small molecule chain extender is ethylenediamine.

[0057] The properties of the stress hardening polymer are as follows: (1) Tensile test was performed on dumbbell-shaped specimens with a thickness of 5 mm; When stretched at a speed of 5 mm / min, the tensile strength is 0.54 MPa, and when stretched at a speed of 50 mm / min, the tensile strength is 6.2 MPa; (2) Compression test was performed on a 100mm*100mm*10mm block sample; When the compression rate is 5 mm / min, the strength is 8.4 MPa when compressed to 60% deformation. When the compression rate is 50 mm / min, the strength is 42.3 MPa when compressed to 60% deformation.

[0058] (3) Impact test was performed on block samples of 100mm*100mm*5mm; When the impact energy is 1000J / m, the energy dissipation rate is 95%, and when the impact energy is 2000J / m, the energy dissipation rate is 73%; the maximum impact energy that can be resisted is about 2900J / m; (4) When the sample thickness is 10 mm, the maximum impact energy it can withstand is approximately 4400 J / m.

[0059] (5) The stress-hardening polymer is measured by a rotational rheometer to determine its rheological properties. Under a 0.1% strain and 1 Hz frequency scan, its storage modulus G' is approximately 2.6*10 4 , under 100Hz frequency scanning, its storage modulus G' is 1.3*10 7 .

[0060] The stress-hardening polymer can be degraded within 3.5 weeks under composting conditions.

[0061] Example 4 A biomass-based stress-hardening polymer is prepared by melt blending a linear polymer A and a biomass colloid of 10% to 20% by mass; the linear polymer A is polymerized by a terminal hydroxyl biopolyester oligomer, an isocyanate-terminated caprolactone oligomer, a multi-hydrogen-bonded biomass unit, and a flexible small molecule chain extender, and its molecular structure contains the following two molecular structure forms, I and II, wherein the molar ratio of type I to type II is about 57:43; I: ZR n Z; II: Z(R a TR b )Z; n, a, b are the degrees of polymerization of each segment; n=6, a+b=12; Where R=

[0062] In the molecular structure formula, A is a biopolyester chain, B is a caprolactone oligomer chain, T is the main chain remaining after the terminal reaction groups of the flexible small molecule chain extender are removed; and Z is the main chain remaining after the terminal reaction groups of the biomass unit with multiple hydrogen bonds are removed.

[0063] The synthesis process of the linear polymer chain A is as follows: adding a terminal hydroxyl biopolyester oligomer and a terminal isocyanate caprolactone oligomer in a ratio of 1:2.1 of the measured hydroxyl content to isocyanate content into a nitrogen-filled reactor, reacting at 80°C for 0.6 hours to obtain a prepolymer A; then adding N,N-dimethylformamide in an amount 7 times the mass of the two reactants to dissolve the prepolymer 1, adding a multi-hydrogen bond biomass unit after the dissolution is complete, fully reacting at 75°C for 2 hours, and finally adding a flexible small The reaction was continued at 75°C for 2 hours, the reaction mixture was introduced into a polytetrafluoroethylene mold, and it was placed in a vacuum oven at 80°C for 24 hours to complete the reaction, and finally the crude polymer was dissolved in tetrahydrofuran and precipitated with hexane to obtain a purified polymer; wherein the molar number of the added multiple hydrogen bonding biomass unit is 55% of the terminal isocyanate caprolactone oligomer, and the molar number of the added flexible small molecule chain extender is between 13% of the terminal isocyanate caprolactone oligomer.

[0064] The terminal hydroxyl biopolyester oligomer is terminal hydroxyl polylactic acid, with a molecular weight between 4000 and 14000 and a molecular weight distribution of 2.1.

[0065] The isocyanate-terminated caprolactone oligomer is an isocyanate-terminated product of a polycaprolactone oligomer, has an average functionality of 1.6, and an average molecular weight of 5100.

[0066] The biomass colloid is agar colloid.

[0067] The multiple hydrogen bonding biomass unit is 6-thio-2-hydroxypurine, and its molecular structure is as follows:

[0068] The flexible small molecule chain extender is propylene diamine.

[0069] The properties of the stress hardening polymer are as follows: (1) Tensile test was performed on dumbbell-shaped specimens with a thickness of 5 mm; When stretched at a speed of 5 mm / min, the tensile strength is 0.36 MPa, and when stretched at a speed of 50 mm / min, the tensile strength is 5.4 MPa; (2) Compression test was performed on a 100mm*100mm*10mm block sample; When the compression rate is 5mm / min, the strength is 7.1MPa when compressed to 60% deformation, and when the compression rate is 50mm / min, the strength is 36.7MPa when compressed to 60% deformation; (3) Impact test was performed on block samples of 100mm*100mm*5mm; When the impact energy is 1000J / m, the energy dissipation rate is 96%, and when the impact energy is 2000J / m, the energy dissipation rate is 74%; the maximum impact energy that can be resisted is about 2600J / m; (4) When the sample thickness is 10 mm, the maximum impact energy it can withstand is approximately 4300 J / m.

[0070] (5) The stress-hardening polymer was measured for its rheological properties by a rotational rheometer. Under a 0.1% strain and 1 Hz frequency scan, its storage modulus G' was approximately 7.8*10 3 , under 100Hz frequency scanning, its storage modulus G' is 9.2*10 6 .

[0071] The stress-hardening polymer can be degraded within 3.5 weeks under composting conditions.

[0072] Comparative Example 1 A biomass-based stress-hardening polymer, compared with Example 1, only gelatin is not added during blending, and other processes are the same.

[0073] The prepared polymer still has shear hardening characteristics, and its properties are as follows: (1) Tensile test was performed on dumbbell-shaped specimens with a thickness of 5 mm; When stretched at a speed of 5 mm / min, the tensile strength is 0.12 MPa, and when stretched at a speed of 50 mm / min, the tensile strength is 3.2 MPa; (2) Compression test was performed on a 100mm*100mm*10mm block sample; When the compression rate is 5 mm / min, the strength is 2.1 MPa when compressed to 60% deformation. When the compression rate is 50 mm / min, the strength is 16.4 MPa when compressed to 60% deformation.

[0074] (3) Impact test was performed on block samples of 100mm*100mm*5mm; When the impact energy is 500J / m, the energy dissipation rate is 94%, and when the impact energy is 1000J / m, the energy dissipation rate is 73%; the maximum impact energy that can be resisted is about 1500J / m; (4) When the sample thickness is 10 mm, the maximum impact energy it can withstand is approximately 1800 J / m.

[0075] (5) The storage modulus G' of the stress-hardening polymer under 0.1% strain and 1 Hz frequency scanning is about 2.1*10 3 , under 100Hz frequency scanning, its storage modulus G' is 2.8*10 5 .

[0076] The stress hardening polymer has significant cold flow properties, and the thickness of a 50mm*50mm*20mm sample is reduced to 4.5mm after 3 days.

[0077] The stress-hardening polymer can be degraded within 5 weeks under composting conditions.

[0078] Due to the lack of gelatin's skeleton and reinforcement effects, although the polymer still has a stress response effect, its strength under normal conditions is significantly reduced, its cold flow is significantly increased, and its ability to resist impact is reduced.

[0079] Comparative Example 2 A biomass-based stress-hardening polymer, compared with Example 1, does not add multiple hydrogen-bonding biomass units in the preparation process, that is, there is no step of adding multiple hydrogen-bonding biomass units and fully reacting at 70°C for 1.5 hours, but directly adds a flexible small molecule chain extender and continues to react at 70°C for 1.5 hours.

[0080] The shear hardening characteristics of the prepared polymer disappeared and its properties were as follows: (1) Tensile test was performed on dumbbell-shaped specimens with a thickness of 5 mm; When stretched at a speed of 5 mm / min, the tensile strength is 1.36 MPa, and when stretched at a speed of 50 mm / min, the tensile strength is 2.14 MPa; (2) Compression test was performed on a 100mm*100mm*10mm block sample; When the compression rate is 5 mm / min, the strength is 6.2 MPa when compressed to 60% deformation. When the compression rate is 50 mm / min, the strength is 8.6 MPa when compressed to 60% deformation.

[0081] (3) Impact test was performed on block samples of 100mm*100mm*5mm; When the impact energy is 500J / m, the energy dissipation rate is 46%, and when the impact energy is 1000J / m, the energy dissipation rate is 31%; the maximum impact energy that can be resisted is about 1120J / m; (4) When the sample thickness is 10 mm, the maximum impact energy it can withstand is approximately 1400 J / m.

[0082] (5) The storage modulus G' of the stress-hardening polymer under 0.1% strain and 1 Hz frequency scanning is about 9.6*10 3 , under 100Hz frequency scanning, its storage modulus G' is 8.4*10 4, The initial modulus increases and the stress hardening effect almost disappears.

[0083] The stress-hardening polymer can be degraded within 3 weeks under composting conditions.

[0084] After removing the hydrogen bonding unit, the uncapped structure leads to an increase in the molecular weight of the polymer. The basic mechanical properties of the polymer are not reduced, but the performance at high deformation rates is not significantly improved. The rheological properties show that its shear hardening characteristics almost disappear and the energy dissipation capacity is greatly weakened.

[0085] Comparative Example 3

[0086] A biomass-based stress-hardening polymer, compared with Example 1, does not add a small molecule flexible small molecule chain extender in the preparation process, that is, omitting the step of adding the flexible small molecule chain extender and continuing the reaction at 60-90° C. for 1-2 hours.

[0087] All the prepared polymers are ZR n Z form, n is between 5-25.

[0088] The shear hardening properties of the prepared polymer also weakened, and the basic properties changed greatly, showing more obvious properties of polyurethane elastomers. Its properties are as follows: (1) Tensile test was performed on dumbbell-shaped specimens with a thickness of 5 mm; When stretched at a speed of 5 mm / min, the tensile strength is 3.36 MPa, and when stretched at a speed of 50 mm / min, the tensile strength is 5.27 MPa; (2) Compression test was performed on a 100mm*100mm*10mm block sample; When the compression rate is 5 mm / min, the strength is 8.1 MPa when compressed to 60% deformation. When the compression rate is 50 mm / min, the strength is 26.4 MPa when compressed to 60% deformation.

[0089] (3) Impact test was performed on block samples of 100mm*100mm*5mm; When the impact energy is 500J / m, the energy dissipation rate is 62%, and when the impact energy is 1000J / m, the energy dissipation rate is 54%; the maximum impact energy that can be resisted is about 1460J / m; (4) When the sample thickness is 10 mm, the maximum impact energy it can withstand is approximately 2270 J / m.

[0090] (5) The storage modulus G' of the stress-hardening polymer under 0.1% strain and 1 Hz frequency scanning is about 6.2*10 2 , under 100Hz frequency scanning, its storage modulus G' is 7.9*10 4 .

[0091] The stress-hardening polymer can be degraded within 4 weeks under composting conditions.

[0092] Since no small molecule chain extender is added, the molecular chains are terminated by hydrogen bonding units, the molecular chain length is reduced, and the molecular weight interaction is enhanced, resulting in a stronger stable bond. Therefore, the basic mechanical properties are improved, but the responsiveness is weakened and the energy dissipation is weakened.

[0093] Comparative Example 4 A biomass-based stress-hardening polymer, compared with Example 1, the molar number of the added multiple hydrogen-bonding biomass units is 8% of the terminal isocyanate caprolactone oligomer, and the molar number of the added flexible small molecule chain extender is between 24% of the terminal isocyanate caprolactone oligomer; at the same time, no gelatin is added for blending.

[0094] The properties of the prepared polymer are as follows: (1) Tensile test was performed on dumbbell-shaped specimens with a thickness of 5 mm; When stretched at a speed of 5 mm / min, the tensile strength is 8.24 MPa, and when stretched at a speed of 50 mm / min, the tensile strength is 12.9 MPa; (2) Compression test was performed on a 100mm*100mm*10mm block sample; When the compression rate is 5 mm / min, the strength is 12.6 MPa when compressed to 60% deformation. When the compression rate is 50 mm / min, the strength is 18.7 MPa when compressed to 60% deformation.

[0095] (3) Impact test was performed on block samples of 100mm*100mm*5mm; When the impact energy is 500J / m, the energy dissipation rate is 96%, and when the impact energy is 1000J / m, the energy dissipation rate is 82%; the maximum impact energy that can be resisted is about 1400J / m; (4) When the sample thickness is 10 mm, the maximum impact energy it can withstand is approximately 2100 J / m.

[0096] (5) The storage modulus G' of the stress-hardened polymer under 0.1% strain and 1 Hz frequency scanning is about 6.1*10 3 , under 100Hz frequency scanning, its storage modulus G' is 8.4*10 5 .

[0097] The stress-hardening polymer can be degraded within 3.5 weeks under composting conditions.

[0098] Due to the reduction of multiple hydrogen-bonding biomass units and the increase of flexible small molecule chain extenders, the responsive binding components are reduced, while the overall molecular weight is greatly increased, the basic mechanical properties are increased, but the stress-strain responsiveness is weakened.

Claims

1. A biomass-based stress-hardening polymer, which is formed by melt blending a linear polymer A and a biomass colloid of 10% to 20% by mass; the linear polymer A is polymerized by a terminal hydroxyl biopolyester oligomer, an isocyanate-terminated caprolactone oligomer, a multi-hydrogen-bonded biomass unit, and a flexible small molecule chain extender, and its molecular structure contains the following two molecular structure forms I and II, and the two forms exist in any proportion in the polymer; I: ZR n Z; II: Z(R a TR b )Z; n, a, b are the degrees of polymerization of each chain segment; n=5-15, a+b=10-20; Where R= ; In the molecular structure formula, A is the main chain of biopolyester except the terminal hydroxyl group, B is the main chain of caprolactone oligomer except the terminal isocyanate group, T is the main chain of flexible small molecule chain extender except the terminal hydroxyl group and amine group; Z is the main chain of biomass unit with multiple hydrogen bonds except the terminal reactive hydroxyl group; Its characteristics are also: The preparation process of the linear polymer A is as follows: a terminal hydroxyl biopolyester oligomer and a terminal isocyanate caprolactone oligomer are prepared as raw materials with a molar ratio of hydroxyl content to isocyanate content of 1:2-2.5, the two are put into a reactor filled with nitrogen, and react at 70-100° C. for 0.5-1 hour to obtain a prepolymer 1; then 5-10 times the mass of the two reactants of N, N-dimethylformamide are added to dissolve the prepolymer A, and after stirring and dissolving completely, multiple hydrogen bonding biomass units are added, and the reaction is fully carried out at 60-90° C. for 1-2 hours, and then a flexible small The molecular chain extender is continued to react at 60-90°C for 1-2 hours, the mixture after the reaction is introduced into a polytetrafluoroethylene mold, and the mixture is placed in a vacuum oven at 70-90°C for 12-24 hours to complete the reaction, and the crude polymer obtained by the reaction is dissolved in tetrahydrofuran, and precipitated with hexane to obtain a purified polymer A; wherein the molar number of the added multiple hydrogen bonding biomass unit is between 30% and 60% of the terminal isocyanate caprolactone oligomer, and the molar number of the added flexible small molecule chain extender is between 5% and 15% of the terminal isocyanate caprolactone oligomer.

2. A biomass-based stress-hardening polymer, characterized in that: The hydroxyl-terminated bio-polyester oligomer may be one of hydroxyl-terminated polycaprolactone, hydroxyl-terminated polylactic acid, and hydroxyl-terminated (lactic acid-caprolactone) copolymer, with a molecular weight between 4000 and 20000 and a molecular weight distribution between 1.2 and 2.

5.

3. A biomass-based stress-hardening polymer, characterized in that: The isocyanate-terminated caprolactone oligomer is an isocyanate-terminated product of a caprolactone oligomer, has an average functionality between 1.4 and 1.8, and has an oligomer molecular weight between 2000 and 6000.

4. A biomass-based stress-hardening polymer, characterized in that: The multiple hydrogen bonding biomass unit is one of 5-hydroxymethyl uracil and 6-thio-2-hydroxypurine, and its molecular structure is as follows: 5-Hydroxymethyluracil: ; 6-Thio-2-hydroxypurine: .

5. A biomass-based stress-hardening polymer, characterized in that: The flexible small molecule chain extender is a small molecule diol, a diamine, or a linear oligomer with a terminal group of a hydroxyl group or an amine group, and the molecular weight is between 100-1000.

6. A biomass-based stress-hardening polymer, characterized in that: The biomass colloid is gelatin, agar, or a mixture of the two in any proportion.

7. A biomass-based stress-hardening polymer, characterized in that: The impact resistance of the stress-hardening polymer is as follows: when the impact energy of a 5 mm thick material is between 0 and 1000 J / m, the energy dissipation rate is between 75 and 100%, and when the impact energy is between 1000 and 2000 J / m, the energy dissipation rate is between 55 and 75%. It can ultimately withstand 2000 to 3000 J / m energy without breaking, and recover flexibility after the impact ends.