Thermocatalytic functional coating material, thermocatalytic functional coating and cooking utensil
By applying thermocatalytic functional coating materials on the surface and cavity of cooking utensils, using variable-price metal oxides and binders to catalytically oxidize and degrade oil stains under low temperature conditions, the problems of oil stain deposition and bacterial growth in cooking utensils are solved, and long-lasting self-treatment is achieved. Cleaning function.
Patent Information
- Application Number
- CN202310404851.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-18
AI Technical Summary
The volatile oil fumes generated by existing cooking utensils during the cooking process are difficult to clean, causing oil stains to accumulate and breed bacteria, affecting health.
Thermal catalytic functional coating material is used, which contains variable-price metal oxides and binders. The coating is applied to the surface and cavity of the cooking utensils, and uses the heat generated during the cooking process to catalytically oxidize and degrade oil stains at 100°C-300°C.
It achieves long-term self-cleaning function on the surface of cooking utensils, avoids the accumulation of oil stains and bacterial growth, and reduces the difficulty of cleaning and energy consumption.
Smart Images

Figure CN118791891A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal catalysts, and in particular to a thermal catalytic functional coating material, a thermal catalytic functional coating, and a cooking utensil. Background Art
[0002] In recent years, with the rapid economic development and the continuous improvement of residents' living standards in my country, consumers have an increasingly strong demand for household cooking appliances. In particular, the popularization and use of small kitchen appliances with various types and functions have satisfied the desire of the majority of residents to easily cook and enjoy delicious food at home. For example, the air fryer, which has been favored by consumers in recent years, has quickly become a star product and "leader" in the domestic small household appliance industry due to its advantages such as less oil consumption, uniform heating, and short baking time. Similar to traditional large kitchen appliances, small kitchen appliances also produce a large amount of volatile oil smoke during the cooking process, which will be deposited and adhered to the surface of the cooking appliances to form oil stains. For small appliances such as air fryers with compact structural design and closed space, it is easy to form cleaning dead corners inside the cooking cavity, which brings many troubles to daily hygiene cleaning. The long-term accumulation of splashing oil stains in the cavity not only affects the appearance, but also makes it easier to breed bacteria, has a risk of cancer, and threatens people's health.
[0003] At present, thermal catalytic materials can be used to degrade the oil stains generated during the cooking process, but the thermal catalytic temperature of the thermal catalytic materials in the prior art is usually around 300°C. For some cooking utensils with cooking temperatures below 200°C, such as air fryers, the cooking temperature can be controlled within a range below 200°C. At this time, an additional self-cleaning function is required. After cooking is completed, the temperature needs to be heated to above 200°C or even above 300°C to complete cleaning, which increases energy loss. Summary of the invention
[0004] The main purpose of the present invention is to provide a thermal catalytic functional coating material and a preparation method and a thermal catalytic functional coating and cooking utensils, which can oxidatively degrade oil stains during the cooking process, thereby solving the technical problem in the prior art that cooking utensils easily generate a large amount of volatile oil smoke to form oil stains during the cooking process, which are deposited and adhered to the surface of the cooking utensils and are difficult to clean.
[0005] To achieve the above-mentioned object, the present invention provides a thermal catalytic functional coating material, which includes a catalyst and a binder, wherein the catalyst includes a metal oxide, and the metal oxide includes a variable-valence metal element.
[0006] In some embodiments of the present application, the variable-valence metal element includes at least one of Ce, Cu, Co, Fe, La, Mn and Ni.
[0007] In some embodiments of the present application, the metal oxide includes CeO 2 ,CuO,CoO,Co 3 O 4 , Fe 2 O 3 , Fe 3 O 4 、MnO 2 , Mn 2 O 3 , Mn 3 O 4 、NiO、LaMn x Co 1-x O 3 ,CuFe 2 O 4 、CuMn 2 O 4 , Cu 1.5 Mn 1.5 O 4 At least one of .
[0008] In some embodiments of the present application, the catalytic temperature of the thermal catalytic functional coating material is between 100°C and 300°C.
[0009] In some embodiments of the present application, the average particle size of the metal oxide is in the range of 2 nm-2 μm.
[0010] In some embodiments of the present application, the binder is an inorganic binder and / or an organic binder, including γ-Al 2 O 3 , SiO 2 , at least one of polyethersulfone and polyamideimide.
[0011] In some embodiments of the present application, calculated by mass percentage, the thermo-catalytic functional coating material includes 10%-90% of the metal oxide; and / or, the thermo-catalytic functional coating material includes 5%-70% of the binder.
[0012] In some embodiments of the present application, calculated by mass percentage, the thermo-catalytic functional coating material includes 30%-80% of the metal oxide; and / or, the thermo-catalytic functional coating material includes 10%-50% of the binder.
[0013] In some embodiments of the present application, the thermal catalytic functional coating material further includes less than or equal to 80% of a support calculated by mass percentage.
[0014] In some embodiments of the present application, the support is a micro-nano particle support with an average particle size ranging from 10 nm to 10 μm.
[0015] In some embodiments of the present application, the loading material includes γ-Al 2 O 3 、SiO 2 、TiO 2 、ZrO 2 , at least one of molecular sieves.
[0016] In some embodiments of the present application, the molecular sieve includes at least one of BETA molecular sieve, USY molecular sieve, and ZSM-5 molecular sieve.
[0017] In addition, to achieve the above-mentioned purpose, the present invention further provides a thermo-catalytic functional coating, wherein the thermo-catalytic functional coating comprises the thermo-catalytic functional coating material of the present invention as described above.
[0018] In some embodiments of the present application, the atomic percentage of the variable-valence metal element on the surface of the thermal catalytic functional coating is not less than 50% of the total atomic percentage of the variable-valence metal element in the thermal catalytic functional coating and is exposed to the air.
[0019] In some embodiments of the present application, the thickness of the thermocatalytic functional coating is in the range of 20 μm-2 mm.
[0020] In addition, to achieve the above-mentioned object, the present invention also provides a cooking utensil, comprising the thermocatalytic functional coating of the present invention as described above.
[0021] In some embodiments of the present application, the cooking appliance includes an electric pressure cooker, a frying pan, an automatic cooking machine, an air fryer or an electric baking pan.
[0022] In some embodiments of the present application, the cooking utensil has a heating module, and the thermo-catalytic functional coating is coated on the surface of the heating module and any inner surface in the cooking cavity.
[0023] In some embodiments of the present application, the cooking utensil is an air fryer, and the thermo-catalytic functional coating is coated on the surface of the heating module of the air fryer and any inner surface in the cooking cavity.
[0024] In some embodiments of the present application, the heating module of the air fryer is a disc-shaped metal heating tube.
[0025] The beneficial effects that can be achieved by the present invention are:
[0026] The present invention provides a thermal catalytic functional coating material, which includes a catalyst and a binder, wherein the catalyst includes a metal oxide, the metal oxide includes a variable-valence metal element, and has a large number of catalytic active sites on the surface, which can give the thermal catalytic functional coating material a stronger thermal catalytic function. When prepared into a coating, the catalytic active sites can be exposed to the air in large quantities and directly contact with oil stains. The catalytic activity can be stimulated under low-temperature heat source conditions of 100°C-300°C, and the oil stains can be oxidized and degraded during the cooking process without increasing additional consumption. Only the heating module of the cooking utensil is used, and the oil stains formed by volatile oil smoke generated by cooking can be degraded during the cooking process, ensuring that there is no grease deposition and residue in the cavity after cooking, avoiding the pain point of difficult cleaning inside the cavity, and truly realizing the long-term surface self-cleaning function of the cooking utensil.
[0027] The above-mentioned variable-valence metal elements include at least one of Ce, Cu, Co, Fe, La, Mn and Ni, so that the thermal catalytic functional coating material has the advantages of high catalytic effect, low cost, safety and reliability.
[0028] The binder can fix the metal oxide on the surface of the cooking utensil and expose its catalytic active sites to the air. The heat generated by the cooking utensil heating module directly catalyzes and oxidizes the grease that splashes onto the surface of the cooking utensil coated with the thermal catalytic functional coating, thereby avoiding the accumulation of grease.
[0029] In addition, a carrier can be added to carry metal oxides, improve the dispersion of metal oxides, make them evenly distributed on the coating surface, and fully expose their catalytic active sites to the air. Under low-temperature heat source conditions of 100°C-300°C, the oil stains can undergo catalytic oxidation reactions, prompting the rapid degradation of the oil stains into carbon dioxide and water. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0031] Figure 1 1 is a schematic diagram of the structure of a thermal catalytic functional coating material prepared in one embodiment of the present invention, wherein 1 is a variable valence metal oxide and a carrier; 2 is a binder; and 3 is a substrate.
[0032] Figure 2Schematic diagram of the structure of a thermal catalytic functional coating prepared in one embodiment of the present invention, wherein 4 is a metal oxide; 5 is a support; and 2 is a binder.
[0033] Figure 3 This is a surface microscopic FESEM morphology image of the thermal catalytic functional coating material prepared in Example 1 of the present invention.
[0034] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0035] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] In the present invention, descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0038] The present invention provides a thermal catalytic functional coating material, which can undergo a catalytic reaction under low-temperature heat source conditions of 100°C-300°C. The heat generated by the heating part of the cooking utensils during cooking can be used to directly catalytically oxidize and degrade the oil stains splashed onto the surface of the thermal catalytic functional coating, thereby avoiding the accumulation of oil stains. No additional consumption is required, and the oil stains can be degraded during the cooking process, ensuring that there is no grease deposition and residue in the cavity after cooking, avoiding the difficulty of cooking scenes in which the cavity is difficult to clean, and truly realizing the long-term surface self-cleaning function of the cooking utensils. For example, the heat generated by the heating module during the cooking process of the air fryer is used to directly catalytically oxidize and degrade the oil stains splashed onto the surface of the reflector coated with the thermal catalytic functional coating, thereby avoiding the accumulation of oil stains and making it easier to clean. It can be understood that 100°C-300°C refers to the temperature at which the thermal catalytic functional coating material of the present invention begins to undergo a catalytic reaction. Under the above temperature conditions, the conversion rate of the reactants undergoing catalytic oxidation reactions can reach 50% or more.
[0039] The thermal catalytic functional coating material of the present invention includes a catalyst and a binder, wherein the catalyst includes a metal oxide, and the metal oxide includes a variable-valence metal element. The variable-valence metal element can give the thermal catalytic functional coating material a stronger thermal catalytic function. When prepared into a coating, a large number of catalytic active sites can be exposed. Under the condition of a relatively low temperature heat source of 100°C-300°C, valence changes and electron transfer can occur, catalytic activity can be stimulated, and the catalytic function of promoting the oxidative degradation of oil pollution can be achieved.
[0040] In some embodiments, the variable-valence metal element includes at least one of Ce, Cu, Co, Fe, La, Mn and Ni. The above variable-valence metal elements have strong catalytic activity, good thermal catalytic effect, are green and environmentally friendly, and are not likely to pose a threat to people's health.
[0041] In some embodiments, the metal oxide includes CeO 2 ,CuO,CoO,Co 3 O 4 , Fe 2 O 3 , Fe 3 O 4 、MnO 2 , Mn 2 O 3 , Mn 3 O 4 、NiO、LaMn x Co 1-x O 3 ,CuFe 2 O 4 、CuMn 2 O 4 , Cu 1.5 Mn1.5 O 4 At least one of the above. The metal elements in the metal oxides are multivalent elements with strong catalytic activity, which can make the thermal catalytic functional coating material have catalytic activity at 100°C-300°C, promote the catalytic oxidation reaction of hydrocarbons in the oil, and achieve the purpose of oxidizing and degrading the oil to generate carbon dioxide and water during the cooking process.
[0042] In some embodiments, the catalytic temperature of the thermal catalytic functional coating material of the present invention is between 100°C and 300°C, and can be 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 175°C, 180°C, 190°C, 200°C, 220°C, 250°C, 300°C, etc. The coating material with thermal catalytic performance can directly catalyze and oxidize the oil stains adhering to the coating material using the heat generated by the heating module of the cooking utensil, thereby avoiding the accumulation of oil stains and realizing the long-term self-cleaning function of the cooking utensil. In particular, for appliances such as air fryers with compact structural design and closed space, it is very easy to form cleaning dead corners inside the cooking cavity. The coating material of the present invention can catalyze and degrade the oil stains during the cooking process, which can solve many problems caused by the difficulty of daily cleaning and reduce the growth of bacteria and carcinogenic risks on the surface of cooking utensils.
[0043] In some embodiments, the average particle size of the metal oxide is in the range of 2nm-2μm. Specifically, the average particle size of the metal oxide can be any value in the range of 2nm-2μm, such as 2nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1μm, 1.2μm, 1.5μm, 1.8μm, 1.9μm, 2μm, etc. The average particle size of the above metal oxide is at the micro-nano level, has a large specific surface area, can expose more catalytic active sites, is added to the coating material, and then the coating material is applied to the surface of the cooking utensil to form a coating, so that the catalytic active sites of the metal oxide are exposed to the air, thereby better promoting the catalytic oxidation reaction of oil stains.
[0044] In some embodiments, the binder of the present invention is an inorganic binder and / or an organic binder having high temperature resistance, including γ-Al 2 O 3 , SiO 2, at least one of polyethersulfone and polyamideimide. The above types of binders have good adhesion, and a small amount of addition can also achieve good adhesion effect, thereby increasing the proportion of metal oxides in the coating material, exposing a large amount of metal oxides on the coating surface, and achieving better catalytic oxidation degradation effect.
[0045] In addition, the above binders and metal oxides have good compatibility and are not likely to cause local accumulation of metal oxides, which is conducive to the uniform dispersion of metal oxides on the surface of the coating and exerting an efficient catalytic oxidation degradation effect.
[0046] In some embodiments, the thermo-catalytic functional coating material includes 10%-90% of metal oxide by weight. In other embodiments, the thermo-catalytic functional coating material includes 30%-80% of metal oxide.
[0047] In some embodiments, the thermocatalytic functional coating material includes 5%-70% of a binder by weight; in other embodiments, the thermocatalytic functional coating material includes 10%-50% of a binder.
[0048] Specifically, calculated by mass percentage, the content of metal oxide in the thermal catalytic functional coating material can be any value in the range of 10%-90%, such as 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, etc.; the content of binder can be any value in the range of 5%-70%, such as 5%.
[0049] If the binder content is too much, it is easy to cover and wrap the metal oxide, making it difficult to expose the catalytic active sites of the metal oxide to the air, which will weaken the catalytic oxidation degradation effect on oil stains; if the metal oxide content is too much and the binder content is too little, it is easy to cause the metal oxide to agglomerate and accumulate, and the adhesion is insufficient. When forming a coating, the metal oxide is difficult to fix on the surface of the cooking utensil, and then it is difficult to exert the best catalytic effect of the metal oxide for a long time. Under the above content range conditions, the metal oxide can be firmly fixed on the surface of the cooking utensil, exposing more catalytic active sites, improving the catalytic oxidation degradation efficiency of oil stains, and achieving a long-term surface self-cleaning effect of the cooking utensil.
[0050] In some embodiments, the thermo-catalytic functional coating material of the present invention also includes a load. Calculated by mass, the content of the load in the thermo-catalytic functional coating material is less than or equal to 80%. For example, it can be 80%, 85%, 70%, 60%, 50%, 40%, 30%, 20%, 10%, 5%, 4%, 3%, 2%, 1%, 0.5%, 0.1%, etc., a content below 80%.
[0051] In some embodiments, the average particle size range of the carrier is 10nm-10μm, for example, it can be 10nm, 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm or 10μm, etc., any value within the range of 10nm-10μm. At this time, the carrier has better dispersibility and a larger specific surface area, and can carry more metal oxides, helping the metal oxides with poor self-dispersibility to be evenly distributed on the surface of the coating, exposed to the air, and under thermal conditions, to better achieve catalytic oxidation degradation of oil stains.
[0052] In some embodiments, the loading material includes γ-Al 2 O 3 、SiO 2 、TiO 2 、ZrO 2 , molecular sieves, the molecular sieves include at least one of BETA5 molecular sieve, USY5 molecular sieve, and ZSM-5 molecular sieve. The above loads have a good specific surface area, can load a large amount of metal oxides, help the metal oxides to be evenly dispersed on the surface of the coating, so that the catalytic active sites on the surface of the metal oxides are exposed to the air in large quantities, and play a good catalytic activity under the conditions of 100-300 ° C. In the daily cooking process, the oil splashed onto the surface of the coating directly contacts the active sites on the surface of the metal oxides. Under the heating conditions of the heating module, the hydrocarbons in the oil can be promoted to undergo catalytic oxidation reactions under the action of oxygen in the air, and the oil is eventually degraded into carbon dioxide and water, achieving the purpose of self-cleaning the surface of the cooking utensils.
[0053] The present invention is not limited to the preparation method of the thermocatalytic functional coating material as described above. In some embodiments, the metal oxide, binder and other raw materials such as a carrier can be mixed evenly under stirring conditions to obtain the thermocatalytic functional coating material of the present invention.
[0054] In addition, the present invention also provides a thermo-catalytic functional coating, which includes the thermo-catalytic functional coating material of the present invention as described above.
[0055] The thermal catalytic functional coating of the present invention can expose the catalytic active sites of the metal oxide to the air. During the cooking process at a relatively low temperature of 100°C-300°C, it promotes the catalytic oxidation reaction of hydrocarbons in the oil stains under the action of oxygen in the air, and eventually degrades them into carbon dioxide and water, thereby achieving the purpose of self-cleaning the surface of the cooking utensil.
[0056] The thermo-catalytic functional coating prepared by the thermo-catalytic functional coating material of the present invention has an atomic percentage of variable-valence metal elements on the surface of the thermo-catalytic functional coating that is not less than 50% of the total atomic percentage of the variable-valence metal elements in the thermo-catalytic functional coating, and is exposed to the air. It can be understood that the atomic percentage of the variable-valence metal elements on the surface of the coating tested by X-ray photoelectron spectroscopy (XPS) is not less than 50% of the total atomic percentage of the variable-valence metal elements in the coating measured by inductively coupled plasma spectroscopy (ICP), that is, calculated by atomic percentage, more than 50% of the variable-valence metal elements in the coating are located on the surface of the coating and exposed to the air. By controlling the content of the variable-valence metal elements on the surface of the coating exposed to the air as described above, a large number of catalytic active sites in the metal oxide are in direct contact with the oil stain, which can enhance the catalytic oxidation degradation effect on the oil stain.
[0057] This embodiment does not limit the method of applying the thermo-catalytic functional coating to the surface of the cooking utensil to form a thermo-catalytic functional coating. In some embodiments, the above thermo-catalytic functional material is sprayed on the surface of the heating module of the cooking utensil and any inner surface in the cooking cavity to form a thermo-catalytic functional coating. The heating module provides a temperature environment of 100°C-300°C, which provides catalytic conditions for the catalytic effect of the thermo-catalytic functional coating, so that it exhibits better catalytic activity during the oxidation process of oil stains.
[0058] In addition, the present invention also provides a cooking utensil having a heating module, which can provide a catalytic temperature of 100° C.-300° C. for the thermal catalytic functional coating material, so that it exhibits better catalytic activity.
[0059] The present invention does not limit the types of cooking utensils. In some embodiments, including electric pressure cookers, frying machines, automatic cooking machines, air fryers or electric baking pans, the heat generated by the heating modules in the above cooking utensils directly catalyzes and oxidizes the oil stains splashed onto the surface of the utensils coated with the thermal catalytic functional coating, thereby degrading the oil stains during the cooking process, effectively avoiding the accumulation of oil stains and truly realizing the long-term surface self-cleaning function of the cooking utensils.
[0060] In some embodiments of the present application, in the thermal catalytic functional coating material, the variable valence metal elements are Co and Mn; and / or, in the coating, the surface atomic percentage of the variable valence elements measured by XPS is 10%-30%, and the total atomic percentage of the variable valence elements measured by ICP is 20%-50%; and / or, the variable valence metal oxide Co 3 O 4 and MnO 2 The average particle size is 10-50nm; and / or the support is SiO 2 , the average particle size is 2μm~5μm, and the mass percentage in the coating material is 20~60%; and / or the binder is PES, and the mass percentage is 20%-50%; it can meet the catalytic temperature in the range of 100℃-220℃, realize synchronous self-cleaning during the cooking process, and achieve the effect of low-temperature catalytic oil stains.
[0061] In some embodiments, the cooking appliance is an air fryer, and the thermocatalytic functional coating material is coated on the surface of the heating module of the air fryer and the inner cavity surface near the heating module to form a thermocatalytic functional coating.
[0062] In some embodiments, the heating module is a disc-shaped metal heating tube, which can make the thermal catalytic functional coating be heated more evenly.
[0063] When the air fryer is working, the metal oxides in the thermal catalytic functional coating are exposed to the air, and the catalytic active sites are in direct contact with the oil. As long as the temperature reaches 100℃-300℃, the catalytic activity of the thermal catalytic functional coating can be stimulated. Under aerobic conditions, the hydrocarbons in the oil are promoted to undergo catalytic oxidation reaction with oxygen. During the cooking process, the oil formed by volatile oil smoke can be degraded into carbon dioxide and water, avoiding the accumulation of oil and truly realizing the long-term surface self-cleaning function of the air fryer.
[0064] The thermal catalytic functional coating at least covers the top wall of the receiving chamber of the air fryer in this embodiment. In the air fryer, the food is generally arranged near the bottom of the receiving chamber. Based on the cooking structure of the air fryer, the cooking medium in the receiving chamber, that is, the hot air flow, is driven to circulate rapidly by the operation of the fan. In one embodiment, the fan is located close to the top wall of the receiving chamber, so the negative pressure area formed by the operation of the fan causes the cooking medium carrying oil fume / grease pollutants to contact the top wall position first, thereby causing the top wall to be most prone to accumulation of oil fume / grease pollutants. In this embodiment, a thermal catalytic functional coating is arranged on the top wall of the receiving chamber to catalytically degrade the oil fume / grease pollutants passing near the top wall. The catalytic efficiency is high, which is conducive to keeping the inner wall of the receiving chamber clean.
[0065] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following specific embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0066] Examples 1 to 10
[0067] The raw materials are weighed according to the formula in Table 1, and then the raw materials are evenly mixed to obtain a thermal catalytic functional coating material.
[0068] Comparative Example 1
[0069] The raw materials are weighed according to the formula in Table 1, and then the raw materials are evenly mixed to obtain a thermal catalytic functional coating material. See Table 1 for details.
[0070] Table 1 Formula of thermal catalytic functional coating materials in Examples and Comparative Examples
[0071]
[0072] Note: “ / ” in Table 1 means no addition.
[0073] Performance Test 1
[0074] The thermal catalytic functional coating material obtained in Example 1 was characterized by a field emission scanning electron microscope, and the following results were obtained: Figure 3 The surface microscopic FESEM morphology shown is Figure 3 It can be seen that:
[0075] ① The brightest contrast is Co 3 O 4 Variable valence metal oxide nanoparticles,
[0076] ② The contrast is in the middle for SiO 2 Load,
[0077] ③The darkest contrast is PES binder;
[0078] Co 3 O 4 Nanoparticles are evenly distributed on SiO 2 The surface of the load is fixed by the PES binder to form a thermal catalytic functional coating.
[0079] Performance Test 2
[0080] The products in the embodiment and the comparative example were sprayed on the surface of a pure aluminum plate as a substrate to form a coating with a thickness of 500 μm. Figure 1 and Figure 2 The load is loaded with metal oxides and is fixed on the surface of the substrate under the bonding action of the adhesive, and the metal oxides are exposed to the air in large quantities.
[0081] XPS was used to test the atomic percentage of the variable valence metal elements on the surfaces of the above coatings, and ICP was used to analyze the variable valence metal elements in the coatings to obtain the total atomic percentage of the variable valence metal elements. Then, the ratio of the atomic percentage of the variable valence metal elements on the surfaces of the above coatings was calculated. The results are shown in Table 2.
[0082] Performance Test 3
[0083] The products in the embodiment and the comparative example were sprayed on the surface of the pure aluminum plate to form a coating with a thickness of 500 μm.
[0084] The aluminum plates coated with the thermal catalytic functional coating were placed on constant temperature platforms at 100°C, 150°C, 200°C, and 300°C respectively, so that the surface temperature of the coating reached the set temperature of the constant temperature platform and remained constant. 50 μL of soybean cooking oil was dripped onto the surface of the coating using a pipette gun. According to the intensity of the reaction, it was divided into three levels: intense reaction, slow reaction, and no reaction. The specific corresponding instructions are as follows:
[0085] Violent reaction: When soybean oil is dropped onto the coating surface, visible smoke and sparks will occur within 1 minute;
[0086] Slow reaction: When soybean oil is dropped onto the coating surface, visible smoke or sparks will occur within 5 minutes;
[0087] No reaction: When soybean oil is dropped onto the coating surface, the oil droplets wet the coating surface in liquid state, and no obvious chemical reaction occurs.
[0088] The above test results are shown in Table 2.
[0089] Table 2 Performance comparison of thermal catalytic functional coatings of examples and comparative examples
[0090]
[0091]
[0092] As can be seen from Table 2, the thermal catalytic functional coating material prepared in the embodiment is prepared into a thermal catalytic functional coating, and the atomic percentage of the variable valence metal element on the surface of the coating is above 50%, which can fully expose the catalytic active sites to the air and promote the catalytic oxidation degradation of oil stains. Compared with the thermal catalysts in the prior art whose catalytic temperatures are generally above 200°C, the temperature at which the thermal catalytic functional coating material prepared in the present invention starts to undergo catalytic reaction drops below 200°C, and a catalytic reaction can occur under the conditions of 100°C-150°C, and a violent catalytic reaction occurs at 150°C-300°C, which has a good catalytic degradation effect on oil stains. In the daily cooking process, for example, in the cooking process of the air fryer, the generated oil stains can be decomposed to complete self-cleaning, without further processing to increase additional consumption, achieving low-temperature catalysis, and completing the purpose of self-cleaning while cooking, ensuring that there is no grease deposition and residue in the cavity after cooking, avoiding the user pain point of difficult cleaning inside the cavity, and truly realizing the long-term surface self-cleaning function of the cooking utensils.
[0093] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A thermal catalytic functional coating material, characterized in that: The thermal catalytic functional coating material includes a catalyst and a binder, wherein the catalyst includes a metal oxide, and the metal oxide includes a variable-valence metal element.
2. The thermal catalytic functional coating material according to claim 1, characterized in that: The variable-valence metal element includes at least one of Ce, Cu, Co, Fe, La, Mn and Ni.
3. The thermal catalytic functional coating material according to claim 1, characterized in that: The metal oxides include CeO2, CuO, CoO, Co3O4, Fe2O3, Fe3O4, MnO2, Mn2O3, Mn3O4, NiO, LaMn x Co 1-x O3, CuFe2O4, CuMn2O4, Cu 1.5 Mn 1.5 At least one of O4.
4. The thermal catalytic functional coating material according to claim 1, characterized in that: The catalytic temperature of the thermal catalytic functional coating material is between 100°C and 300°C.
5. The thermal catalytic functional coating material according to claim 1, characterized in that: The average particle size of the metal oxide is in the range of 2 nm to 2 μm.
6. The thermal catalytic functional coating material according to claim 1, characterized in that: The binder is an inorganic binder and / or an organic binder, including at least one of γ-Al2O3, SiO2, polyethersulfone and polyamideimide.
7. The thermal catalytic functional coating material according to claim 1, characterized in that: Calculated by mass percentage, the thermal catalytic functional coating material includes 10%-90% of the metal oxide; and / or, the thermal catalytic functional coating material includes 5%-70% of the binder.
8. The thermal catalytic functional coating material according to claim 7, characterized in that: Calculated by mass percentage, the thermal catalytic functional coating material includes 30%-80% of the metal oxide; and / or, the thermal catalytic functional coating material includes 10%-50% of the binder.
9. The thermal catalytic functional coating material according to claim 1, characterized in that: Calculated by mass percentage, the thermal catalytic functional coating material also includes less than or equal to 80% of a load.
10. The thermal catalytic functional coating material according to claim 9, characterized in that: The load is a micro-nano particle load with an average particle size ranging from 10 nm to 10 μm.
11. The thermal catalytic functional coating material according to claim 9, characterized in that: The load includes at least one of γ-Al2O3, SiO2, TiO2, ZrO2 and molecular sieve.
12. The thermal catalytic functional coating material according to claim 11, characterized in that: The molecular sieve includes at least one of BETA molecular sieve, USY molecular sieve and ZSM-5 molecular sieve.
13. A thermal catalytic functional coating, characterized in that: The thermocatalytic functional coating comprises the thermocatalytic functional coating material according to any one of claims 1 to 12.
14. The thermocatalytic functional coating according to claim 13, characterized in that: The atomic percentage content of the variable-valence metal element on the surface of the thermal catalytic functional coating is not less than 50% of the overall atomic percentage content of the variable-valence metal element in the thermal catalytic functional coating and is exposed to the air.
15. The thermocatalytic functional coating according to claim 13, characterized in that: The thickness of the thermal catalytic functional coating ranges from 20 μm to 2 mm.
16. A cooking utensil, characterized in that: The cooking utensil comprises the thermocatalytic functional coating according to any one of claims 13 to 15.
17. The cooking appliance according to claim 16, characterized in that The cooking appliance includes an electric pressure cooker, a frying pan, an automatic cooking machine, an air fryer or an electric baking pan.
18. The cooking appliance according to claim 16, characterized in that The cooking utensil has a heating module, and the thermal catalytic functional coating is coated on the surface of the heating module and / or any inner surface in the cooking cavity.
19. The cooking appliance according to claim 18, characterized in that The cooking utensil is an air fryer, and the thermal catalytic functional coating is coated on the surface of a heating module of the air fryer and / or any inner surface in a cooking cavity.
20. The cooking appliance according to claim 19, characterized in that The heating module of the air fryer is a disc-shaped metal heating tube.
Citation Information
Patent Citations
Coating as well as preparation method and application thereof
CN115926617A
Cooker
JP2001082747A
Catalyst-coated filter in which activity of catalyst is increased by adding lithium cocatalyst
WO2017111350A1