Anti-corona paint for high-altitude large-scale hydroelectric generating set equipment and preparation method of anti-corona paint
Through the combination of modified silica powder and epoxy adhesive, anti-corona paint for large hydropower units is prepared, which solves the problem of corona discharge in high-altitude environments and significantly improves the service life and safety of the equipment.
Patent Information
- Application Number
- CN202310914729.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-25
- Publication Date
- 2024-10-18
AI Technical Summary
Existing anti-corona paint cannot effectively solve the corona discharge problem caused by low air pressure and air density in high-altitude large-scale hydropower equipment, resulting in corona discharge in the generator stator winding, thereby reducing service life and safe operation.
Anti-corona paint is prepared using epoxy adhesive and modified silica powder. The specific surface area of the silica powder is increased through surface modification treatment to improve dispersion, and 0.5 to 1.5wt% micron SiO2 or nanometer SiO2 is added. Into the epoxy adhesive, an anti-corona paint is formed, filling the gaps in the winding structure and surface burrs, improving the potential distribution and inhibiting the generation of corona.
It effectively reduces the average field strength and maximum field strength distribution of the stator bars and windings, inhibits the generation and development of corona, ensures the long-term safe and stable operation of large hydropower units, and significantly improves the anti-corona effect.
Smart Images

Figure CN118791941A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-corona of large generator windings, and in particular relates to an anti-corona paint for large-scale hydropower unit equipment at high altitudes and a preparation method thereof. Background Art
[0002] Corona is a local discharge phenomenon, often accompanied by sound, light, and heat signals. Local free discharge with blue fluorescence often appears in high-voltage stator windings, which is called winding corona. Common locations where corona appears at the winding end include: 1) where the wire rod exits the notch; 2) between the wire rods of different phases at the end; 3) where there are sharp corners and burrs on the surface of the winding end; 4) where the wire rod end contacts the end hoop, binding rope, pad, or the unevenness of the wrapping. In the air, the corona effect can produce ozone (O 3 ) and nitrogen oxides (NO, NO 2 ), they can combine with moisture to form harmful acidic substances, corroding the insulation layer. Corona can also cause local heating of the insulation layer, accelerate the aging of the insulation layer, and even quickly destroy the insulation layer in severe cases.
[0003] When large generators are in operation, they are affected by multiple physical fields such as electricity, heat, environmental stress and mechanical stress, which will cause corona discharge in the weak links of the stator winding insulation (such as the winding slots and end binding areas where the electric field distribution is extremely uneven). The small gaps between the insulating fixed structural parts (pads, felts, etc.) and between the structural parts and the stator wire bars, as well as the surface burrs, accelerate the occurrence and development of corona discharge. Long-term corona discharge will cause electrical corrosion, insulation aging, thermal cracking and other phenomena in the insulation layer, leading to insulation failure, reducing the service life of the generator, and threatening the safe operation of the motor.
[0004] Chinese patent CN2013101152079 discloses a nano anti-corona paint, the ingredients of which include epoxy resin, organic montmorillonite, toluene or xylene, silicon carbide powder, etc. The heat resistance grade of the anti-corona paint reaches F grade (155°C), and the resistivity after curing is 1×10 9 ~1×10 12 Ω. However, the anti-corona paint still cannot meet the demand under extreme weather conditions such as Northeast or Northwest my country. Chinese patent CN201810753848X discloses a high-resistance anti-corona paint for high-voltage motor coils, whose ingredients include epoxy resin, honeycomb silica nanotubes, polyamide resin, toluene or xylene, etc. The honeycomb silica nanotubes added to this high-resistance anti-corona paint have very good elasticity during slight shrinkage and expansion, so the high and low temperature impact performance of the high-resistance anti-corona paint layer can be significantly improved. However, this high-resistance anti-corona paint cannot solve the problem of corona discharge of the stator windings of large-capacity hydro-turbine generators caused by low air pressure and air density, which leads to a decrease in the surface discharge voltage of the stator bars and stator windings of large-capacity hydro-turbine generators.
[0005] In summary, the present invention proposes an anti-corona paint for large-scale hydropower equipment at high altitudes to alleviate the problems existing in the prior art. Summary of the invention
[0006] In view of this, the object of the present invention is to provide a novel anti-corona paint and a preparation method thereof, and the specific technical scheme is as follows.
[0007] The invention discloses an anti-corona paint, which is a discharge corona filling adhesive for large hydropower unit equipment, and comprises an epoxy adhesive and silicon dioxide powder; the epoxy adhesive comprises component A, component B and a diluent; the component A is a bisphenol A type matrix, the component B adhesive curing agent comprises polyamide or phenolic amine; the usage ratio of the component A to the component B is 3:1-2; the usage of the diluent is 6% of the component A; the silicon dioxide powder comprises micron SiO2 with an addition amount of 0.5-1.5wt%; the epoxy adhesive comprises component A, component B and a diluent; the epoxy adhesive comprises component A, component B and a diluent; the epoxy adhesive comprises component A, component B and a diluent; the epoxy adhesive comprises component A, component B and a diluent; the epoxy adhesive comprises component A, component B and a diluent; the epoxy adhesive comprises component A, component B and a diluent; the epoxy adhesive comprises component A, component B and a diluent; the epoxy adhesive comprises component A, component B and a diluent; the epoxy adhesive comprises component A, component B and a diluent; the epoxy adhesive comprises component A, component B and a diluent; the epoxy adhesive comprises component B, component B and a diluent; the epoxy adhesive comprises component A ... 2 Or adding 0.5-1.5wt% nano-SiO 2 , the amount added is based on the weight of the epoxy adhesive.
[0008] Furthermore, the usage ratio of component A to component B of the epoxy adhesive is 3:0.87.
[0009] Furthermore, the silicon dioxide powder is a micron SiO 2 Or adding 1wt% nano-SiO 2 .
[0010] Furthermore, the micron SiO 2 The particle size is 2 to 5 μm.
[0011] Furthermore, the nano-SiO 2 The particle size is 10 to 30 nm.
[0012] The preparation method of the above-mentioned anti-corona paint comprises the following steps:
[0013] 1) Surface modification of silica powder, the specific surface area of the modified silica powder is 100-120m 2 / g;
[0014] 2) Component A of the epoxy adhesive and the modified silicon dioxide powder are uniformly mixed, and then component B and a diluent are added to prepare the anti-corona paint.
[0015] Further, the specific operation steps of step 1) are: taking KH550 and deionized water in a ratio of 1:1, adding anhydrous ethanol, and magnetically stirring at a speed of 500 r / min for 30 minutes to obtain a KH550 hydrolyzate; taking SiO 2After mixing with anhydrous ethanol, KH550 hydrolyzate was added and ultrasonically shaken for 30 min. The mixed solution was placed in a 90°C water bath for 6 h, and the solution was magnetically stirred at a speed of 600 r / min to make SiO 2 After the reaction, the mixed solution was centrifuged, washed and dried to obtain the modified SiO 2 particle.
[0016] In the present invention, SiO 2 The purpose of modifying the particle surface is to make it more dispersible.
[0017] Preferably, the SiO 2 Micron SiO 2 , particle size is 2 to 5 μm.
[0018] Further, the specific operation steps of step 2) are: mixing component A of the epoxy adhesive with the modified SiO 2 After the powders are mixed, they are magnetically stirred at 60° C. for 1 hour, and then ultrasonically shaken for 1 hour to obtain a first mixed solution; component B and a diluent are added to the first mixed solution, and magnetically stirred at room temperature for 10 minutes to obtain a second mixed solution; the second mixed solution is placed in a vacuum drying oven, and after vacuuming to remove bubbles at room temperature, a discharge corona filling glue is obtained.
[0019] Preferably, the usage ratio of component A to component B of the epoxy adhesive is 3:0.87.
[0020] The anti-corona paint prepared by the method of the invention is used on the stator wire rods and stator winding ends of a hydroelectric generator set.
[0021] Beneficial technical effects
[0022] The method of the present invention first modifies the surface of silicon dioxide powder, and the specific surface area is increased after the modification, so that it has better dispersibility in the matrix glue. Compared with the prior art, the anti-corona paint provided by the present invention has a simple component structure, good dispersibility, and a simple and easy-to-operate preparation method. The anti-corona paint is applied to the ends of the stator wire rods and stator windings of the hydropower unit, and can fill and cover the gaps and surface burrs of the winding structure at the end of the hydropower unit, improve the potential distribution on the winding surface, reduce the average field strength and maximum field strength distribution of the stator wire rods and the winding air gap, inhibit the generation and development of corona, and ensure the long-term safe and stable operation of large hydropower units. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, each element or part is not necessarily drawn according to the actual scale. Obviously, the drawings described below are some embodiments of the present invention. For those of ordinary skill in the art, other drawings can also be obtained based on these drawings without paying creative labor.
[0024] Figure 1 The micron SiO provided by the present invention 2 SEM and EDS images of the filling glue;
[0025] Figure 2 The micron SiO provided by the present invention 2 Thermal conductivity curve of the filling glue;
[0026] Figure 3 The micron SiO provided by the present invention 2 A graph showing the dielectric constant and dielectric loss factor of the filler as a function of frequency;
[0027] Figure 4 The micron SiO provided by the present invention 2 Histogram of breakdown field strength data of the filling glue;
[0028] Figure 5 The nano-SiO 2 Plot of the dielectric constant and dissipation factor of the filler as a function of frequency. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0030] Herein "and / or" includes any and all combinations of one or more of the associated listed items.
[0031] Herein, "plurality" means two or more than two, ie, it includes two, three, four, five, etc.
[0032] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0033] As used in this specification, the term "about" typically means + / - 5% of the stated value, more typically + / - 4% of the stated value, more typically + / - 3% of the stated value, more typically + / - 2% of the stated value, even more typically + / - 1% of the stated value, and even more typically + / - 0.5% of the stated value.
[0034] In this specification, some embodiments may be disclosed in a format of being within a certain range. It should be understood that such description of "being within a certain range" is only for convenience and brevity, and should not be interpreted as a rigid limitation on the disclosed range. Therefore, the description of the range should be considered to have specifically disclosed all possible sub-ranges and independent numerical values within this range. For example, the range The description of should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6 etc., as well as individual numbers within this range, for example, 1, 2, 3, 4, 5, and 6. The above rules apply regardless of the breadth of the range.
[0035] Example 1
[0036] raw material:
[0037] Epoxy adhesive: DECJ1403 room temperature curing epoxy adhesive, comprising component A, component B and diluent (the optimal ratio of component A to component B is 3:0.87). The diluent is phenyl glycidyl ether (690).
[0038] Nano-SiO 2 : Particle size 10-30nm, unmodified, produced by Shanghai McLean Biochemical Technology Co., Ltd.
[0039] Micron SiO 2 : Particle size 3μm, unmodified, produced by Zhejiang Manli Nano Technology Co., Ltd.
[0040] Silane coupling agent KH550: produced by Nanjing Chuangshi Chemical Additives Co., Ltd.
[0041] 1. Sample preparation method
[0042] 1. Filler surface modification: Use chemical method to modify micron SiO 2 Surface modification was performed to enhance the bonding force between micron particles and the matrix resin (DECJ, i.e., resin without silica particles) and improve the dispersibility of particles in the matrix resin. First, 0.5 ml of KH550 and deionized water were mixed at a ratio of 1:1, and then 49 ml of anhydrous ethanol was added. The KH550 hydrolyzate was obtained after magnetic stirring at a speed of 500 r / min for 30 min. 5 g of micron SiO 2 After mixing with 200 ml of anhydrous ethanol, KH550 hydrolyzate was added and ultrasonically shaken for 30 min. The mixed solution was placed in a water bath at 90 °C for 6 h, and the solution was magnetically stirred at a speed of 600 r / min to make SiO 2 After the reaction, the mixed solution is centrifuged, washed and dried to obtain the modified micron SiO 2 particle.
[0043] Modified SiO 2 The particle surface area is 100~120m 2 / g.
[0044] 2. Preparation of anti-corona paint (also known as filling glue): Mix a certain proportion of epoxy adhesive component A with modified silica powder, stir magnetically for 1 hour at 60°C, and then ultrasonically vibrate for 1 hour to obtain a first mixed solution; add component B and diluent to the first mixed solution, stir magnetically for 10 minutes at room temperature to obtain a second mixed solution; put the second mixed solution into a vacuum drying oven, evacuate at room temperature to remove bubbles, pour into a mold, and cure at room temperature for 24 hours to obtain a sample.
[0045] 2. Micron SiO 2 Study on the performance of anti-corona paint
[0046] 1. Micronized SiO before and after modification 2 The filling glue was prepared according to the addition amount of 0%, 0.5%, 1.0%, and 1.5%, and the filling glue was obtained after curing. The microscopic morphology of the obtained filling glue was observed by SEM. Figure 1 As shown, the modified micron SiO 2 The dispersion in the matrix glue is good, and no obvious agglomeration is observed. EDS was used to analyze the Si element of the sample cross section to characterize the micron SiO 2 The distribution of fillers in the matrix glue. The results show that the points where Si elements are concentrated in the EDS image are consistent with the micron SiO observed in the corresponding SEM image. 2 The filler position is roughly the same, and as the micron SiO 2 The more the filler is added, the more points the Si element concentrates.
[0047] 2. Modified micron SiO 2 The thermal conductivity of the filling glue sample was tested at 50°C. The results are as follows Figure 2 As shown, when micron SiO 2 When the content is 1wt%, the thermal conductivity of the micron-filled glue is the highest, 0.014W / (m·k) higher than that of the matrix resin; 2 When the content is 0.5wt%, the thermal conductivity of the micron-filled glue is the lowest, which is 0.011W / (m·k) lower than that of the matrix resin.
[0048] 3. Modified micron SiO 2 The dielectric constant and dielectric loss factor of the filled resin sample were tested, and the results are shown in Figure 3 As shown. Figure 3 , it can be concluded that the modified micron SiO 2 The dielectric loss of the filled resin sample at the power frequency (50Hz) and the comparison data with the matrix resin DECJ are shown in Table 1 below.
[0049] Table 1DECJ / modified micron SiO 2 Dielectric loss data table of filled resin at power frequency (50Hz)
[0050] The above experiments show that with the increase of micron SiO 2 As the content increases, the dielectric constant of the material gradually decreases. 2 To a certain extent, it can reduce the dielectric constant of the matrix resin. This may be because the micron SiO 2 As an insulating inorganic filler dispersed in the resin, it strengthens the internal structure of the matrix resin, restricts the orientation movement of polar groups, reduces the degree of EP surface polarization, and thus reduces the dielectric loss of the material.
[0051] 4. Modified micron SiO 2 The breakdown field strength of the filling glue sample was tested, and the results are shown in Figure 4 As shown. Figure 4 It can be seen that the three different SiO 2 The breakdown field strength of the added micron filler is higher than that of the base glue; when the micron SiO 2 When the content is 1wt%, the breakdown field strength of the micron-filled glue is the highest, which is 17.4kv / mm higher than that of the matrix glue. 2 With the increase of SiO content, the breakdown field strength of micron filler increases first and then decreases. The reason for this phenomenon may be that when the amount of SiO 2When added to the matrix colloid, due to the interface effect between the micron particles and the colloid, the binding ability of electrons is enhanced, which hinders the formation of conductive paths, thereby increasing the breakdown field strength; when SiO 2 When the content is 1.5wt%, due to the large number of micron particles, overlapping and uneven dispersion may occur in the matrix glue, reducing the SiO 2 The interfacial bonding force between the adhesive and the matrix causes the interface effect between the two to be weakened, thereby reducing the breakdown field strength.
[0052] Considering the test performance of the above micron filling glue, when the micron SiO 2 When the addition amount is 1wt%, the thermal conductivity and breakdown field strength of the material are the highest, and the dielectric loss is also reduced to a certain extent compared with the base glue. Therefore, the addition amount of 1wt% of micron SiO 2 The anti-corona filling adhesive is prepared by mixing with epoxy adhesive.
[0053] 3. Nano-SiO 2 Study on the performance of anti-corona paint
[0054] 1. Nano-SiO 2 The preparation methods were the same as those of micron SiO 2 After curing, the nano-filled glue is obtained. The dielectric constant and dielectric loss factor of the obtained nano-filled glue sample are tested. The results are shown in Figure 5 As shown. Figure 5 , it can be concluded that nano-SiO 2 The dielectric loss of the filling glue sample at the power frequency (50Hz) and the comparison data with the matrix resin DECJ are shown in Table 2 below.
[0055] Table 2. DECJ / Nano-SiO 2 Dielectric loss data table of filling glue at power frequency (50Hz)
[0056] The above experiments show that with the increase of nano-SiO 2 With the increase of content, the dielectric constant of the material shows a trend of first decreasing and then increasing, but overall, nano-SiO 2 The dielectric constant is higher than that of micron SiO 2 Relatively high.
[0057] Example 2
[0058] Preparation of micronized SiO 2 Anti-corona paint
[0059] (1) Preparation of micronized SiO 2Modified powder: 0.5 ml KH550 and deionized water were mixed in a ratio of 1:1, and then 49 ml anhydrous ethanol was added. The mixture was stirred magnetically at a speed of 500 r / min for 30 min to obtain KH550 hydrolyzate. 5 g micron SiO 2 After mixing with 200 ml of anhydrous ethanol, KH550 hydrolyzate was added and ultrasonically shaken for 30 min. The mixed solution was placed in a water bath at 90 °C for 6 h, and the solution was magnetically stirred at a speed of 600 r / min to make SiO 2 After the reaction, the mixed solution was centrifuged, washed and dried to obtain micron SiO 2 Modified powder;
[0060] (2) Epoxy adhesive component A and micronized SiO 2 After the modified powders were mixed, they were magnetically stirred at 60°C for 1 hour, and then subjected to ultrasonic vibration for 1 hour to obtain a first mixed solution; component B and a diluent were added to the first mixed solution, and magnetically stirred at room temperature for 10 minutes to obtain a second mixed solution; the second mixed solution was placed in a vacuum drying oven, and vacuumed to remove bubbles at room temperature to obtain micron SiO 2 Anti-corona paint; wherein the usage ratio of component A to component B of the epoxy adhesive is 3:0.87, micron SiO 2 The added amount of the modified powder is 1 wt % based on the weight of the epoxy adhesive.
[0061] Micron SiO 2 The room temperature curing time of the anti-corona paint is 24 hours and the heat resistance grade is F.
[0062] Example 3
[0063] Preparation of Nano-SiO 2 Anti-corona paint
[0064] The epoxy adhesive component A and nano-SiO 2 After the powders were mixed, they were magnetically stirred at 60°C for 1 hour, and then subjected to ultrasonic vibration for 1 hour to obtain a first mixed solution; component B and a diluent were added to the first mixed solution, and magnetically stirred at room temperature for 10 minutes to obtain a second mixed solution; the second mixed solution was placed in a vacuum drying oven, and vacuumed at room temperature to remove bubbles to obtain nano-SiO 2 Anti-corona paint; wherein the usage ratio of component A to component B of the epoxy adhesive is 3:0.87, nano-SiO 2 The powder was added in an amount of 1 wt % based on the weight of the epoxy adhesive.
[0065] Nano-SiO 2 The room temperature curing time of the anti-corona paint is 24 hours and the heat resistance grade is F.
[0066] Example 4
[0067] The stator winding of a high-head large-capacity hydropower unit with an insulation level of 18kV and an anti-corona level of 20kV was treated with anti-corona treatment, and the corona inception voltage at the winding end before and after the anti-corona treatment was tested. The results are shown in Table 4 below.
[0068] The anti-corona treatment method is: apply the filling glue to the entire end of the stator bar and stator winding of the finished product of the hydro-turbine generator with a brush, apply it one or two times, and inject the filling glue into the gaps that are difficult to be applied by the brush with a syringe. The thickness of the applied filling glue is controlled to be about 1mm, and it is cured at room temperature for 24 hours. The filling glue uses the micron SiO 2 Filling glue or nano-SiO obtained in Example 3 2 Filling glue.
[0069] Table 4 Changes in winding corona initiation voltage of hydro-turbine generator before and after anti-corona treatment UV photon number Corona inception voltage / kV Anti-corona pre-treatment 17280 22 Example 2 After anti-corona glue treatment 10160 26 Example 3 After anti-corona glue treatment 17200 24
[0070] Experimental conclusion: The number of ultraviolet photons is used to judge corona discharge, and the voltage applied to the winding when the number of ultraviolet photons exceeds 1500 is the corona initiation voltage. As can be seen from Table 4, compared with the anti-corona treatment, whether it is the use of micron SiO 2 Filling glue or nano-SiO 2 The corona inception voltage of the winding after the filling glue coating is significantly improved. 2 The anti-corona effect of the filling glue is better than that of nano-SiO 2 Filling glue.
[0071] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.
Claims
1. An anti-corona paint, characterized in that: The anti-corona paint is an anti-corona filling adhesive used for large hydropower unit equipment, including epoxy adhesive and silicon dioxide powder; the epoxy adhesive includes component A, component B and a diluent, and the component A is a bisphenol A type matrix; The component B is a curing agent, including polyamide or phenolic amine; the dosage ratio of the component A to the component B is 3:1-2; the dosage of the diluent is 6% of the component A; the silicon dioxide powder includes micron SiO2 with an addition amount of 0.5-1.5wt% or nano SiO2 with an addition amount of 0.5-1.5wt%, and the addition amount is calculated based on the weight of the epoxy adhesive.
2. The anti-corona paint according to claim 1, characterized in that The usage ratio of component A to component B of the epoxy adhesive is 3:0.
87.
3. The anti-corona paint according to claim 1, characterized in that The silicon dioxide powder is micron SiO2 with an addition amount of 1wt% or nanometer SiO2 with an addition amount of 1wt%.
4. The anti-corona paint according to claim 1, characterized in that The particle size of the micron SiO2 is 2 to 5 μm.
5. The anti-corona paint according to claim 1, characterized in that The particle size of the nano-SiO2 is 10-30 nm.
6. The method for preparing the anti-corona paint according to claim 1, characterized in that: The following steps are involved: 1) Surface modification of silica powder, the specific surface area of the modified silica powder is 100-120m 2 / g; 2) Component A of the epoxy adhesive and the modified silicon dioxide powder are uniformly mixed, and then component B and a diluent are added to prepare the anti-corona paint.
7. The preparation method according to claim 6, characterized in that: The specific operation steps of step 1) are as follows: KH550 and deionized water are mixed in a ratio of 1:1, anhydrous ethanol is added, and the mixture is magnetically stirred at a speed of 500 r / min for 30 minutes to obtain a KH550 hydrolyzate; SiO2 and anhydrous ethanol are mixed, the KH550 hydrolyzate is added, and ultrasonic vibration is performed for 30 minutes; the mixed solution is placed in a 90°C water bath for modification for 6 hours, and the solution is magnetically stirred at a speed of 600 r / min to allow SiO2 and KH550 to fully react; the mixed solution after the full reaction is centrifuged, washed, and dried to obtain modified SiO2 particles.
8. The preparation method according to claim 7, characterized in that: The SiO2 is micron SiO2 with a particle size of 2 to 5 μm.
9. The preparation method according to claim 6, characterized in that: The specific operation steps of step 2) are as follows: after mixing component A of the epoxy adhesive with the modified SiO2 powder, magnetically stirring at 60°C for 1 hour, and then ultrasonically oscillating for 1 hour to obtain a first mixed solution; adding component B and a diluent to the first mixed solution, magnetically stirring at room temperature for 10 minutes to obtain a second mixed solution; placing the second mixed solution in a vacuum drying oven, and vacuuming at room temperature to remove bubbles to obtain an anti-corona filling glue.
10. The preparation method according to claim 9, characterized in that: The usage ratio of component A to component B of the epoxy adhesive is 3:0.87.
Citation Information
Patent Citations
Preparation method of nano-composite nonlinear anti-corona paint
CN113583504A
Corona resistant electric insulating wire
JP2009146753A