High-density coating aluminum plate and preparation method thereof
By using high-density coated aluminum panels on the curtain wall panels, sandblasting and spraying processes are used to form a coating containing n-butanol etherified melamine formaldehyde resin and water-based polyurethane, combined with an insulating inorganic mixture, which solves the problem of easy installation of curtain wall panels in chemical plants. The problem of contamination and lightning damage is improved, the resistance to electrical breakdown and corrosion is improved, and the service life is extended.
Patent Information
- Application Number
- CN202410804892.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Curtain wall panels on high-rise buildings inside chemical plants are easily affected by chemical smoke pollution and thunderstorms, resulting in shortened service life.
A high-density coated aluminum plate is used, and the surface of the alloy aluminum substrate is coated with a primer layer, a high-density coating and an outer protective layer in sequence. The high-density coating is composed of n-butanol etherified melamine formaldehyde resin, water-based polyurethane and It is composed of an insulating inorganic mixture containing phosphoric acid, magnesium oxide, aluminum hydroxide, boric acid and silicon oxide, and is formed into a dense coating through sandblasting roughening and spraying processes.
It improves the stain resistance and electric breakdown resistance of the aluminum plate, prevents aging discoloration and lightning strike damage caused by chemical smoke, and extends the service life.
Smart Images

Figure CN118791952A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy surface treatment, in particular to a high-density coated aluminum plate and a preparation method thereof. Background Art
[0002] Curtain wall panels are building exterior enclosure systems or decorative structures composed of surface materials and supporting structural systems. They are usually used for the exterior walls of large and high-rise buildings. Curtain wall panels are made of aluminum plates, and thus have the physical properties of aluminum, namely, they are light, flexible in design, and have strong earthquake resistance. According to the requirements of different use environments, curtain wall panels need to be produced in combination with the requirements of the environment and with aluminum plates using different processing techniques.
[0003] For example, the Chinese patent publication number is CN102848639B, which is an imitation stainless steel wire drawing coated aluminum plate and its manufacturing method. The imitation stainless steel coated aluminum plate of the present invention has a wire drawing layer, a first passivation layer and a top coating layer on the alloy aluminum substrate in sequence, and a second passivation layer and a back paint layer on the alloy aluminum substrate in sequence. The manufacturing method is to wire draw the alloy aluminum substrate, pre-treat degreasing, passivation, and then high-temperature baking after coating, so as to form the imitation stainless steel wire drawing coated aluminum plate of the present invention.
[0004] The curtain wall panels installed on high-rise buildings inside chemical plants are easily polluted by the chemical fumes generated by the chemical plants, causing the facades of the curtain wall panels to discolor and age. They are also easily affected by lightning strikes on rainy days, causing the curtain wall panels to age and be damaged, thereby shortening the service life of the curtain wall panels on high-rise buildings. Summary of the invention
[0005] The purpose of the present invention is to provide a high-density coated aluminum plate and a preparation method thereof, so as to solve the problem proposed in the above background technology that curtain wall panels installed on high-rise buildings inside chemical plants are easily affected by chemical smog pollution generated by the chemical plants and lightning strikes during thunderstorms, resulting in a shortened service life of the curtain wall panels on high-rise buildings.
[0006] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a high-density coated aluminum plate, comprising an alloy aluminum substrate, the surface of which is coated with a primer layer, a high-density coating, a top coating and an outer protective layer in sequence, and the coating components of the high-density coating include n-butanol etherified melamine formaldehyde resin, water-based polyurethane and an insulating inorganic mixture.
[0007] The present invention is further configured as follows: the coating components of the primer layer include acrylic acid and polyurethane.
[0008] The present invention is further configured as follows: the components of the insulating inorganic mixture include 26.1%-32.5% by mass of phosphoric acid, 4.2%-5.6% by mass of magnesium oxide, 7.21%-8.65% by mass of aluminum hydroxide, 0.25%-0.85% by mass of boric acid and 15.2%-17.3% by mass of silicon oxide and water.
[0009] A method for preparing a high-density coated aluminum plate comprises the following steps:
[0010] S1. Pre-treating the surface of the alloy aluminum substrate to be coated, sequentially performing water washing, acid washing, ethanol washing and pure water washing steps on the alloy aluminum substrate to obtain an aluminum plate with a clean surface and no oil, and then air-drying the aluminum plate;
[0011] S2, 3% to 8% by mass of n-butanol etherified melamine formaldehyde resin, 8% to 16% by mass of waterborne polyurethane, 45% to 60% by mass of insulating inorganic mixture and 15% to 25% by mass of stainless steel shot peening particles are fully mixed under stirring conditions to obtain a uniformly mixed liquid coating;
[0012] S3, sending the alloy aluminum substrate obtained in step S2 into a spray box, and performing a sandblasting roughening process on the alloy aluminum substrate, wherein the spray box sprays abrasives onto the surface of the alloy aluminum substrate through an air pump, so that dense pits are formed on the surface of the aluminum material, so that the subsequent liquid coating can adhere to the surface of the alloy aluminum substrate;
[0013] S4, performing a spraying process on the alloy aluminum substrate treated in step S1 to obtain a high-density coated aluminum plate;
[0014] S5. Send the high-density coated aluminum plate obtained in step S4 to a drying room for curing treatment to obtain a high-density coated aluminum plate with a stable surface coating.
[0015] The present invention is further configured as follows: according to the method for preparing a high-density coated aluminum plate according to claim 4, the pickling process in step S1 comprises the following steps:
[0016] S10, immersing the washed aluminum alloy substrate in a pickling tank for 5-8 minutes;
[0017] S11, taking the soaked alloy aluminum substrate out of the pickling tank, and sending it into a warm water tank for soaking and washing, the soaking and washing time is 3min-5min, the water temperature is 30-55°, and the reaction substances and residual acid generated during the pickling process are removed;
[0018] S12. Take the alloy aluminum substrate out of the warm water pool and put it into the cleaning box. Use water guns on both sides of the cleaning box to rinse the outer surface of the alloy aluminum substrate to ensure that residual substances are completely removed. Control the water temperature to avoid aging effects on the aluminum alloy plate. The temperature of the water sprayed from the water gun is 10°-20°.
[0019] The present invention is further configured as follows: according to the method for preparing a high-density coated aluminum plate according to claim 4, the ethanol washing process in step S1 comprises the following steps:
[0020] S20, sending the alloy aluminum substrate into an ethanol water washing tank for immersion treatment, wherein the ethanol concentration in the ethanol solution is 62.5%-71.25%, and the immersion time is 3min-5min;
[0021] S21. Send the alloy aluminum substrate washed with ethanol into a warm water pool for immersion washing. The immersion washing time is 2 min-3 min, and the water temperature is 20-45° to remove the ethanol solution attached to the surface of the aluminum plate during the ethanol washing process.
[0022] The present invention is further configured as follows: according to the method for preparing a high-density coated aluminum plate according to claim 4, the sandblasting roughening process in step S3 comprises the following steps:
[0023] S30, fixing the alloy aluminum substrate on the outside of the spray positioning frame;
[0024] S31, sending the abrasive into the sandblasting tank, starting the air pump, and blowing the abrasive in the sandblasting tank out through the spray gun to roughen the facade of the alloy aluminum substrate for 10-20 minutes;
[0025] S32. After the roughening treatment is completed, the fan is started to clean the surface of the alloy aluminum substrate and blow away the abrasive remaining on the surface of the alloy aluminum substrate.
[0026] The present invention is further configured as follows: the diameter of the stainless steel shot peening particles in step S2 is 200-280 μm.
[0027] The present invention is further configured as follows: the abrasive is G40 steel sand.
[0028] The present invention is further configured as follows: the spraying process in step S4 comprises the following steps:
[0029] S40, injecting the liquid paint obtained in step S2 into the paint bin of the spray box in step S3 to complete the loading operation;
[0030] S41, start the air pump, and the air pump sprays the liquid paint inside the paint tank out from the spray gun mouth;
[0031] S42, the spray gun performs periodic reciprocating motion on the surface of the alloy aluminum substrate, and the spraying time is 18min-22min.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The high-density coated aluminum plate produced by the present invention has a primer layer and a high-density coating on its surface to improve its anti-fouling and anti-electrical breakdown performance. Chemical fumes will not cause the high-density coated aluminum plate to age and discolor. The insulating inorganic mixture is composed of phosphoric acid, magnesium oxide aluminum hydroxide, boric acid and silicon oxide, so that the insulating inorganic mixture has good anti-electrical breakdown performance and corrosion resistance, thereby making the high-density coated aluminum plate have good anti-electrical breakdown performance and corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a schematic structural diagram of a high-density coated aluminum plate of the present invention;
[0035] Figure 2 This is a flow chart of a method for preparing a high-density coated aluminum plate according to the present invention;
[0036] Figure 3 This is a bar chart analysis of the breakdown voltage of a high-density coated aluminum plate of the present invention.
[0037] In the figure: 1. Alloy aluminum substrate; 11. Primer layer; 12. High-density coating; 13. Topcoat; 14. Outer protective layer. DETAILED DESCRIPTION
[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the implementation regulations described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Embodiment 1
[0040] A high-density coated aluminum plate comprises an alloy aluminum substrate 1, wherein a primer layer 11, a high-density coating layer 12, a top coating layer 13 and an outer protective layer 14 are sequentially coated on the surface of the alloy aluminum substrate 1, wherein the coating components of the high-density coating layer 12 comprise n-butanol etherified melamine formaldehyde resin, water-based polyurethane and an insulating inorganic mixture, the coating components of the primer layer 11 comprise acrylic acid and polyurethane, and the components of the insulating inorganic mixture comprise 26.1% by mass of phosphoric acid, 4.2% by mass of magnesium oxide, 7.21% by mass of aluminum hydroxide, 0.25% by mass of boric acid, 15.2% by mass of silicon oxide and 47.04% by mass of water.
[0041] A method for preparing a high-density coated aluminum plate comprises the following steps:
[0042] S1, sequentially subjecting the alloy aluminum substrate 1 to be processed and coated to water washing, pickling, ethanol washing and pure water washing steps to obtain an aluminum plate with a clean surface and no oil;
[0043] S10, immersing the washed aluminum alloy substrate 1 in a pickling tank for 5-8 minutes;
[0044] S11, taking the soaked alloy aluminum substrate 1 out of the pickling tank, and sending it into a warm water tank for soaking and washing, the soaking and washing time is 3min-5min, the water temperature is 30-55°, and the reaction substances and residual acid generated during the pickling process are removed;
[0045] S12, taking out the alloy aluminum substrate 1 from the warm water pool and sending it into the interior of the cleaning box, and using water guns on both sides of the interior of the cleaning box to rinse the outer surface of the alloy aluminum substrate 1 to ensure that the residual substances are completely removed, and controlling the water temperature to avoid aging effects on the aluminum alloy plate, and the temperature of the water sprayed by the water gun is 10°-20°;
[0046] S20, sending the alloy aluminum substrate 1 into an ethanol water washing tank for immersion treatment, wherein the ethanol concentration in the ethanol solution is 62.5%-71.25%, and the immersion time is 3min-5min;
[0047] S21. Send the alloy aluminum substrate 1 washed with ethanol into a warm water pool for immersion washing. The immersion washing time is 2 min-3 min, and the water temperature is 20-45° to remove the ethanol solution attached to the surface of the aluminum plate during the ethanol washing process.
[0048] S2, 3% to 8% by mass of n-butanol etherified melamine formaldehyde resin, 8% to 16% by mass of waterborne polyurethane, 45% to 60% by mass of insulating inorganic mixture and 15% to 25% by mass of stainless steel shot peening particles are fully mixed under stirring conditions to obtain a uniformly mixed liquid coating;
[0049] S3, performing a sandblasting roughening process on the alloy aluminum substrate 1 obtained in step S2;
[0050] S30, fixing the alloy aluminum substrate 1 on the outside of the spraying positioning frame;
[0051] S31, feeding the abrasive into the sandblasting pot, starting the air pump, and blowing the abrasive in the sandblasting pot out through the spray gun to roughen the facade of the alloy aluminum substrate 1. The roughening treatment time is 10-20 minutes. The diameter of the stainless steel shot peening particles in step S31 is 200-280 μm.
[0052] S32, after the roughening treatment is completed, start the fan to clean the surface of the alloy aluminum substrate 1 and blow away the abrasive remaining on the surface of the alloy aluminum substrate 1.
[0053] S4, performing a spraying process on the alloy aluminum substrate 1 treated in step S1 to obtain a high-density coated aluminum plate;
[0054] S40, injecting the liquid paint obtained in step S2 into the paint bin of the spray box in step S3 to complete the loading operation;
[0055] S41, start the air pump, and the air pump sprays the liquid paint inside the paint tank out from the spray gun mouth;
[0056] S42, the spray gun performs periodic reciprocating motion on the surface of the alloy aluminum substrate 1, and the spraying time is 18 minutes to 22 minutes.
[0057] S5. Send the high-density coated aluminum plate obtained in step S4 to a drying room for curing treatment to obtain a high-density coated aluminum plate with a stable surface coating.
[0058] In this embodiment, the spray box sprays abrasives onto the surface of the alloy aluminum substrate 1 through an air pump, so that dense pits are formed on the surface of the aluminum material, which facilitates the subsequent liquid coating to adhere to the surface of the alloy aluminum substrate 1.
[0059] Embodiment 2
[0060] The high-density coated aluminum plate and its preparation method provided in this embodiment are roughly the same as those in Example 1, with the main difference being that the components of the insulating inorganic mixture include 32.5% by mass of phosphoric acid, 5.6% by mass of magnesium oxide, 8.65% by mass of aluminum hydroxide, 0.85% by mass of boric acid, 17.3% by mass of silicon oxide and 35.1% by mass of water.
[0061] Embodiment 3
[0062] The high-density coated aluminum plate and its preparation method provided in this embodiment are roughly the same as those in Example 1, with the main difference being that the components of the insulating inorganic mixture include 29.2% by mass of phosphoric acid, 5% by mass of magnesium oxide, 7.92% by mass of aluminum hydroxide, 0.55% by mass of boric acid, 16.3% by mass of silicon oxide and 41.03% by mass of water.
[0063] Comparative Example 1
[0064] The high-density coated aluminum plate and the preparation method thereof provided in this embodiment are substantially the same as those in Embodiment 1, with the main difference being that no insulating inorganic mixture is added.
[0065] Comparative Example 2
[0066] The high-density coated aluminum plate and the preparation method thereof provided in this embodiment are substantially the same as those in Embodiment 1, the main difference being that no n-butanol-etherified melamine formaldehyde resin and water-based polyurethane are added.
[0067] Comparative Example 3
[0068] The high-density coated aluminum plate and the preparation method thereof provided in this embodiment are substantially the same as those in Embodiment 1, the main difference being that no primer layer is sprayed.
[0069] Comparative Example 4
[0070] The high-density coated aluminum plate and the preparation method thereof provided in this embodiment are substantially the same as those in Embodiment 1, the main difference being that no sandblasting roughening process is performed.
[0071] Performance Testing
[0072] Take the aluminum plates prepared in Examples 1 to 3 and Comparative Examples 1 to 4, and conduct a comparative performance analysis experiment on the prepared aluminum plates;
[0073] Performance analysis experiment: Six groups of test racks were placed in the laboratory, and the aluminum plates made by Examples 1 to 3 and Comparative Examples 1 to 4 were placed on seven groups of test racks in turn. There were ten aluminum plates on each test rack. The metallographic structure of the coating was observed and the coating thickness was measured using an OLYMPUS-BX60M optical metallographic microscope. The surface morphology of the coating was observed using a Quanta200 environmental scanning electron microscope, and the porosity of the coating was analyzed using Scandium software; the aluminum plate was sent to a JY-60 salt spray tester for a neutral salt spray test according to the GB / T 10125-2012 method. The test solution was a 5% NaCl solution, the test temperature was 35°C, and the salt spray pH value was 6.5 to 7.2; the aluminum plate was placed inside a withstand voltage tester, and a high voltage current with a gradually increasing voltage was passed through, and the alarm current was set to 100nA. The test results were averaged and recorded as shown in Table 1:
[0074] Table 1 Aluminum plate coating test table
[0075]
[0076]
[0077] By analyzing the relevant data in the above table, it can be known that the disease-preventing and production-increasing fish feed produced by the present invention adds a sandblasting roughening treatment process to the existing aluminum plate preparation method, and the stainless steel shot peening particles impact the surface of the alloy aluminum substrate 1 at high speed, so that the surface of the alloy aluminum substrate 1 is roughened, and the mixed coating can be more easily attached to its surface, thereby preparing an aluminum plate with a high-density coating, so that the aluminum plate has good corrosion resistance and electrical breakdown resistance; the coating components on the surface of the aluminum plate include n-butanol etherified melamine formaldehyde resin, water-based polyurethane and insulating inorganic mixture, which can improve the electrical breakdown resistance of the aluminum plate, wherein an etherifying agent is added to the n-butanol etherified melamine formaldehyde resin for synthesis reaction, and more amino groups react with the etherifying agent to form ether bonds, and the generated highly etherified n-butanol etherified melamine formaldehyde resin is etherified. Butanol-etherified melamine formaldehyde resin can cross-link and modify waterborne polyurethane, improve the gloss, hardness, heat resistance, water resistance, acid and alkali resistance and other properties of waterborne polyurethane, so that the waterborne polyurethane can improve the bonding performance of the insulating inorganic mixture, so that the insulating inorganic mixture can stably adhere to the surface of the aluminum alloy aluminum substrate, thereby improving the corrosion resistance and electrical breakdown resistance of the high-density coating, and chemical fumes will not cause the high-density coated aluminum plate to age and discolor. The insulating inorganic mixture is composed of phosphoric acid, magnesium oxide aluminum hydroxide, boric acid and silicon oxide, so that the insulating inorganic mixture has good electrical breakdown resistance and corrosion resistance; in addition, a primer layer 11 is sprayed on the surface of the alloy aluminum substrate 1, so that the high-density coating can stably adhere to the surface of the primer layer 11.
[0078] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high-density coated aluminum plate, comprising an alloy aluminum substrate (1), characterized in that: The surface of the alloy aluminum substrate (1) is coated with a primer layer (11), a high-density coating (12), a top coating (13) and an outer protective layer (14) in sequence, and the coating components of the high-density coating (12) include n-butanol etherified melamine formaldehyde resin, water-based polyurethane and an insulating inorganic mixture.
2. The high-density coated aluminum plate according to claim 1, characterized in that: The coating composition of the primer layer (11) includes acrylic acid and polyurethane.
3. The high-density coated aluminum plate according to claim 1, characterized in that: The components of the insulating inorganic mixture include 26.1%-32.5% by mass of phosphoric acid, 4.2%-5.6% by mass of magnesium oxide, 7.21%-8.65% by mass of aluminum hydroxide, 0.25%-0.85% by mass of boric acid, 15.2%-17.3% by mass of silicon oxide and 35.1%-47.04% by mass of water.
4. A method for preparing a high-density coated aluminum plate, characterized in that: Using any one of the high-density coated aluminum plates of claims 1 to 3, the method comprises the following steps: S1, sequentially subjecting the alloy aluminum substrate (1) to be processed and coated to water washing, acid washing, ethanol washing and pure water washing steps to obtain an aluminum plate with a clean surface and no oil; S2, 3% to 8% by mass of n-butanol etherified melamine formaldehyde resin, 8% to 16% by mass of waterborne polyurethane, 45% to 60% by mass of insulating inorganic mixture and 15% to 25% by mass of stainless steel shot peening particles are fully mixed under stirring conditions to obtain a uniformly mixed liquid coating; S3, subjecting the alloy aluminum substrate (1) obtained in step S2 to a sandblasting roughening process; S4, performing a spraying process on the alloy aluminum substrate (1) treated in step S1 to obtain a high-density coated aluminum plate; S5. Send the high-density coated aluminum plate obtained in step S4 to a drying room for curing treatment to obtain a high-density coated aluminum plate with a stable surface coating.
5. The method for preparing a high-density coated aluminum plate according to claim 4, characterized in that: The pickling process in step S1 comprises the following steps: S10, immersing the washed aluminum alloy substrate (1) in a pickling tank for 5 minutes to 8 minutes; S11, taking the soaked aluminum alloy substrate (1) out of the pickling tank, and sending it into a warm water tank for soaking and washing, the soaking and washing time is 3 min-5 min, the water temperature is 30-55°, and the reaction substances and residual acid generated during the pickling process are removed; S12. The alloy aluminum substrate (1) is taken out from the warm water pool and placed into a cleaning box. The water guns on both sides of the cleaning box are used to rinse the outer surface of the alloy aluminum substrate (1) to ensure that residual substances are completely removed. The water temperature is controlled to avoid aging effects on the aluminum alloy plate. The temperature of the water sprayed from the water gun is 10°-20°.
6. The method for preparing a high-density coated aluminum plate according to claim 4, characterized in that: The ethanol washing process in step S1 comprises the following steps: S20, sending the alloy aluminum substrate (1) into an ethanol water washing tank for immersion treatment, wherein the ethanol concentration in the ethanol solution is 62.5%-71.25%, and the immersion time is 3 minutes-5 minutes; S21. Send the ethanol-washed alloy aluminum substrate (1) into a warm water pool for immersion washing. The immersion washing time is 2 min-3 min, and the water temperature is 20-45°, so as to remove the ethanol solution attached to the surface of the aluminum plate during the ethanol washing process.
7. The method for preparing a high-density coated aluminum plate according to claim 4, characterized in that: The sandblasting roughening process in step S3 includes the following steps: S30, fixing the alloy aluminum substrate (1) on the outer side of the spraying positioning frame; S31, feeding the abrasive into the sandblasting pot, starting the air pump, and blowing the abrasive in the sandblasting pot out through the spray gun to roughen the outer surface of the alloy aluminum substrate (1), the roughening treatment time being 10-20 minutes; S32. After the roughening treatment is completed, the fan is started to clean the surface of the alloy aluminum substrate (1) and blow away the abrasive remaining on the surface of the alloy aluminum substrate (1).
8. The method for preparing a high-density coated aluminum plate according to claim 7, characterized in that: The diameter of the stainless steel shot peening particles in step S31 is 200-280 μm.
9. The method for preparing a high-density coated aluminum plate according to claim 8, characterized in that: The abrasive is G40 steel grit.
10. The method for preparing a high-density coated aluminum plate according to claim 4, characterized in that: The spraying process in step S4 includes the following steps: S40, injecting the liquid paint obtained in step S2 into the paint bin of the spray box in step S3 to complete the loading operation; S41, start the air pump, and the air pump sprays the liquid paint inside the paint tank out from the spray gun mouth; S42, the spray gun performs periodic reciprocating motion on the surface of the alloy aluminum substrate (1), and the spraying time is 18 minutes to 22 minutes.
Citation Information
Patent Citations
Imitation stainless steel brushed coated aluminum sheet and its manufacturing method
CN102848639B
Coating materials and the use thereof in coating systems for compnents in vehicle interiors
CN105531335A
Polyester film coating and pre-coated UV (ultraviolet) reinforced polyester film obtained by coating polyester film coating
CN117659845A
Low temperature curing 1k basecoat and method to coat a substrate with the 1k basecoat