Chemical mechanical polishing solution and chemical mechanical polishing method for cobalt interconnection barrier layer titanium
By using a chemical mechanical polishing solution containing citric acid or citrate in the cobalt interconnect barrier layer, combined with hydrogen peroxide and potassium hydroxide to adjust the pH, the problem of reduced removal rate caused by titanium surface oxidation is solved and efficient titanium polishing is achieved Removal and surface smoothing effects for polishing processes on cobalt interconnect structures.
Patent Information
- Application Number
- CN202410792194.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-19
AI Technical Summary
In a weakly alkaline solution containing H2O2, the titanium surface is oxidized into denser and more passivating TiO2, resulting in a reduction in its removal rate and affecting the polishing efficiency of the cobalt interconnect barrier layer.
It is composed of 1-10wt.% abrasive, 0.5-5wt.% oxidant, 10-150mmol/L citric acid or citrate as complexing agent, and the pH regulator is potassium hydroxide, sodium hydroxide or sulfuric acid. The chemical mechanical polishing solution combines hydrogen peroxide as the oxidant, adjusts the pH range to 7-10, and uses a 2-4 inch polishing machine for chemical mechanical polishing.
The material removal rate of titanium is improved, a high-quality smooth surface is obtained, the polishing needs of the cobalt interconnect barrier layer are met, and the resistivity and signal transmission delay are reduced.
Smart Images

Figure CN118791973A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polishing of cobalt interconnection barrier layer titanium, in particular to a chemical mechanical polishing liquid and a chemical mechanical polishing method for cobalt interconnection barrier layer titanium. Background Art
[0002] In the traditional 14nm and above technology nodes of integrated circuits, metal tungsten (W) is used as contact plugs and via filling materials, and titanium / titanium nitride (Ti / TiN) double-layer structures are used as liner / diffusion barrier layers, which are widely used in local interconnect structures of middle-of-line (MOL) processes. As integrated circuits develop towards narrower feature sizes and higher aspect ratios, W contact plugs face disadvantages such as high resistivity and difficulty in conformal deposition without voids. In addition, the feature size of copper (Cu) as the M0-M1 interconnect filling structure is constantly approaching the physical basic size of Cu (the mean free path of Cu electrons is about 40nm), resulting in a sharp increase in the contact resistance of the copper interconnect structure, thereby exacerbating signal transmission delays and interconnect power consumption. Although the bulk resistivity of cobalt (Co) is relatively high, its electron mean free path is only 1 / 4 of that of copper. Using Co instead of W and Cu as contact plugs and local interconnect filling materials has lower resistivity and thinner diffusion barrier layers at low line widths (<10nm). In addition, Co also has the advantages of good substrate adhesion, high resistance to electromigration, and easy conformal deposition without voids in high aspect ratio interconnect trenches. Therefore, Co is considered to be a new interconnect material that can replace tungsten and copper in MOL.
[0003] Chemical mechanical polishing (CMP) is a process that removes material from the wafer through the synergistic effect of chemical reaction and mechanical wear of abrasive particles. Chemical mechanical polishing runs through all aspects of chip manufacturing and is the only enabling technology for wafer surface flattening. The CMP of Co interconnect structures is specifically divided into two steps: the first step is to remove the material at a higher rate. Rapid removal of bulk Co capping and stopping at the barrier layer; second step with lower removal rate The Co / Ti / TiN / dielectric layer is removed simultaneously, and a controllable heterogeneous material removal rate selectivity and good surface quality after polishing are obtained. It needs to be larger than the interconnect metal Co to avoid the formation of dishing defects in the Co interconnect trench.
[0004] In the traditional W / Ti polishing process, the polishing liquid is generally selected to be acidic, so Ti can maintain a high MRR. However, acidic solutions will cause serious corrosion to the interconnect metal Co, greatly reducing the reliability of logic devices. Therefore, the polishing liquid of the Co interconnect barrier layer Ti still needs to remain weakly alkaline. Usually, the polishing liquid used for metals mainly uses colloidal silicon dioxide (SiO2) as abrasive, hydrogen peroxide (H2O2) as an oxidant, and amino acids or carboxylic acids as complexing agents. Among them, the complexing agent promotes the dissolution rate of the metal by chemically reacting with the outer oxide of the metal and the metal, thereby increasing the MRR of the metal. In a weakly alkaline solution containing H2O2, the surface of Ti will be oxidized to TiO2 with stronger density and higher passivation, thereby reducing the removal rate of Ti. Therefore, it is necessary to find a suitable complexing agent to improve the MRR of Ti. Summary of the invention
[0005] The purpose of the present invention is to provide a chemical mechanical polishing solution for cobalt interconnect barrier layer titanium to address the problem in the prior art that the surface of Ti will be oxidized into TiO2 with stronger density and higher passivation in a weak alkaline solution containing H2O2, thereby reducing the removal rate of Ti.
[0006] Another object of the present invention is to provide a chemical mechanical polishing method based on the chemical mechanical polishing solution.
[0007] The technical solution adopted to achieve the purpose of the present invention is:
[0008] A chemical mechanical polishing liquid for cobalt interconnection barrier layer titanium consists of 1-10wt.% abrasive, 0.5-5wt.% oxidant, 10-150mmol / L complexing agent, pH regulator and the balance of water, wherein the complexing agent is citric acid or citrate.
[0009] In the above technical solution, the abrasive is colloidal silica, and the particle size of the colloidal silica is 20-100 nm, preferably 40 nm.
[0010] In the above technical solution, the oxidant is hydrogen peroxide.
[0011] In the above technical solution, the pH adjuster is potassium hydroxide, sodium hydroxide, sulfuric acid or nitric acid.
[0012] In the above technical solution, the pH range of the chemical mechanical polishing solution is 7-10, preferably pH=8.
[0013] In the above technical solution, the complexing agent is potassium citrate.
[0014] Another aspect of the present invention provides a chemical mechanical polishing method for a cobalt interconnect barrier layer titanium, comprising the following steps:
[0015] Step 1, preparing the chemical mechanical polishing solution for the cobalt interconnect barrier layer titanium;
[0016] Step 2: Use a polishing machine to perform chemical mechanical polishing on the titanium metal for 2-5 minutes.
[0017] In the above technical solution, the flow rate of the chemical mechanical polishing liquid is 20-100 mL / min, preferably 50 mL / min.
[0018] In the above technical solution, the polishing machine is a 2-4 inch polishing machine, and the rotation speed of the polishing disc of the polishing machine is 60-90 rpm, preferably 79 rpm.
[0019] In the above technical solution, the rotation speed of the polishing head of the polishing machine is 60-90 rpm, preferably 81 rpm; the polishing pressure is 1-2 psi, preferably 1.5 psi.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The chemical mechanical polishing liquid of the present invention selects suitable oxidant and complexing agent types and concentration ratios. Under the synergistic effect of the chemical reaction of the chemical substances in the polishing liquid and the mechanical wear of the abrasive particles, the material removal rate of metal titanium is improved, and a high-quality and smooth surface is obtained. It has broad application prospects in the CMP process of cobalt interconnect barrier layer titanium. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Shown are MRR graphs of colloidal silica to titanium at different weight ratios.
[0023] Figure 2 Shown are MRR graphs of hydrogen peroxide to titanium at different weight ratios.
[0024] Figure 3 Shown are the electrochemical experimental results of titanium in hydrogen peroxide solutions with different weight ratios: (a) is the electrochemical impedance spectrum; (b) is the Tafel polarization curve.
[0025] Figure 4 Shown is the MRR diagram of different types of complexing agents on titanium.
[0026] Figure 5 Shown is the MRR graph of different concentrations of potassium citrate against titanium.
[0027] Figure 6 The results of electrochemical experiments on titanium in potassium citrate (CAK) solutions with different concentrations of hydrogen peroxide are shown: (a) is the electrochemical impedance spectrum; (b) is the Tafel polarization curve
[0028] Figure 7 Shown is an AFM image of titanium after polishing in a 5 wt.% colloidal silica, 3 wt.% hydrogen peroxide, and 100 mmol / L potassium citrate solution. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0030] The preparation method of the polishing liquid in this specific embodiment is: add a certain amount of abrasive, oxidant, and chelating agent into deionized water, use a pH adjuster to adjust the pH of the polishing liquid, use a magnetic stirrer to stir for 10 minutes to make the abrasive particles evenly dispersed and the chemical reagents fully dissolved, and use a magnetic stirrer to continuously stir the polishing liquid during the chemical mechanical polishing process.
[0031] The chemical mechanical polishing method is: using a 2-4 inch commercial polishing machine, the polishing material is titanium (purity 99.99%) with a diameter of 3 inches and a thickness of 1.5 mm, and an IC 1010 hard polishing pad, and the chemical mechanical polishing operation is performed. The polishing parameters are set as follows: polishing pressure 1.5 psi, polishing disc speed 79 rpm, polishing head speed 81 rpm, polishing liquid flow 50 mL / min, and polishing time 3 min.
[0032] The measurement and characterization methods used in the present invention are: using a weighing method to measure the weight change of titanium before and after chemical mechanical polishing, and calculating the material removal rate of titanium; using an atomic force microscope to measure the surface roughness Ra and surface morphology of the titanium after polishing.
[0033] Example 1
[0034] 1.1 Comparison of the effect of abrasive content on titanium MRR
[0035] 1000g of polishing liquid was prepared, in which the amount of abrasive added was used as a variable, different weight percentages (1wt.%, 3wt.%, 5wt.%) of colloidal silica (SiO2, mass fraction 40wt.%) were taken, and the rest was deionized water, and the pH of the polishing liquid was adjusted to 8. Chemical mechanical polishing of titanium was performed to explore the effect of abrasive content on titanium MRR.
[0036] like Figure 1The figure shows the effect of adding different weight ratios of colloidal silica on the MRR of titanium. When 1wt.% colloidal silica is added, the MRR of titanium is 0.54nm / min; when 3wt.% colloidal silica is added, the MRR of titanium increases to 1.08nm / min; when the weight ratio of colloidal silica is increased to 5wt.%, the MRR of titanium increases to 2.16nm / min. According to the above results, it can be seen that the change in the abrasive content in the polishing liquid does not significantly affect the MRR of titanium. Therefore, 5wt.% colloidal silica is determined as the abrasive addition amount.
[0037] 1.2 Comparison of the effect of oxidant content on titanium MRR
[0038] 1000g of polishing liquid was prepared, which contained 5wt.% colloidal silica (SiO2, mass fraction 40wt.%), and the amount of oxidant added was used as a variable, and different weight percentages (0.5wt.%, 1wt.%, 3wt.%, 5wt.%) of hydrogen peroxide (H2O2, mass fraction 30wt.%) were selected, and the rest was deionized water, and the pH of the polishing liquid was adjusted to 8. Chemical mechanical polishing of titanium was performed to explore the effect of oxidant content on titanium MRR.
[0039] like Figure 2 As shown, the results of the effect of adding hydrogen peroxide in different weight ratios on the MRR of titanium. When 0.5wt.% hydrogen peroxide was added on the basis of adding 5wt.% colloidal silica, the MRR of titanium increased to 3.26nm / min; when the amount of hydrogen peroxide added gradually increased, the MRR of titanium also gradually increased. When the amount of hydrogen peroxide added increased to 5wt.%, the MRR of titanium increased to 12.98nm / min, which still could not meet the removal rate requirements of the barrier layer titanium, and at this time, due to the high content of hydrogen peroxide, the degree of corrosion on the polishing head and polishing pad was high, and obvious corrosion could be observed with the naked eye. Therefore, the amount of hydrogen peroxide oxidizing agent added was determined to be 3wt.%. However, it is still necessary to find a suitable titanium complexing agent to improve the MRR of titanium.
[0040] The polishing liquid mentioned in Example 1.2 was configured to conduct an electrochemical experiment to explore the mechanism of action of the oxidant hydrogen peroxide on Ti. The prepared solution did not contain abrasives to prevent the silica particles from agglomerating into flocs and affecting the results of the electrochemical experiment. The instrument used in the electrochemical experiment was the VersaSTAT 3F electrochemical workstation of Princeton, USA. A three-electrode system was used, including a working electrode (titanium electrode, purity 99.99%), a counter electrode (platinum electrode) and a reference electrode (saturated Ag / AgCl electrode). The electrochemical impedance spectrum and Tafel polarization curve of the working electrode in different contents of hydrogen peroxide were measured, and its surface electrochemical parameters were calculated and analyzed. The measurement results are shown in the figure. Figure 3 As shown in Table 1.
[0041] Table 1 Electrochemical experimental results of titanium in different contents of hydrogen peroxide
[0042]
[0043] According to the results in Table 1, it can be seen that with the increase of hydrogen peroxide addition, the polarization impedance of the titanium surface gradually decreases. When no hydrogen peroxide is added initially, the polarization impedance of the titanium surface is 191600Ω·cm 2 When 5wt.% H2O2 is added, the surface polarization impedance of titanium decreases to 2047Ω·cm 2 , reduced by 98.93%; with the increase of hydrogen peroxide addition, the corrosion current on the titanium surface increased. When no hydrogen peroxide was added, the corrosion current density on the titanium surface was 0.22μA·cm -2 When the amount of hydrogen peroxide added increased to 5wt.%, the corrosion current density on the titanium surface increased to 14.80μA·cm -2 , an increase of 98.51%. Therefore, the addition of hydrogen peroxide can reduce the density and passivation of the natural oxide titanium dioxide on the titanium surface, thereby reducing its surface impedance and increasing the corrosion of the titanium surface.
[0044] 1.3 Comparison of the effects of complexing agent types on titanium MRR
[0045] 1000g of polishing liquid was prepared, which contained 5wt.% colloidal silicon dioxide (SiO2, mass fraction 40wt.%), 3wt.% hydrogen peroxide (H2O2, mass fraction 30wt.%), and the type of complexing agent was used as a variable, and different types of complexing agents (glycine, citric acid, potassium citrate, arginine) with the same additive amount were selected, and the rest was deionized water, and the pH of the polishing liquid was adjusted to 8. Chemical mechanical polishing was performed on titanium to explore the effect of the type of complexing agent on the MRR of titanium.
[0046] like Figure 3 The results of adding different types of complexing agents on the MRR of titanium are shown in Figure 1. On the basis of adding 5wt.% colloidal silica and 3wt.% hydrogen peroxide, 100mmol / L of glycine, citric acid, potassium citrate, and arginine were added respectively. The surface morphology of titanium after polishing in 5wt.% colloidal silica, 3wt.% hydrogen peroxide and 100mM potassium citrate solution is shown in Figure 2. Figure 7 The results show that when citric acid / potassium citrate is added, the MRR of titanium increases significantly to about 120nm / min, while after polishing with the polishing liquid containing glycine and arginine, the MRR of titanium remains basically unchanged or increases slightly. Therefore, by comparison, it can be seen that citric acid and potassium citrate have a significant complexing effect on titanium.
[0047] Example 2
[0048] 1000g of polishing liquid was prepared, which contained 5wt.% colloidal silicon dioxide (SiO2, mass fraction 40wt.%), 3wt.% hydrogen peroxide (H2O2, mass fraction 30wt.%), and the amount of complexing agent added was used as a variable, different concentrations (10mmol / L, 25mmol / L, 50mmol / L, 100mmol / L) of potassium citrate were selected, and the rest was deionized water, and the pH of the polishing liquid was adjusted to 8. Chemical mechanical polishing of titanium was carried out to explore the effect of complexing agent content on titanium MRR.
[0049] like Figure 4 The results show the effect of adding different concentrations of potassium citrate on titanium MRR. Figure 4 It can be seen that in the base polishing solution of 5wt.% colloidal silica and 3wt.% hydrogen peroxide, as the concentration of potassium citrate increases, the MRR of titanium also increases, which once again proves the effective complexing effect of potassium citrate on titanium.
[0050] In order to explore the mechanism of action of potassium citrate on Ti in a hydrogen peroxide solution, 1wt.% hydrogen peroxide was used as the base solution to explore the effect of different concentrations of potassium citrate on the electrochemical experimental structure of Ti. The experimental process is as described in Example 1. The electrochemical results are shown in Figure 6 As shown in Table 2.
[0051] Table 2 Electrochemical experimental results of titanium in different concentrations of potassium citrate (CAK) solutions containing hydrogen peroxide
[0052]
[0053] According to the results shown in Table 2, it can be seen that in the potassium citrate solution containing hydrogen peroxide, as the concentration of potassium citrate increases, the compactness of the oxide on the titanium surface can be further reduced, the polarization impedance of the titanium surface can be reduced, and the corrosion current can be increased.
[0054] The above results show that the chemical mechanical polishing solution of the present invention can greatly improve the material removal rate of titanium during the chemical mechanical polishing process. Figure 7 As shown in the figure, the surface is smooth after polishing, with a roughness of 0.119nm. The mechanism of action is that hydrogen peroxide and potassium citrate can reduce the compactness of the oxide on the titanium surface and accelerate its corrosion, so the titanium can be quickly removed under the mechanical action of the abrasive, and its removal rate can be increased. Therefore, the proposed effective complexing agent selection for the cobalt interconnection barrier layer titanium and the chemical mechanical polishing method can meet the removal rate requirements of the barrier layer titanium, and have broad application prospects in the polishing process of the cobalt interconnection titanium barrier layer structure of the integrated circuit.
[0055] The above is only a preferred embodiment of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A chemical mechanical polishing solution for cobalt interconnect barrier layer titanium, characterized in that: The invention comprises 1-10wt.% of abrasive, 0.5-5wt.% of oxidant, 10-150mmol / L of complexing agent, pH regulator and the balance of water, wherein the complexing agent is citric acid or citrate.
2. The chemical mechanical polishing solution for the cobalt interconnect barrier layer titanium according to claim 1, characterized in that: The abrasive is colloidal silica, and the particle size of the colloidal silica is 20-100 nm, preferably 40 nm.
3. The chemical mechanical polishing solution for the cobalt interconnect barrier layer titanium according to claim 1, characterized in that: The oxidant is hydrogen peroxide.
4. The chemical mechanical polishing solution for the cobalt interconnect barrier layer titanium according to claim 1, characterized in that: The pH regulator is potassium hydroxide, sodium hydroxide, sulfuric acid or nitric acid.
5. The chemical mechanical polishing solution for the cobalt interconnect barrier layer titanium according to claim 1, characterized in that: The pH range of the chemical mechanical polishing solution is 7-10, preferably pH=8.
6. The chemical mechanical polishing solution for the cobalt interconnect barrier layer titanium according to claim 1, characterized in that: The complexing agent is potassium citrate.
7. A chemical mechanical polishing method for cobalt interconnect barrier layer titanium, characterized in that: The following steps are involved: Step 1, preparing a chemical mechanical polishing solution for a cobalt interconnect barrier layer titanium as described in any one of claims 1 to 6; Step 2: Use a polishing machine to perform chemical mechanical polishing on the titanium metal for 2-5 minutes.
8. The chemical mechanical polishing method according to claim 7, characterized in that: The flow rate of the chemical mechanical polishing liquid is 20-100 mL / min, preferably 50 mL / min.
9. The chemical mechanical polishing method according to claim 7, characterized in that: The polishing machine is a 2-4 inch polishing machine, and the rotation speed of the polishing disc of the polishing machine is 60-90 rpm, preferably 79 rpm.
10. The chemical mechanical polishing method according to claim 7, characterized in that: The rotation speed of the polishing head of the polishing machine is 60-90 rpm, preferably 81 rpm; the polishing pressure is 1-2 psi, preferably 1.5 psi.
Citation Information
Patent Citations
Chemical mechanical polishing aqueous composite and chemical mechanical polishing process of titanium substrate
CN102796458A
Chemical mechanical polishing composition and method
CN103773248A
Chemical mechanical polishing liquid for titanium
CN104593776A
Chemical mechanical polishing liquid and use method thereof
CN104726028A
Titanium alloy grinding and chemical-mechanical polishing method
CN106112791A
Cited By
Copper / titanium / TEOS (tetraethyl orthosilicate) rate selective control CMP (chemical mechanical polishing) solution based on TSV (through silicon via)
CN119709023A