Polymer film-based composite nickel film and preparation method thereof
By optimizing the process to combine the polymer film and the nickel metal layer, the problems of weak interfacial bonding force, complex process and poor environmental compatibility of the composite nickel film have been solved, and the preparation of high-performance composite nickel film has been achieved. It is suitable for a variety of high-tech fields and has Excellent mechanical and electrical properties.
Patent Information
- Application Number
- CN202411032941.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-18
AI Technical Summary
Existing composite nickel films have problems with weak interface bonding, complex preparation processes, high costs, and poor environmental compatibility, making it difficult to meet the needs of high-performance materials for battery electrodes, electromagnetic shielding, sensors, and microelectronic devices.
By optimizing the preparation process, plasma treatment and ultraviolet irradiation treatment are used to pretreat the substrate to form an intermediate adhesive layer, and then deposit a nickel metal layer on it and thicken the nickel plating layer through electrodeposition, combining the mechanical strength and mechanical strength of the polymer film. The conductivity of nickel ensures strong interface bonding, simplifies the process and reduces costs, while focusing on environmental friendliness.
The polymer thin film-based composite nickel film has excellent comprehensive performance, excellent mechanical strength, electrical conductivity and corrosion resistance, and the preparation process is simple and controllable. It is suitable for applications in a variety of high-tech fields, especially in wearable electronics and flexible displays. Excellent performance in screen and aerospace materials.
Smart Images

Figure BDA0004970382630000131 
Figure BDA0004970382630000141 
Figure BDA0004970382630000142
Abstract
Description
Technical Field
[0001] The invention relates to a field, and in particular to a polymer film-based composite nickel film and a preparation method thereof. Background Art
[0002] At present, with the rapid development of electronics, energy, aerospace and other fields, the demand for high-performance materials is growing, especially in applications such as battery electrode materials, electromagnetic shielding, sensors and microelectronic devices, the comprehensive performance requirements of materials are particularly stringent. Although traditional single materials such as pure nickel film or polymer film have their own characteristics, they all face limitations in practical applications. Pure nickel film has good conductivity and corrosion resistance, but its mechanical strength is insufficient and it is easy to break; while polymer film has excellent mechanical strength and flexibility, but its conductivity and corrosion resistance are unsatisfactory. Therefore, the development of a new composite material that integrates the mechanical properties of polymer film and the electrical properties of metal film has become the key to solving the above problems.
[0003] In the prior art, attempts have been made to combine metals with polymer materials in order to achieve complementary properties, but these attempts often face problems such as weak bonding, complex preparation processes, high costs, or environmental unfriendliness. For example, some studies use simple physical mixing or coating methods, but the interface bonding is not strong and is easy to delaminate; while other studies may use complex multi-step chemical reactions, which improve the bonding strength but sacrifice the simplicity and cost-effectiveness of the process.
[0004] The main disadvantages of the existing technology include: 1. Weak interface bonding, which makes the composite material easy to delaminate or peel off during use. 2. The preparation process is complicated and the cost is high, which is not conducive to large-scale production. 3. Poor environmental compatibility, the use of harmful chemicals, does not meet the requirements of sustainable development. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a polymer film-based composite nickel film and a preparation method thereof in view of the deficiencies in the above-mentioned prior art. The present invention innovatively combines the high strength and toughness of polymer materials with the electrical conductivity and corrosion resistance of nickel metal, ensures a strong interface bond through an optimized preparation process, simplifies the process flow, reduces production costs, and focuses on environmental friendliness to meet the market demand for high-performance materials.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: in the first aspect of the present invention, a method for preparing a polymer film-based composite nickel film is provided, comprising the following steps:
[0007] S1, substrate pretreatment: the substrate surface is sequentially subjected to plasma treatment and ultraviolet irradiation treatment to obtain a pretreated substrate;
[0008] S2, preparing an intermediate bonding layer on the pretreated substrate;
[0009] S3, preparing a nickel metal layer on the intermediate bonding layer;
[0010] S4, electro-depositing a thickened nickel-plated layer on the nickel metal layer to obtain a polymer film-based composite nickel film;
[0011] The substrate is any one of a PI film, a reinforced modified PI substrate, a reinforced PET substrate, a surface modified PI substrate, and a surface modified PET substrate.
[0012] Preferably, step S1 specifically includes: treating the surface of the substrate with an oxygen plasma process, and the processing parameters are set as follows: power 50W, processing time 3 minutes, vacuum degree 10 -3 Torr; then ultraviolet light irradiation treatment for 1 min to obtain a pretreated substrate.
[0013] Preferably, step S2 specifically comprises:
[0014] S2-1, preparing adhesive solution:
[0015] By weight, 50 parts of polyether polyol, 45 parts of isocyanate, 5 parts of solvent, 3 parts of crosslinking agent and 2 parts of catalyst were mixed uniformly to obtain a polyurethane prepolymer;
[0016] According to the weight ratio of tetrabutyl titanate to polyurethane prepolymer being 1:100, tetrabutyl titanate is added to the polyurethane prepolymer, and stirred evenly to obtain an adhesive solution;
[0017] S2-2. Spin, dip or spray the adhesive solution evenly on the surface of the pretreated substrate, and cure it at 70-90°C for 15-60 minutes to form an intermediate adhesive layer.
[0018] Preferably, step S3 specifically comprises:
[0019] A nickel metal layer was deposited on the intermediate bonding layer using a DC magnetron sputtering process, and the process conditions were as follows: the working gas was argon, the power was set to 100 W, the gas pressure was 1 Pa, and the sputtering time was 30 minutes.
[0020] Preferably, step S4 is specifically:
[0021] The substrate after the nickel metal layer is deposited obtained in step S3 is used as a cathode, and a pure nickel plate is used as an anode to electro-deposit a thickened nickel plating layer on the deposited nickel metal layer, and the electrolyte formula used is: nickel sulfate concentration is 200g / L, boric acid concentration is 30g / L, sodium chloride concentration is 10g / L, and nickel chloride concentration is 10g / L;
[0022] The electrodeposition process parameters are: current density is 10mA / cm 2 , the electrodeposition time was 1 hour, the pH value of the electrolyte was maintained at 4-5, and the temperature was controlled at 50°C.
[0023] Preferably, the substrate is a reinforced modified PI substrate, which is prepared by the following method:
[0024] 1-1) adding 20 parts of pyromellitic anhydride, 10 parts of 4,4'-diaminodiphenyl ether, and 2 parts of 3,4'-diaminodiphenyl ether diglycidyl ether to 100 parts of N,N-dimethylformamide by weight, stirring and reacting for 24 hours under ice bath to obtain a prepolymer solution;
[0025] 1-2) After degassing, the prepolymer solution was uniformly coated on a clean glass substrate, and then heated to 250°C at a heating rate of 5°C / min, reacted for 3 hours, and finally the obtained film was completely removed from the glass substrate to obtain a reinforced modified PI substrate with a thickness of 25 μm.
[0026] Preferably, the substrate is a reinforced PET substrate, which is prepared by the following method:
[0027] 2-1) adding glass fiber into an ethanol solution of a silane coupling agent having a mass concentration of 1%, immersing the solution at 50° C. for 2 hours, filtering, and drying to a constant weight to obtain pretreated glass fiber;
[0028] 2-2) mixing the pretreated glass fiber and the PET resin in a mass ratio of 1:10, and melt-extruded at 200° C. through a twin-screw extruder to obtain a sheet;
[0029] 2-3) The extruded sheet was biaxially stretched at 120°C, with a longitudinal stretching ratio of 3 times and a transverse stretching ratio of 3 times. The product thickness after biaxial stretching was 25 μm, and then heat-set at 150°C, cooled, and rolled to obtain a reinforced PET substrate.
[0030] Preferably, the substrate is a surface-modified PI substrate, which is prepared by the following method:
[0031] 3-1) The PI film with a thickness of 25 μm was treated with oxygen plasma, the power was set to 200 W, and the treatment time was 5 minutes;
[0032] 3-2) Add 3-aminopropyltriethoxysilane to anhydrous ethanol to prepare a silane coupling agent solution with a concentration of 1%, and evenly coat the silane coupling agent solution on the surface of the PI film obtained in step 3-1) to control the coating amount to 10 mg / m 2 , and then cured at 140 °C for 30 minutes to obtain a surface-modified PI substrate
[0033] Preferably, the substrate is a surface-modified PET substrate, which is prepared by the following method:
[0034] 4-1) A PET substrate with a thickness of 50 μm was subjected to corona treatment, with the corona discharge power set to 1.5 kW and the treatment speed set to 1 m / min;
[0035] 4-2) 3-(triethoxysilyl)propylmethyldimethoxysilane was added to anhydrous ethanol to prepare a silane coupling agent solution with a concentration of 1%, and the silane coupling agent solution was evenly coated on the surface of the PET substrate obtained in step 4-1) to control the coating amount to 10 mg / m 2 , and then cured at 120°C for 30 minutes to finally obtain a surface-modified PET substrate.
[0036] The second aspect of the present invention provides a polymer film-based composite nickel film, which is prepared by the method as described above.
[0037] The beneficial effects of the present invention are:
[0038] 1. Excellent comprehensive performance: The polymer film-based composite nickel film provided by the present invention successfully integrates the respective advantages of polymer film and pure nickel film. The polymer substrate brings excellent mechanical strength and toughness, effectively resisting physical damage, while the nickel layer provides excellent conductivity and corrosion resistance. This unique combination enables the composite nickel film to maintain lightness and flexibility while also having a wide range of application potentials, especially in those fields that require both high strength and good conductivity, such as wearable electronic devices, flexible displays, aerospace materials and new energy vehicle components.
[0039] 2. The preparation process is simple and controllable: Another highlight of the present invention is its optimized preparation process. By precisely controlling the parameters of key steps such as sputtering and electroplating, the thickness, uniformity and bonding strength of the nickel layer with the substrate can be efficiently and stably controlled. This high degree of adjustability not only ensures the consistency and reliability of the product, but also greatly improves the flexibility of the preparation process. It can be quickly adjusted according to different application requirements to achieve personalized customization, thereby broadening its market application scope.
[0040] 3. Strong environmental adaptability: The polymer film-based composite nickel film provided by the present invention exhibits excellent corrosion resistance and electrical stability, which means that it can maintain long-term stable working performance in harsh environments such as high temperature, humidity, and salt spray; this is especially important for applications in outdoor electronic equipment, marine engineering materials, and the chemical industry, and can reduce maintenance costs while extending service life and improving the reliability and economy of the overall system.
[0041] In summary, the polymer thin film-based composite nickel film provided by the present invention has achieved not only a leap in performance, but also a breakthrough in process feasibility and environmental adaptability by integrating the latest achievements in materials science and precision processing technology, providing strong technical support for the development of multiple industries and having significant innovative value and social and economic benefits. DETAILED DESCRIPTION
[0042] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.
[0043] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0044] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0045] The present invention provides a polymer film-based composite nickel film, and a preparation method thereof comprises the following steps:
[0046] S1, substrate pretreatment: the substrate surface is sequentially subjected to plasma treatment and ultraviolet irradiation treatment to obtain a pretreated substrate;
[0047] S2, preparing an intermediate bonding layer on the pretreated substrate;
[0048] S3, preparing a nickel metal layer on the intermediate bonding layer;
[0049] S4. Electrodepositing a thickened nickel plating layer on the nickel metal layer to obtain a polymer film-based composite nickel film.
[0050] In a preferred embodiment, the substrate is a polymer material such as a polyimide (PI) film, a polyester (PET) film, a polyvinyl formal (PVDF) film, etc. These materials not only have excellent mechanical strength and flexibility, but also have good chemical stability and thermal stability, providing a good physical basis for subsequent processing. In a further preferred embodiment, the substrate is any one of a reinforced modified PI substrate, a reinforced PET substrate, a surface modified PI substrate, and a surface modified PET substrate.
[0051] In a preferred embodiment, step S1 specifically includes: treating the substrate surface with an oxygen plasma process, and the processing parameters are set as follows: power 50W, processing time 3 minutes, vacuum degree 10 -3Torr to completely remove organic pollutants on the surface of the substrate and enhance surface activity; then ultraviolet light irradiation treatment for 1 minute to obtain a pretreated substrate, further enhance the chemical reaction activity of the substrate, and promote the close bonding of subsequent coating layers.
[0052] In a preferred embodiment, step S2 is specifically as follows:
[0053] S2-1, preparing adhesive solution:
[0054] By weight, 50 parts of polyether polyol, 45 parts of isocyanate, 5 parts of solvent, 3 parts of crosslinking agent and 2 parts of catalyst were mixed uniformly to obtain a polyurethane prepolymer.
[0055] Further preferably, the polyether polyol is selected from Dow Corning DOWFAX TM 2A1; Isocyanate: Bayer Desmodur N 3300A; Solvent: Ethyl acetate (analytical grade); Crosslinking agent: Dow Corning Z-6020; Catalyst: Dow Corning Z-6030;
[0056] According to the weight ratio of tetrabutyl titanate (TBT) to polyurethane prepolymer being 1:100, tetrabutyl titanate is added to the polyurethane prepolymer and stirred evenly to obtain an adhesive solution;
[0057] S2-2. Use spin coating, dip coating or spray coating to ensure that the bonding layer is uniform and thin, avoiding the stress concentration problem caused by local excessive thickness; evenly apply the adhesive solution on the surface of the pretreated substrate, and cure it at 70-90°C for 15-60 minutes to form an intermediate bonding layer to ensure the stability and durability of the bonding layer.
[0058] Among them, TBT, as a highly efficient titanate coupling agent, can significantly enhance the adhesion between polymer materials and metal substrates, forming a stable chemical bonding interface.
[0059] In a preferred embodiment, step S3 is specifically as follows:
[0060] A DC magnetron sputtering process (a form of PVD) is used to deposit a nickel metal layer on the intermediate bonding layer. The process conditions are: the target material uses a high-purity nickel target with a purity of ≥99.99%, the working gas is argon, the power is set to 100W, the gas pressure is 1Pa, the sputtering time is 30 minutes, and the substrate temperature is maintained at room temperature to avoid additional heating to prevent affecting the properties of the substrate material. During the preparation process, the current and voltage changes during the sputtering process are monitored in real time to ensure process stability. After the deposition is completed, the actual thickness of the nickel layer is measured using an ellipsometer to confirm whether it meets the design requirements.
[0061] The magnetron sputtering process can not only accurately control the thickness of the nickel layer, but also ensure the continuity and uniformity of its structure, providing a good conductive foundation for subsequent electrodeposition. In this step, the microstructure and purity of the nickel layer can be optimized by precisely controlling the sputtering power, gas pressure and deposition time.
[0062] In a preferred embodiment, step S4 is specifically as follows:
[0063] The substrate after the nickel metal layer is deposited obtained in step S3 is used as a cathode, and a pure nickel plate is used as an anode to electro-deposit a thickened nickel plating layer on the deposited nickel metal layer, and the electrolyte formula used is: nickel sulfate concentration is 200g / L, boric acid concentration is 30g / L, sodium chloride concentration is 10g / L, and nickel chloride concentration is 10g / L;
[0064] The electrodeposition process parameters are: current density is 10mA / cm 2 , the electrodeposition time was 1 hour, the pH value of the electrolyte was maintained at 4-5, and the temperature was controlled at 50°C.
[0065] On the basis of PVD nickel film, the thickness of the nickel layer is further increased through electroplating technology. According to the actual application requirements, the current density, deposition time and plating solution composition are adjusted to flexibly control the final thickness and crystal morphology of the nickel layer to achieve the required conductivity and mechanical strength requirements.
[0066] In a preferred embodiment, the substrate is a reinforced modified PI substrate, which is prepared by the following method:
[0067] 1-1) adding 20 parts of pyromellitic anhydride, 10 parts of 4,4'-diaminodiphenyl ether, and 2 parts of 3,4'-diaminodiphenyl ether diglycidyl ether to 100 parts of N,N-dimethylformamide by weight, stirring and reacting for 24 hours under ice bath to obtain a prepolymer solution;
[0068] 1-2) After degassing, the prepolymer solution was uniformly coated on a clean glass substrate, and then heated to 250°C at a heating rate of 5°C / min, reacted for 3 hours, and finally the obtained film was completely removed from the glass substrate to obtain a reinforced modified PI substrate with a thickness of 25 μm.
[0069] In the present invention, standard polyimide precursors, pyromellitic anhydride (PMDA) and 4,4'-diaminodiphenyl ether (ODA), are selected as main chain building blocks, and a small amount of comonomer containing epoxy groups (such as 3,4'-diaminodiphenyl ether diglycidyl ether) is introduced to enhance adhesion to the metal layer. The enhanced modified PI substrate has the following advantages:
[0070] Enhanced Adhesion: Due to the introduction of epoxy groups, the adhesion of the modified PI substrate to the metal layer is significantly enhanced, reducing the risk of delamination.
[0071] Improved dielectric properties: The addition of comonomer optimizes the dielectric constant and loss tangent of the PI substrate, making it more suitable for high-frequency electronic applications.
[0072] Higher heat resistance: The modified PI substrate has a higher glass transition temperature (Tg), which can maintain structural stability and electrical insulation properties at higher temperatures.
[0073] In a preferred embodiment, the substrate is a reinforced PET substrate, which is prepared by the following method:
[0074] 2-1) adding glass fibers with a diameter of 10 μm and a length of 5 mm into an ethanol solution of a silane coupling agent (specifically Dow Corning Z-6020, provided by Dow Corning) with a mass concentration of 1%, immersing at 50° C. for 2 hours, filtering, and drying to constant weight to obtain pretreated glass fibers; coating with a silane coupling agent to enhance its compatibility and adhesion with a PET substrate;
[0075] 2-2) mixing the pretreated glass fiber and PET resin (brand name: Eastman PETG 6763, provided by Eastman Chemical Company) in a mass ratio of 1:10, and melt-extruded at 200° C. through a twin-screw extruder to obtain a sheet;
[0076] 2-3) The extruded sheet is biaxially stretched at 120°C, with a longitudinal stretching ratio of 3 times and a transverse stretching ratio of 3 times. The product thickness after biaxial stretching is 25 μm, and then heat-set at 150°C, cooled, and rolled to obtain a reinforced PET substrate. The reinforced PET substrate is designed to overcome the poor dimensional stability and thermal deformation problems of traditional PET substrates in high temperature environments, while improving its mechanical strength and chemical resistance to adapt to more demanding application environments.
[0077] The enhanced PET substrate has the following advantages:
[0078] Enhanced mechanical properties: The addition of glass fiber significantly improves the tensile strength and modulus of the substrate, making it less likely to deform when subjected to external forces.
[0079] Improved thermal stability: Through optimized formulation and heat treatment process, the heat deformation temperature of the reinforced PET substrate has been significantly improved, which can maintain dimensional stability at higher temperatures.
[0080] In a preferred embodiment, the substrate is a surface-modified PI substrate, which is prepared by the following method:
[0081] 3-1) The PI film with a thickness of 25 μm was treated with oxygen plasma, the power was set to 200 W, and the treatment time was 5 minutes; plasma treatment can clean the surface, remove organic pollutants, and increase the surface energy, which is beneficial to subsequent bonding;
[0082] 3-2) 3-2) 3-aminopropyltriethoxysilane (brand name Dow Corning Z-6040, provided by Dow Corning) was added to anhydrous ethanol to prepare a silane coupling agent solution with a concentration of 1%. The silane coupling agent solution was evenly coated on the surface of the PI film obtained in step 3-1) and the coating amount was controlled to be 10 mg / m 2 (or coating thickness is 0.1 μm), and then cured at 140° C. for 30 min to form a functional coating to obtain a surface-modified PI substrate.
[0083] The PI substrate is designed to further improve the adhesion, thermal stability, electrical insulation or mechanical strength of the PI film through surface modification or structural modification to adapt to a wider range of applications, especially in the electronics and aerospace fields that require high performance and high reliability.
[0084] Advantages of surface modified PI-based:
[0085] Not only does it retain the advantages of the original PI film, such as excellent thermal stability and electrical insulation, but it also enhances its bonding properties with subsequent layers through surface modification, providing a better substrate option for the preparation of high-performance composite materials.
[0086] In a preferred embodiment, the substrate is a surface-modified PET substrate, which is prepared by the following method:
[0087] 4-1) A PET substrate with a thickness of 50 μm was subjected to corona treatment, with the corona discharge power set to 1.5 kW and the treatment speed set to 1 m / min; free radicals were generated on the surface of the substrate through a high-energy electric field, thereby increasing the surface energy and polarity and enhancing the adhesion of subsequent coatings;
[0088] 4-2) 3-(triethoxysilyl)propylmethyldimethoxysilane (brand name Dow Corning Z-6030, provided by Dow Corning) was added to anhydrous ethanol to prepare a silane coupling agent solution with a concentration of 1%. The silane coupling agent solution was evenly coated on the surface of the PET substrate obtained in step 4-1) to control the coating amount to 10 mg / m 2(or coating thickness of 0.1 μm), and then cured at 120°C for 30 minutes to promote the curing reaction of the silane coupling agent, form a stable siloxane network structure, further improve the chemical stability and temperature resistance of the surface, and finally obtain a surface-modified PET substrate. The modified coating formed by the silane coupling agent can increase the hydrophilicity of the substrate, while providing additional chemical bonding points to enhance adhesion to the subsequent metal layer.
[0089] The goal of surface-modified PET substrate is to improve its thermal stability, chemical stability and adhesion to other materials through modification so that it can be used in a wider range of application scenarios, especially in areas that require higher temperature resistance and durability.
[0090] Advantages of surface modified PET substrate:
[0091] Enhanced Adhesion: The surface energy of the modified PET substrate is significantly improved, and the adhesion to the metal layer or other composite materials is significantly enhanced.
[0092] Improved thermal stability: Through surface modification, the thermal stability of the substrate is improved, allowing it to maintain dimensional stability and mechanical strength at higher temperatures.
[0093] Chemical stability: The introduction of silane coupling agents enhances the chemical stability of the substrate, making it less susceptible to degradation when exposed to chemicals.
[0094] Advantages of homemade process: The surface modified PET substrate can adjust the modification parameters according to the specific application requirements, such as the type and concentration of silane coupling agent, the power and speed of corona discharge, to achieve the best modification effect.
[0095] The surface-modified PET substrate not only retains the original advantages of PET materials, such as good transparency, flexibility and processability, but also significantly improves its application performance in complex environments through surface modification, providing a better substrate option for the preparation of high-performance composite materials.
[0096] The present invention effectively solves the problems existing in the prior art through the following technical improvement means, improves the comprehensive performance of the composite nickel film, and broadens its application field:
[0097] 1. Interface bonding technology between substrate and nickel layer: The bonding force between the substrate material and the nickel layer is enhanced through special surface pretreatment technology (such as plasma treatment and chemical etching), avoiding the delamination or shedding problems in complex environments or long-term use, and ensuring the long-term stability and durability of the composite film.
[0098] 2. Uniformity and precise thickness control of the nickel layer: Advanced sputtering or electroplating technology is used, and process parameters (such as power, time, gas pressure, etc.) are optimized to achieve uniform deposition and precise thickness control of the nickel layer, which is essential to ensure the conductivity and corrosion resistance of the composite film. At the same time, it meets the customized requirements of the nickel layer thickness in different application scenarios.
[0099] 3. Multilayer structure design and functionalization: Multilayer structures with specific functions are designed and implemented, such as combining different metal or alloy layers, or applying functional coatings on the surface of the nickel layer, which not only enhances the basic properties of the composite film, but also gives it additional functional properties, such as improving wear resistance, increasing self-cleaning ability or improving optical properties.
[0100] 4. Environmentally friendly preparation process: We have developed a green preparation method with low energy consumption and low pollution, which reduces the impact on the environment during the production process, while ensuring the high quality of the product and complying with the global requirements for sustainable development.
[0101] 5. Performance optimization and customization services: According to different application scenarios, the entire preparation process can be flexibly adjusted and optimized, providing full-chain customization services from substrate selection to surface treatment and metal layer deposition, ensuring that the composite nickel film can meet the special needs of specific industries or products.
[0102] The above-mentioned technical means work together to not only solve the shortcomings of traditional composite films in strength, conductivity, corrosion resistance and environmental adaptability, but also greatly improve the comprehensive performance and market competitiveness of composite nickel films, laying a solid foundation for its application in many high-tech fields.
[0103] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.
[0104] In the following examples, the preparation methods of the four homemade modified substrates (reinforced modified PI substrate, reinforced PET substrate, surface modified PI substrate, surface modified PET substrate) involved are as follows.
[0105] 1. Enhanced modified PI substrate
[0106] 1-1) adding 20 parts of pyromellitic anhydride, 10 parts of 4,4'-diaminodiphenyl ether, and 2 parts of 3,4'-diaminodiphenyl ether diglycidyl ether to 100 parts of N,N-dimethylformamide by weight, stirring and reacting for 24 hours under ice bath to obtain a prepolymer solution;
[0107] 1-2) After degassing, the prepolymer solution was uniformly coated on a clean glass substrate, and then heated to 250°C at a heating rate of 5°C / min, reacted for 3 hours, and finally the obtained film was completely removed from the glass substrate to obtain a reinforced modified PI substrate with a thickness of 25 μm.
[0108] 2. Enhanced PET substrate
[0109] 2-1) adding glass fibers with a diameter of 10 μm and a length of 5 mm into an ethanol solution of a silane coupling agent (specifically Dow Corning Z-6020) with a mass concentration of 1%, immersing at 50° C. for 2 hours, filtering, and drying to constant weight to obtain pretreated glass fibers; coating with a silane coupling agent to enhance its compatibility and adhesion with a PET substrate;
[0110] 2-2) 2-2) The pretreated glass fiber and PET resin (brand name: Eastman PETG 6763, provided by Eastman Chemical Company) were uniformly mixed in a mass ratio of 1:10, and melt-extruded at 200° C. through a twin-screw extruder to obtain a sheet;
[0111] 2-3) The extruded sheet was biaxially stretched at 120°C, with a longitudinal stretching ratio of 3 times and a transverse stretching ratio of 3 times. The product thickness after biaxial stretching was 25 μm, and then heat-set at 150°C, cooled, and rolled to obtain a reinforced PET substrate.
[0112] 3. Surface modified PI substrate
[0113] 3-1) The PI film with a thickness of 25 μm was treated with oxygen plasma, the power was set to 200 W, and the treatment time was 5 minutes; plasma treatment can clean the surface, remove organic pollutants, and increase the surface energy, which is beneficial to subsequent bonding;
[0114] 3-2) 3-aminopropyltriethoxysilane (brand name Dow Corning Z-6030, provided by Dow Corning) was added to anhydrous ethanol to prepare a silane coupling agent solution with a concentration of 1%. The silane coupling agent solution was evenly coated on the surface of the PI film obtained in step 3-1) to control the coating amount to 10 mg / m 2 (or coating thickness is 0.1 μm), and then cured at 140° C. for 30 min to obtain a surface-modified PI substrate.
[0115] 4. Surface modified PET substrate
[0116] 4-1) A PET substrate with a thickness of 50 μm was subjected to corona treatment, with the corona discharge power set to 1.5 kW and the treatment speed set to 1 m / min; free radicals were generated on the surface of the substrate through a high-energy electric field, thereby increasing the surface energy and polarity and enhancing the adhesion of subsequent coatings;
[0117] According to the previous description, we can supplement the specific solvent name, concentration of the silane coupling agent solution, coating amount and coating thickness in the preparation process of the surface-modified PET substrate in Example 20:
[0118] 4-2) 3-(triethoxysilyl)propylmethyldimethoxysilane (brand name Dow Corning Z-6040, provided by Dow Corning) was added to anhydrous ethanol to prepare a silane coupling agent solution with a concentration of 1%. The silane coupling agent solution was evenly coated on the surface of the PET substrate obtained in step 4-1) to control the coating amount to 10 mg / m 2 (or coating thickness is 0.1 μm), and then cured at 120° C. for 30 min to finally obtain a surface-modified PET substrate.
[0119] Anhydrous ethanol is a commonly used solvent for dissolving silane coupling agents and preparing solutions. A concentration of 1% is a typical ratio that can ensure the stability of the silane coupling agent solution and effectively coat it on the surface of the PET film. 2 A coating amount of 0.1 μm (or a coating thickness of 0.1 μm) is a reasonable value that can ensure the effectiveness of surface modification while avoiding potential problems caused by too thick a coating.
[0120] In the following embodiments, the test standards of the test items involved are as follows:
[0121] Corrosion resistance test: According to GB / T 10125-1997 (Chinese national standard) or ASTM G85 (American Society for Testing and Materials standard).
[0122] Hardness test: Follow ASTM D2240 (Shore hardness test method).
[0123] Tensile strength and elongation: in accordance with ISO 6892-1 (tensile test methods for metallic materials).
[0124] Friction coefficient: ASTM G99-577 or DIN 50329 and other related standards are adopted.
[0125] Brightness measurement: According to ASTM D4032 or relevant standards for specific application areas.
[0126] Example 1
[0127] A polymer film-based composite nickel film, the preparation method of which comprises the following steps:
[0128] S1. Substrate pretreatment:
[0129] The substrate surface was treated with oxygen plasma process, and the processing parameters were set as follows: power 50W, processing time 3 minutes, vacuum degree 10 -3 Torr to completely remove organic pollutants on the substrate surface and enhance surface activity; then ultraviolet light irradiation treatment for 1 minute to obtain a pretreated substrate.
[0130] S2. Preparing an intermediate bonding layer on the pretreated substrate:
[0131] S2-1, preparing adhesive solution:
[0132] Polyether polyol: Dow Corning DOWFAX TM 2A1, 50 parts by weight;
[0133] Isocyanate: Bayer Desmodur N 3300A, 45 parts by weight;
[0134] Solvent: ethyl acetate (analytical grade) was selected, 5 parts by weight;
[0135] Crosslinking agent: Dow Corning Z-6020, 3 parts by weight;
[0136] Catalyst: Dow Corning Z-6030 was selected, with a weight portion of 2 parts.
[0137] The components are uniformly mixed according to the above ratio to obtain a polyurethane prepolymer;
[0138] According to the weight ratio of tetrabutyl titanate (TBT) to polyurethane prepolymer being 1:100, tetrabutyl titanate is added to the polyurethane prepolymer and stirred evenly to obtain an adhesive solution;
[0139] S2-2. Use spin coating, dip coating or spray coating to ensure that the bonding layer is uniform and thin, avoiding the stress concentration problem caused by local excessive thickness; evenly apply the adhesive solution on the surface of the pretreated substrate, and cure it at 70-90°C for 15-60 minutes to form an intermediate bonding layer to ensure the stability and durability of the bonding layer.
[0140] S3, preparing a nickel metal layer on the intermediate bonding layer:
[0141] A DC magnetron sputtering process (a form of PVD) is used to deposit a nickel metal layer on the intermediate bonding layer. The process conditions are: a high-purity nickel target with a purity of ≥99.99% is used as the target material, argon is used as the working gas, the power is set to 100W, the gas pressure is 1Pa, and the sputtering time is 30 minutes.
[0142] S4. Electrodepositing a thickened nickel plating layer on the nickel metal layer to obtain a polymer film-based composite nickel film.
[0143] The substrate after the nickel metal layer is deposited obtained in step S3 is placed in an electroplating tank as a cathode, and a pure nickel plate is used as an anode to electroplatingly thicken the nickel-plated layer on the deposited nickel metal layer, and the electrolyte formula used is: nickel sulfate concentration is 200g / L, boric acid concentration is 30g / L, sodium chloride concentration is 10g / L, and nickel chloride concentration is 10g / L;
[0144] The electrodeposition process parameters are: current density is 10mA / cm 2 , the electrodeposition time was 1 hour, the pH value of the electrolyte was maintained at 4.5, and the temperature was controlled at 50°C.
[0145] In this embodiment, the thickness of the thickened nickel plating layer prepared by electrodeposition can reach about 5 μm.
[0146] Example 2-6 Coating process optimization experiment
[0147] In Examples 2-6, the only difference from Example 1 is that different coating processes are used to prepare the intermediate adhesive layer in step S2. Referring to Table 1, the coating processes of Examples 1-6 and the corresponding performance test results are shown.
[0148] Table 1
[0149]
[0150]
[0151] By comparing different coating processes, it was found that the process mode directly affects the surface quality and bonding strength of the composite film. Spray coating (Example 1) can obtain better overall performance. Dip coating (Example 2) is superior to spin coating (Example 1) in improving corrosion resistance and brightness, which is attributed to the fact that dip coating can cover the substrate more evenly and form a denser bonding layer. This finding emphasizes the role of coating process in improving the comprehensive performance of composite films.
[0152] After comparative analysis, spray coating was selected as the relatively optimal coating process. Spray coating process performs best in corrosion resistance, hardness, tensile strength and brightness, and it can better guarantee material performance compared to other coating methods.
[0153] Example 7-10 Sputtering process parameter optimization experiment
[0154] In Examples 7-10, the only difference from Example 1 is the magnetron sputtering process parameters in step S3. Referring to Table 2, the magnetron sputtering process parameters of Examples 1, 7-10 and the corresponding performance test results are shown.
[0155] Table 2
[0156]
[0157]
[0158] According to the test results in Table 2, it can be seen that slight changes in sputtering process parameters such as sputtering power, gas pressure, and deposition time significantly affect the structure and purity of the nickel layer, and thus affect the mechanical and electrical properties of the composite film. For example, increasing the sputtering power (Example 7) and gas pressure (Example 8) can improve corrosion resistance and hardness, but may be at the expense of ductility. This type of analysis emphasizes the importance of precise control of parameters during the sputtering process to achieve the best performance balance.
[0159] By comparative analysis, the relatively optimal sputtering process parameters are selected as follows:
[0160] Power: 100W, providing a stable and controllable sputtering process;
[0161] Gas pressure: 1Pa, to maintain sputtering efficiency and film quality;
[0162] Time: 30min. A longer sputtering time helps to form a denser metal layer and improve corrosion resistance and mechanical strength.
[0163] Example 11-13 Electroplating process parameter optimization experiment
[0164] In Examples 11-13, the only difference from Example 1 is the electroplating process parameters in step S4. Referring to Table 3, the electroplating process parameters of Examples 1, 11-13 and the corresponding performance test results are shown.
[0165] Table 3
[0166]
[0167] According to the experimental results, the adjustment of electroplating current density shows the ability to directly control the deposition rate, grain size and surface roughness. In Examples 11-13, although the gradual increase in current density accelerates the deposition rate, it may also cause grain coarsening, affecting the surface quality and mechanical properties. This set of data reveals that the current density selection needs to find the optimal balance between the deposition rate and the coating quality.
[0168] Comparative analysis shows that the relatively optimal electroplating current density is 10mA / cm 2 , ensuring uniform deposition and good bonding of the metal layer.
[0169] Example 14 Plating solution composition optimization experiment
[0170] In Example 14, the only difference from Example 1 is that NiCl2 is added to the electroplating solution. Referring to Table 4, the electroplating solution components of Examples 1 and 14 and the corresponding performance test results are shown.
[0171] Table 4
[0172]
[0173] The test results of Example 14 show that the optimization of the composition of the electroplating solution can significantly improve the comprehensive performance of the composite film. For example, by adding NiCl2 for concentration, both the corrosion resistance and the brightness are enhanced.
[0174] Through comparative analysis, the relatively optimal electroplating solution composition is selected as follows: nickel sulfate concentration is 200g / L, boric acid concentration is 30g / L, sodium chloride concentration is 10g / L, and nickel chloride concentration is 10g / L; adding NiCl2 for concentration further optimizes the electroplating solution composition and improves the hardness and wear resistance of the metal layer.
[0175] Examples 15-20 Substrate Optimization Experiments
[0176] In Examples 15-20, NiCl2 at a concentration of 10 g / L is added to the plating solution components. The only difference from Example 1 is the selection of different base materials. Refer to Table 5 for the base materials of Examples 1 and 15-20 and the corresponding performance test results.
[0177] Table 5
[0178]
[0179] According to the experimental results, different polymer film substrates (such as PI, PET, PVDF, reinforced modified PI, reinforced PET, surface modified PI, surface modified PET) have different effects on the comprehensive performance of the composite film. From the examples, each substrate material has its unique advantages: for example, the surface modified PET substrate may exhibit excellent corrosion resistance and brightness (Example 20), while the reinforced modified PI substrate (Example 17) may perform well in hardness and tensile strength. These results show that the choice of substrate material is crucial to the final performance of the composite film and needs to be optimized according to specific application requirements. According to comprehensive analysis,
[0180] Through comparative analysis, the relatively optimal substrate is surface-modified PET, which exhibits the best comprehensive performance, especially in terms of hardness, tensile strength, elongation, friction coefficient and brightness.
[0181] Based on the experimental results of Examples 1-20, the solution of Example 20 can be used as a relatively optimal choice. Its test results show excellent performance in all performance indicators, especially its ultra-high hardness and brightness, and low friction coefficient, making it an ideal choice for high-performance flexible electronic applications.
[0182] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A method for preparing a polymer film-based composite nickel film, characterized in that: The following steps are involved: S1, substrate pretreatment: the substrate surface is sequentially subjected to plasma treatment and ultraviolet irradiation treatment to obtain a pretreated substrate; S2, preparing an intermediate bonding layer on the pretreated substrate; S3, preparing a nickel metal layer on the intermediate bonding layer; S4, electro-depositing a thickened nickel-plated layer on the nickel metal layer to obtain a polymer film-based composite nickel film; The substrate is any one of a PI film, a reinforced modified PI substrate, a reinforced PET substrate, a surface modified PI substrate, and a surface modified PET substrate.
2. The method for preparing a polymer film-based composite nickel film according to claim 1, characterized in that: Step S1 is as follows: the surface of the substrate is treated by oxygen plasma process, and the treatment parameters are set as follows: power 50W, treatment time 3 minutes, vacuum degree 10 -3 Torr; then ultraviolet light irradiation treatment for 1 min to obtain a pretreated substrate.
3. The method for preparing a polymer film-based composite nickel film according to claim 1, characterized in that: Step S2 is specifically as follows: S2-1, preparing adhesive solution: By weight, 50 parts of polyether polyol, 45 parts of isocyanate, 5 parts of solvent, 3 parts of crosslinking agent and 2 parts of catalyst were mixed uniformly to obtain a polyurethane prepolymer; According to the weight ratio of tetrabutyl titanate to polyurethane prepolymer being 1:100, tetrabutyl titanate is added to the polyurethane prepolymer, and stirred evenly to obtain an adhesive solution; S2-2. Spin, dip or spray the adhesive solution evenly on the surface of the pretreated substrate, and cure it at 70-90°C for 15-60 minutes to form an intermediate adhesive layer.
4. The method for preparing a polymer film-based composite nickel film according to claim 1, characterized in that: Step S3 is specifically as follows: A nickel metal layer was deposited on the intermediate bonding layer using a DC magnetron sputtering process, and the process conditions were as follows: the working gas was argon, the power was set to 100 W, the gas pressure was 1 Pa, and the sputtering time was 30 minutes.
5. The method for preparing a polymer film-based composite nickel film according to claim 1, characterized in that: Step S4 is specifically as follows: The substrate after the nickel metal layer is deposited obtained in step S3 is used as a cathode, and a pure nickel plate is used as an anode to electro-deposit a thickened nickel plating layer on the deposited nickel metal layer, and the electrolyte formula used is: nickel sulfate concentration is 200g / L, boric acid concentration is 30g / L, sodium chloride concentration is 10g / L, and nickel chloride concentration is 10g / L; The electrodeposition process parameters are: current density is 10mA / cm 2 , the electrodeposition time was 1 hour, the pH value of the electrolyte was maintained at 4-5, and the temperature was controlled at 50°C.
6. The method for preparing a polymer film-based composite nickel film according to claim 1, characterized in that: The substrate is a reinforced modified PI substrate, which is prepared by the following method: 1-1) adding 20 parts of pyromellitic anhydride, 10 parts of 4,4'-diaminodiphenyl ether, and 2 parts of 3,4'-diaminodiphenyl ether diglycidyl ether to 100 parts of N,N-dimethylformamide by weight, stirring and reacting for 24 hours under ice bath to obtain a prepolymer solution; 1-2) After degassing, the prepolymer solution was uniformly coated on a clean glass substrate, and then heated to 250°C at a heating rate of 5°C / min, reacted for 3 hours, and finally the obtained film was completely removed from the glass substrate to obtain a reinforced modified PI substrate with a thickness of 25 μm.
7. The method for preparing a polymer film-based composite nickel film according to claim 1, characterized in that: The substrate is a reinforced PET substrate, which is prepared by the following method: 2-1) adding glass fiber into an ethanol solution of a silane coupling agent having a mass concentration of 1%, immersing the solution at 50° C. for 2 hours, filtering, and drying to a constant weight to obtain pretreated glass fiber; 2-2) mixing the pretreated glass fiber and the PET resin in a mass ratio of 1:10, and melt-extruded at 200° C. through a twin-screw extruder to obtain a sheet; 2-3) The extruded sheet was biaxially stretched at 120°C, with a longitudinal stretching ratio of 3 times and a transverse stretching ratio of 3 times. The product thickness after biaxial stretching was 25 μm, and then heat-set at 150°C, cooled, and rolled to obtain a reinforced PET substrate.
8. The method for preparing a polymer film-based composite nickel film according to claim 1, characterized in that: The substrate is a surface-modified PI substrate, which is prepared by the following method: 3-1) The PI film with a thickness of 25 μm was treated with oxygen plasma, the power was set to 200 W, and the treatment time was 5 minutes; 3-2) Add 3-aminopropyltriethoxysilane to anhydrous ethanol to prepare a silane coupling agent solution with a concentration of 1%, and evenly coat the silane coupling agent solution on the surface of the PI film obtained in step 3-1) to control the coating amount to 10 mg / m 2 , and then cured at 140 °C for 30 minutes to obtain a surface-modified PI substrate 9. The method for preparing a polymer film-based composite nickel film according to claim 1, characterized in that: The substrate is a surface-modified PET substrate, which is prepared by the following method: 4-1) A PET substrate with a thickness of 50 μm was subjected to corona treatment, with the corona discharge power set to 1.5 kW and the treatment speed set to 1 m / min; 4-2) 3-(triethoxysilyl)propylmethyldimethoxysilane was added to anhydrous ethanol to prepare a silane coupling agent solution with a concentration of 1%, and the silane coupling agent solution was evenly coated on the surface of the PET substrate obtained in step 4-1) to control the coating amount to 10 mg / m 2 , and then cured at 120°C for 30 minutes to finally obtain a surface-modified PET substrate.
10. A polymer film-based composite nickel film, characterized in that: It is prepared by the method according to any one of claims 1 to 9.