Bi-component adhesive with flame retardant property and preparation method thereof
By using polyether polyol, piperazine pyrophosphate and self-made GO-DPDO and PPy-Zn1-xYxB2O4 in polyurethane adhesives, the problems of poor flame retardant performance and reduced mechanical properties are solved, and efficient flame retardant and The improved mechanical properties solve the safety hazards and insufficient performance problems of polyurethane adhesives.
Patent Information
- Application Number
- CN202410968443.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-18
AI Technical Summary
After adding flame retardants to existing polyurethane adhesives, their flame retardant properties are poor and their mechanical properties are reduced. They are also easily flammable and release toxic smoke, posing safety risks.
A two-component adhesive is used, including component A and component B. Component A is composed of polyether polyol, rheology additive, defoaming agent, piperazine pyrophosphate, GO-DPDO and PPy-Zn1-xYxB2O4 , Component B is polymethyl polyphenyl isocyanate, and the flame retardant properties and mechanical properties are significantly improved through self-made GO-DPDO and PPy-Zn1-xYxB2O4.
The flame retardant performance and mechanical properties of the adhesive are significantly improved, with excellent performance and good market application prospects.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of adhesives, and more specifically, relates to a two-component adhesive with flame retardant properties and a preparation method thereof. Background Art
[0002] Polyurethane molecular chains contain isocyanate (-NCO) and carbamate (-NH-COO-), showing high activity and polarity. They have excellent chemical adhesion to substrates containing active hydrogen, such as porous materials such as foam, plastic, wood, leather, fabric, paper, ceramics, and smooth-surfaced materials such as metal, glass, rubber, and plastic. They are gradually gaining importance in the fields of aerospace, electronics, footwear, and furniture manufacturing.
[0003] The limiting oxygen index of polyurethane without flame retardant treatment is only about 18%, which is very easy to burn and releases a large amount of toxic smoke when burning, posing a threat to life safety. At present, in industrial production, it is usually improved by adding flame retardants to polyurethane, but there is a phenomenon that the compatibility of flame retardants with the matrix is poor, resulting in a decrease in mechanical properties, and there are also disadvantages such as short flame retardancy.
[0004] CN114958279A discloses a high-performance hybrid two-component polyurethane adhesive and its preparation method and application. Component A: includes polyester polyol, polyether polyol, and polyisocyanate. The present invention provides an adhesive, which is beneficial to the improvement of the molecular chain density of the cured film by using high molecular weight polyester polyol as the main component, and is hybridized by epoxy resin, which also promotes the improvement of heat resistance and impact strength. The type of suitable polyester polyol one is combined with relatively small molecular weight polyester polyol two and polyether polyol to adjust the flexibility of the molecule, and also promotes the improvement of impact strength. Its flexibility and impact strength are higher than similar products on the market, and the inventors have also found that by adding aromatic diisocyanate as a connection, it is more conducive to the arrangement of cross-linking density, while improving the coating performance and avoiding defects such as foreign bodies on the substrate.
[0005] CN118027878A discloses a polyurethane adhesive, the raw materials of which include: hydroxylated modified polyester, isocyanate compound, first catalyst and flame retardant; and the molar ratio of -OH functional group in hydroxylated modified polyester to -NCO functional group in isocyanate compound is 1:(2-20). The present invention constructs the polyurethane main chain structure with hydroxylated modified polyester, and obtains an adhesive with a three-dimensional network structure by adding excess isocyanate, and the structure contains both polyurethane segments and polyurea segments, and the stability, heat resistance, flame retardancy and mechanical strength are significantly improved.
[0006] CN118006281A discloses a polyurethane adhesive suitable for FFC that is resistant to moisture and heat aging without post-baking, including a main agent, a curing agent and other preparations. The main agent is composed of a saturated hydrolysis-resistant polyester resin, a phenolic epoxy resin, an acrylic block copolymer, a flame retardant, a matting powder and a catalyst. The curing agent adopts a flexible reaction curing agent that reacts with hydroxyl groups at room temperature. The components are respectively calculated by mass: 90 to 100 parts of hydrolysis-resistant polyester resin, 10 to 20 parts of phenolic epoxy resin, 5 to 9 parts of acrylic block copolymer, 60 to 70 parts of flame retardant, 1 to 5 parts of matting powder, 0.05 to 0.1 parts of catalyst, and 1.5 to 3.5 parts of flexible curing agent. When the polyurethane adhesive prepared by the present invention is applied to FFC (flexible flat cable), the product defects that may be caused by post-baking can be improved due to the absence of a post-baking process, and the cost can be effectively reduced, and it has high peel strength and aging resistance.
[0007] CN117551415A discloses a polyurethane adhesive and a preparation method thereof. The polyurethane adhesive is composed of a prepolymer component A and a curing agent component B. The prepolymer component A includes, by weight percentage, 7.2% to 28.5% of polyol 1, 37.5% to 70.0% of polyol 2, and 22.8% to 34.0% of isocyanate 1; the curing agent component B includes, by weight percentage, 54.1% to 59.6% of polyol 3, and 22.8% to 34.0% of isocyanate 2. 2.1%~4.3%, chain extender 35.6%~38.0%, leveling agent 2.1%~2.7%, antioxidant 0.6%~0.9%; the polyol 1 is a polytetramethylene ether polyol with a number average molecular weight of 250~650; the polyol 2 is a polytetramethylene ether polyol with a number average molecular weight of 1000~2000; the polyol 3 is a polytetramethylene ether polyol with a number average molecular weight of 1000~2000. The polyurethane adhesive of the present invention not only has high tensile strength and elongation, but also is more conducive to the packaging and bonding of complex electronic devices.
[0008] The flame retardant properties can be improved by adding flame retardant components to the adhesive, but the flame retardant properties are poor or the mechanical properties are reduced. The present invention provides a two-component adhesive with flame retardant properties, which has excellent flame retardant properties and mechanical properties. Summary of the invention
[0009] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art and provide a two-component adhesive with flame retardant properties and a preparation method thereof. The adhesive comprises the following components A and B; the mass ratio of the components A to B is 1.4-1.6:1; the raw materials and weight proportions of the components A are as follows: 100 parts of polyether polyol; 0.5-1.5 parts of rheological additive; 3-6 parts of defoaming agent; 0.1-0.3 parts of catalyst; 10-30 parts of piperazine pyrophosphate; 5-15 parts of GO-DPDO; PPy-Zn 1- x Y x B2O4, wherein x=0.02-0.04, 10-20 parts; the B component is polymethyl polyphenyl isocyanate. The present invention uses self-made GO-DPDO and PPy-Zn 1-x Y x B2O4, combined with piperazine pyrophosphate, significantly improved the flame retardant and mechanical properties of the adhesive.
[0010] The object of the present invention is to provide a two-component adhesive with flame retardant properties.
[0011] Another object of the present invention is to provide a method for preparing a two-component adhesive with flame retardant properties.
[0012] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0013] A two-component adhesive with flame retardant properties, comprising the following component A and component B; the mass ratio of the component A to the component B is 1.4-1.6:1;
[0014] The raw materials and weight proportions of the A component are as follows:
[0015] 100 parts of polyether polyol;
[0016] Rheological additive 0.5~1.5 parts;
[0017] 3~6 parts of defoaming agent;
[0018] Catalyst 0.1~0.3 parts;
[0019] 10-30 parts of piperazine pyrophosphate;
[0020] GO-DPDO 5~15 parts;
[0021] PPy-Zn 1-x Y x B2O4, where x = 0.02~0.04, 10~20 parts;
[0022] The B component is polymethyl polyphenyl isocyanate.
[0023] The preferred technical solution is that the preparation method of GO-DPDO comprises the following steps:
[0024] (1) Add triethylamine and 5',5-diallyl-2,2'-biphenol to a toluene solvent, stir evenly, then slowly drop phenylphosphonic acid dichloride, and then heat and reflux to react. Wash the turbid solution obtained by the reaction with deionized water until it is clear, then distill off the toluene, let it stand overnight, extract and filter, and vacuum dry to obtain DPDO;
[0025] (2) Add the DPDO, graphene oxide (GO) and AlCl3 obtained in step (1) to toluene, stir evenly, then react, cool to room temperature, filter, wash, and vacuum dry to obtain GO-DPDO.
[0026] Preferably, in step (1), the molar ratio of triethylamine, 5',5-diallyl-2,2'-biphenylene glycol and phenylphosphonic acid dichloride is 2:1:1; the conditions for the heating reflux reaction are: heating reflux reaction at 60-70°C for 10-14h; and the vacuum drying is vacuum drying at 80-90°C for 20-30h.
[0027] Preferably, in step (2), the mass ratio of DPDO, graphene oxide (GO) and AlCl3 is: 4-6:1:0.4-0.8; the reaction is carried out at 60-70°C for 20-30h; and the vacuum drying is carried out at 70-90°C for 10-16h.
[0028] The preferred technical solution is that the PPy-Zn 1-x Y x The preparation method of B2O4 comprises the following steps:
[0029] (1) Mix zinc oxide, yttrium oxide and boron oxide according to the ratio, grind and pass through a 300-500 mesh sieve, press into tablets, place in a muffle furnace for calcination, cool naturally, and then grind thoroughly to obtain Zn 1-x Y x B2O4;
[0030] (2) Zn obtained in step (1) 1-x Y x B2O4 was ultrasonically dispersed in ethanol water to obtain a dispersion, and then pyrrole was added to the above dispersion, stirred for 20-40 min, and then ferric chloride solution was added dropwise, stirred at room temperature for 20-30 h, filtered, and vacuum dried to obtain PPy-Zn 1-x Y x B2O4.
[0031] Preferably, in step (1), the calcination is carried out by heating the temperature to 950-1050°C at a rate of 1°C / min and keeping the temperature for 16-24h.
[0032] Preferably, in step (2), the Zn 1-x Y x The ratio of B2O4 to pyrrole is: 25~35g:1mL; the volume ratio of the pyrrole to the ferric chloride solution is: 1:300; the concentration of the ferric chloride solution is 30g / L; the vacuum drying is vacuum drying at 50~70°C for 10~20h.
[0033] According to a preferred technical solution, the polyether polyol is polyether polyol 4110; the rheological additive is BYK-410; the defoamer is BYK-028; and the catalyst is dibutyltin diacetate.
[0034] Based on the above-mentioned method for preparing a two-component adhesive with flame retardant properties, the preparation method comprises the following steps:
[0035] The polyether polyol, rheological additive, defoamer and catalyst were stirred and mixed, and then piperazine pyrophosphate, GO-DPDO and PPy-Zn were added. 1-x Y x B2O4, then stir at 400~600rpm for 10~20min, and carry out vacuum degassing in a vacuum degassing machine with a vacuum degree of -50~-90 kPa and a degassing time of 10~30 min to obtain component A; component B is multi-methyl polyphenyl isocyanate.
[0036] Preferably, the stirring speed during the uniform stirring process is 200-300 rpm, and the stirring time is 3-7 min.
[0037] The present invention has the following beneficial effects:
[0038] Modification of GO by DPDO not only improves the dispersibility of GO, but also introduces the flame retardant element P, which significantly improves the flame retardant efficiency. 1-x Y x B2O4 can improve the flame retardant component Zn 1-x Y x The dispersibility of B2O4, combined with piperazine pyrophosphate, significantly improves the flame retardant properties of the adhesive, and also improves the mechanical properties. It has excellent performance and good market application prospects. DETAILED DESCRIPTION
[0039] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0040] The polyether polyol is polyether polyol 4110; the rheological additive is BYK-410; the defoamer is BYK-028; the catalyst is dibutyltin diacetate; polymethyl polyphenyl isocyanate, PM-200, Wanhua.
[0041] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0042] Example 1
[0043] A two-component adhesive with flame retardant properties, comprising the following component A and component B; the mass ratio of the component A to the component B is 1.5:1;
[0044] The raw materials and weight proportions of the A component are as follows:
[0045] 100 parts of polyether polyol;
[0046] 1 part of rheological additive;
[0047] 5 parts of defoaming agent;
[0048] 0.2 parts of catalyst;
[0049] 20 parts of piperazine pyrophosphate;
[0050] GO-DPDO 10 parts;
[0051] PPy-Zn 0.97 Y 0.03 B2O4, 15 parts;
[0052] The B component is polymethyl polyphenyl isocyanate;
[0053] The preparation method of GO-DPDO comprises the following steps:
[0054] (1) Add 2 mol of triethylamine and 1 mol of 5',5-diallyl-2,2'-biphenol to 200 mL of toluene solvent, stir evenly, then slowly dropwise add 1 mol of phenylphosphonic acid dichloride, and then heat under reflux at 65°C for 12 h. Wash the turbid solution obtained by the reaction with deionized water until it is clear, then distill off the toluene, let it stand overnight, extract and filter, and vacuum dry at 85°C for 26 h to obtain DPDO;
[0055] (2) 5 g of DPDO obtained in step (1), 1 g of graphene oxide (GO) and 0.6 g of AlCl3 were added to toluene, stirred evenly, and then reacted at 65°C for 25 h. The mixture was cooled to room temperature, filtered, washed, and vacuum dried at 80°C for 14 h to obtain GO-DPDO.
[0056] The PPy-Zn 0.97 Y 0.03 The preparation method of B2O4 comprises the following steps:
[0057] (1) Zinc oxide, yttrium oxide and boron oxide were mixed in an atomic ratio of 0.97:0.03:2, then ground and passed through a 400-mesh sieve, and then pressed into tablets and placed in a muffle furnace. The temperature was raised to 1000°C at a rate of 1°C / min and kept at that temperature for 20 hours, then naturally cooled, and then fully ground to obtain Zn 0.97 Y 0.03 B2O4;
[0058] (2) 30 g of Zn obtained in step (1) was added 0.97 Y 0.03 B2O4 was ultrasonically dispersed in 150 mL of ethanol water (the volume ratio of ethanol to water was 1:1) to obtain a dispersion, and then pyrrole was added to the above dispersion, stirred for 30 min, and then 300 mL of 30 g / L ferric chloride solution was added dropwise, stirred at room temperature for 25 h, filtered, and vacuum dried at 60 ° C for 16 h to obtain PPy-Zn 0.97 Y 0.03 B2O4.
[0059] A method for preparing a two-component adhesive with flame retardant properties, the preparation method comprising the following steps:
[0060] The polyether polyol, rheological additive, defoamer and catalyst were stirred and mixed at a stirring speed of 250 rpm for 5 min; then piperazine pyrophosphate, GO-DPDO and PPy-Zn 0.97 Y 0.03 B2O4, then stirred at 500rpm for 15min, the mixed materials were vacuum degassed in a vacuum degasser with a vacuum degree of -70 kPa and a degassing time of 20min to obtain component A; component B was polymethyl polyphenyl isocyanate.
[0061] Example 2
[0062] A two-component adhesive with flame retardant properties, comprising the following component A and component B; the mass ratio of the component A to the component B is 1.4:1;
[0063] The raw materials and weight proportions of the A component are as follows:
[0064] 100 parts of polyether polyol;
[0065] 1.5 parts of rheological additive;
[0066] 3 parts of defoaming agent;
[0067] 0.3 parts of catalyst;
[0068] 10 parts of piperazine pyrophosphate;
[0069] GO-DPDO 15 parts;
[0070] PPy-Zn 0.96 Y 0.04 B2O4, 10 parts;
[0071] The B component is polymethyl polyphenyl isocyanate;
[0072] The preparation method of GO-DPDO comprises the following steps:
[0073] (1) Add 2 mol of triethylamine and 1 mol of 5',5-diallyl-2,2'-biphenol to 200 mL of toluene solvent, stir evenly, then slowly drop 1 mol of phenylphosphonic acid dichloride, and then heat under reflux at 70°C for 10 h. Wash the turbid solution obtained by the reaction with deionized water until it is clear, then distill off the toluene, let it stand overnight, extract and filter, and vacuum dry at 90°C for 20 h to obtain DPDO;
[0074] (2) 6 g of DPDO obtained in step (1), 1 g of graphene oxide (GO) and 0.8 g of AlCl3 were added to toluene, stirred evenly, and then reacted at 70°C for 20 h. The mixture was cooled to room temperature, filtered, washed, and vacuum dried at 90°C for 10 h to obtain GO-DPDO.
[0075] The PPy-Zn 0.96 Y 0.04 The preparation method of B2O4 comprises the following steps:
[0076] (1) Zinc oxide, yttrium oxide and boron oxide were mixed in an atomic ratio of 0.96:0.04:2, then ground and passed through a 500-mesh sieve, and then pressed into a tablet and placed in a muffle furnace. The temperature was raised to 1050°C at 1°C / min and kept at this temperature for 16 hours, then naturally cooled and fully ground to obtain Zn 0.96 Y 0.04 B2O4;
[0077] (2) 35 g of Zn obtained in step (1) 0.96 Y 0.04B2O4 was ultrasonically dispersed in 150 mL of ethanol water (the volume ratio of ethanol to water was 1:1) to obtain a dispersion, and then 1 mL of pyrrole was added to the above dispersion, stirred for 40 min, and then 300 mL of 30 g / L ferric chloride solution was added dropwise, stirred at room temperature for 30 h, filtered, and vacuum dried at 70 °C for 10 h to obtain PPy-Zn 0.96 Y 0.04 B2O4.
[0078] The preparation method of a two-component adhesive with flame retardant properties is the same as that of Example 1.
[0079] Example 3
[0080] A two-component adhesive with flame retardant properties, comprising the following component A and component B; the mass ratio of the component A to the component B is 1.6:1;
[0081] The raw materials and weight proportions of the A component are as follows:
[0082] 100 parts of polyether polyol;
[0083] 0.5 parts of rheological additive;
[0084] 6 parts of defoaming agent;
[0085] 0.1 part of catalyst;
[0086] 30 parts of piperazine pyrophosphate;
[0087] GO-DPDO 5 parts;
[0088] PPy-Zn 0.98 Y 0.02 B2O4, 20 parts;
[0089] The B component is polymethyl polyphenyl isocyanate;
[0090] The preparation method of GO-DPDO comprises the following steps:
[0091] (1) Add 2 mol of triethylamine and 1 mol of 5',5-diallyl-2,2'-biphenol to 200 mL of toluene solvent, stir evenly, then slowly drop 1 mol of phenylphosphonic acid dichloride, and then heat under reflux at 60°C for 14 h. Wash the turbid solution obtained by the reaction with deionized water until it is clear, then distill off the toluene, let it stand overnight, extract and filter, and vacuum dry at 80°C for 30 h to obtain DPDO;
[0092] (2) 4 g of DPDO obtained in step (1), 1 g of graphene oxide (GO) and 0.4 g of AlCl3 were added to toluene, stirred evenly, and then reacted at 60°C for 30 h, cooled to room temperature, filtered, washed, and vacuum dried at 70°C for 16 h to obtain GO-DPDO.
[0093] The PPy-Zn 0.98 Y 0.02 The preparation method of B2O4 comprises the following steps:
[0094] (1) Zinc oxide, yttrium oxide and boron oxide were mixed in an atomic ratio of 0.98:0.02:2, then ground and passed through a 300-mesh sieve, and then pressed into tablets and placed in a muffle furnace. The temperature was raised to 950°C at a rate of 1°C / min and kept at this temperature for 24 hours, then naturally cooled and fully ground to obtain Zn 0.98 Y 0.02 B2O4;
[0095] (2) Zn obtained in step (1) 0.98 Y 0.02 B2O4 was ultrasonically dispersed in 150 mL of ethanol water (the volume ratio of ethanol to water was 1:1) to obtain a dispersion, and then 1 mL of pyrrole was added to the above dispersion, stirred for 20 min, and then 300 mL of 30 g / L ferric chloride solution was added dropwise, stirred at room temperature for 20 h, filtered, and vacuum dried at 50 °C for 20 h to obtain PPy-Zn 0.98 Y 0.02 B2O4.
[0096] The preparation method of a two-component adhesive with flame retardant properties is the same as that of Example 1.
[0097] Comparative Example 1
[0098] Comparative Example 1 is basically the same as Example 1, except that an equal amount of PPy-ZnB2O4 is used to replace PPy-Zn 0.97 Y 0.03 B2O4. The preparation method of PPy-ZnB2O4 comprises the following steps:
[0099] (1) Mix zinc oxide and boron oxide in an atomic ratio of 1:2, grind and pass through a 400-mesh sieve, press into tablets and place in a muffle furnace, heat to 1000°C at 1°C / min and keep at this temperature for 20 hours, then cool naturally and grind thoroughly to obtain ZnB2O4;
[0100] (2) 30 g of the ZnB2O4 obtained in step (1) was ultrasonically dispersed in 150 mL of ethanol water (the volume ratio of ethanol to water was 1:1) to obtain a dispersion, and then pyrrole was added to the above dispersion, stirred for 30 min, and then 300 mL of 30 g / L ferric chloride solution was dropwise added, stirred at room temperature for 25 h, filtered, and vacuum dried at 60 ° C for 16 h to obtain PPy-ZnB2O4.
[0101] Comparative Example 2
[0102] Comparative Example 2 is basically the same as Example 1, except that an equal amount of Zn 0.97 Y 0.03 B2O4 replaces PPy-Zn 0.97 Y 0.03 B2O4. Zn 0.97 Y 0.03 The preparation method of B2O4 comprises the following steps: mixing zinc oxide, yttrium oxide and boron oxide according to the atomic ratio of 0.97:0.03:2, then grinding and passing through a 400-mesh sieve, then pressing into tablets and placing them in a muffle furnace, heating to 1000°C at 1°C / min and keeping the temperature for 20 hours, then cooling naturally, and then fully grinding to obtain Zn 0.97 Y 0.03 B2O4.
[0103] Comparative Example 3
[0104] Comparative Example 3 is substantially the same as Example 1, except that an equal amount of GO is used to replace GO-DPDO.
[0105] Comparative Example 4
[0106] Comparative Example 4 is substantially the same as Example 1, except that an equal amount of piperazine pyrophosphate is used to replace GO-DPDO.
[0107] Comparative Example 5
[0108] Comparative Example 5 is basically the same as Example 1, except that an equal amount of PPy-Zn 0.97 Y 0.03 B2O4 replaces GO-DPDO.
[0109] The performance of Examples 1-3 and Comparative Examples 1-5 was tested. The specific test results are shown in Table 1:
[0110] Among them, shear strength: tested using GB / T 7124-2008
[0111] Limiting oxygen index%: Tested according to GB / T 2406.2-2009
[0112] Table 1
[0113] Shear strength (MPa) Limiting oxygen index (%) Example 1 5.3 40.2 Example 2 4.9 38.9 Example 3 5.2 39.4 Comparative Example 1 - 38.2 Comparative Example 2 4.6 37.7 Comparative Example 3 4.4 38.4 Comparative Example 4 - 35.4 Comparative Example 5 3.9 36.2
[0114] It can be seen from Table 1 that the flame retardant two-component adhesive prepared by the present invention has excellent shear strength and flame retardant properties. By comparing Example 1 with Comparative Examples 1-5, it can be seen that by modifying GO with DPDO, not only the dispersibility of GO is improved, but also the flame retardant element P is introduced, which significantly improves the flame retardant efficiency. 1-x Y x B2O4 can improve the flame retardant component Zn 1-x Y x The dispersibility of B2O4, combined with piperazine pyrophosphate, significantly improves the flame retardant properties of the adhesive, and also improves the mechanical properties, with excellent performance.
[0115] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A two-component adhesive with flame retardant properties, characterized in that: It comprises the following component A and component B; the mass ratio of the component A to the component B is 1.4-1.6:1; The raw materials and weight proportions of the A component are as follows: 100 parts of polyether polyol; Rheological additive 0.5~1.5 parts; 3~6 parts of defoaming agent; Catalyst 0.1~0.3 parts; 10-30 parts of piperazine pyrophosphate; GO-DPDO 5~15 parts; PPy-Zn 1-x Y x B2O4, where x = 0.02~0.04, 10~20 parts; The B component is polymethyl polyphenyl isocyanate.
2. The two-component adhesive with flame retardant properties according to claim 1, characterized in that: The preparation method of GO-DPDO comprises the following steps: (1) Add triethylamine and 5',5-diallyl-2,2'-biphenol to a toluene solvent, stir evenly, then slowly drop phenylphosphonic acid dichloride, and then heat and reflux to react. Wash the turbid solution obtained by the reaction with deionized water until it is clear, then distill off the toluene, let it stand overnight, extract and filter, and vacuum dry to obtain DPDO; (2) Add the DPDO, graphene oxide (GO) and AlCl3 obtained in step (1) to toluene, stir evenly, then react, cool to room temperature, filter, wash, and vacuum dry to obtain GO-DPDO.
3. The two-component adhesive with flame retardant properties according to claim 2, characterized in that: In step (1), the molar ratio of triethylamine, 5',5-diallyl-2,2'-biphenylphenol and phenylphosphonic acid dichloride is 2:1:1; the heating reflux reaction conditions are: heating reflux reaction at 60-70°C for 10-14h; the vacuum drying is vacuum drying at 80-90°C for 20-30h.
4. The two-component adhesive with flame retardant properties according to claim 2, characterized in that: In step (2), the mass ratio of DPDO, graphene oxide (GO) and AlCl3 is: 4-6:1:0.4-0.8; the reaction is carried out at 60-70°C for 20-30h; and the vacuum drying is carried out at 70-90°C for 10-16h.
5. The two-component adhesive with flame retardant properties according to claim 1, characterized in that: The PPy-Zn 1-x Y x The preparation method of B2O4 comprises the following steps: (1) Mix zinc oxide, yttrium oxide and boron oxide according to the ratio, grind and pass through a 300-500 mesh sieve, press into tablets, place in a muffle furnace for calcination, cool naturally, and then grind thoroughly to obtain Zn 1-x Y x B2O4; (2) Zn obtained in step (1) 1-x Y x B2O4 was ultrasonically dispersed in ethanol water to obtain a dispersion, and then pyrrole was added to the above dispersion, stirred for 20-40 min, and then ferric chloride solution was added dropwise, stirred at room temperature for 20-30 h, filtered, and vacuum dried to obtain PPy-Zn 1-x Y x B2O4.
6. The two-component adhesive with flame retardant properties according to claim 5, characterized in that: In step (1), the calcination is performed by heating the temperature to 950-1050°C at a rate of 1°C / min and keeping the temperature for 16-24 hours.
7. The two-component adhesive with flame retardant properties according to claim 5, characterized in that: In step (2), the Zn 1-x Y x The ratio of B2O4 to pyrrole is: 25~35g:1mL; the volume ratio of the pyrrole to the ferric chloride solution is: 1:300; the concentration of the ferric chloride solution is 30g / L; the vacuum drying is vacuum drying at 50~70°C for 10~20h.
8. The two-component adhesive with flame retardant properties according to claim 1, characterized in that: The polyether polyol is polyether polyol 4110; the molecular weight is 300-500; the rheological additive is BYK-410; the defoamer is BYK-028; and the catalyst is dibutyltin diacetate.
9. A method for preparing a two-component adhesive with flame retardant properties according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: The polyether polyol, rheological additive, defoamer and catalyst were stirred and mixed, and then piperazine pyrophosphate, GO-DPDO and PPy-Zn were added. 1-x Y x B2O4, then stir at 400~600rpm for 10~20min, and carry out vacuum degassing in a vacuum degassing machine with a vacuum degree of -50~-90 kPa and a degassing time of 10~30 min to obtain component A; component B is multi-methyl polyphenyl isocyanate.
10. The method for preparing a two-component adhesive with flame retardancy according to claim 9, characterized in that: The stirring speed during the uniform stirring process is 200-300 rpm, and the stirring time is 3-7 min.
Citation Information
Cited By