Preparation method of direct coal liquefaction circulating solvent
By using Ni-W and Ni-Mo or Ni-Mo-W catalysts in fixed-bed and ebullating-bed reactors respectively for hydrogenation reactions, the problems of high hydrogen consumption and harsh reaction conditions in the preparation of circulating solvents for direct liquefaction of coal are solved. Improved hydrogen supply performance and process stability.
Patent Information
- Application Number
- CN202410870862.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The preparation method of circulating solvent for direct liquefaction of coal has problems such as high hydrogen consumption, harsh reaction conditions, and difficulty in controlling the depth of hydrogenation, which affects hydrogen supply performance and process stability.
Hydrogenation of light fractions using Ni-W catalysts in fixed-bed reactors and heavy fractions using Ni-Mo or Ni-Mo-W catalysts in ebullating-bed reactors with forced circulation Reaction, medium-temperature and high-temperature solvents are obtained through separation, and a circulating solvent with excellent hydrogen supply performance is synthesized.
It effectively avoids the problems of excessive hydrogenation of light fractions and insufficient hydrogenation of heavy fractions, improves the hydrogen supply performance of the circulating solvent, reduces N, O, and S contents, and ensures long-term stable operation of the process.
Smart Images

Figure CN118792073A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of direct coal liquefaction, further to the technical field of hydrogenation catalyst for direct coal liquefaction circulating solvent, and specifically to a method for preparing direct coal liquefaction circulating solvent. Background Art
[0002] The direct liquefaction process of coal is essentially a process of pyrolysis and hydrogenation of the unsaturated macromolecular structure of coal. The hydrogen supply solvent plays an important role in dissolving and dispersing coal and transferring hydrogen, thereby promoting the hydrogenation and liquefaction of coal. In addition to the physical effects of dissolving, swelling, diluting, and dispersing coal powder solids, improving the transportation performance and thermodynamic properties of materials, the solvent also has a good hydrogen supply and transfer function. The hydrogen supply performance of the solvent is very important for easing the reaction conditions and improving the oil yield of direct coal liquefaction.
[0003] During the continuous operation of the coal direct liquefaction unit, the actual solvent used is a mixed oil of the middle distillate and the heavy distillate produced by the coal direct liquefaction unit, which is recycled through catalytic hydrogenation treatment and is called the circulating solvent. The aromatic composition of the hydrogen supply solvent for coal direct liquefaction is very complex, among which the bicyclic, tricyclic and polycyclic partially saturated hydrogenated aromatic compounds have good hydrogen supply performance. In order to improve the hydrogen supply capacity of solvent oil, a common method is to subject the circulating solvent to moderate hydrogenation treatment.
[0004] The processing characteristics of the circulating solvent of the Japanese NEDOL process are that the coal liquefaction oil produced by the coal liquefaction unit is used as the feed of the hydrogenation unit after distillation, and the hydrogenation unit uses Ni-Mo catalyst. The processing characteristics of the circulating solvent of the China Shenhua coal direct liquefaction process (authorization announcement number is CN1257252C) are that the full-fraction coal liquefaction oil produced by the coal liquefaction unit is used as the feed of the hydrogenation unit, the heavy distillate oil cut out by fractionation is used as the circulating solvent, and the hydrogenation unit uses Ni-Mo catalyst. The Chinese patent application with publication number CN1844318A discloses a hydrogenation process of a lignite direct liquefaction circulating solvent, and provides a catalyst grading technology for the hydrogenation process of the coal direct liquefaction full-fraction oil, and obtains a hydrogen supply circulating solvent under appropriate chemical reaction conditions. The patent with publication number CN 104194830 first fractionates the coal direct liquefaction oil, selectively cuts the heavy oil fraction therein, and then hydrogenates and stabilizes the heavy oil with a narrower fraction, thereby obtaining a coal direct liquefaction circulating solvent with better hydrogen supply performance. The patent with publication number CN109852419A performs catalytic hydrogenation on coal direct liquefaction oil to obtain hydrogenated oil; then fractionates the hydrogenated oil to obtain light distillate oil, middle distillate oil and heavy distillate oil; returns part of the heavy distillate oil and mixes it with coal direct liquefaction oil for catalytic hydrogenation; finally, mixes another part of the heavy distillate oil with part of the middle distillate oil to form a coal liquefaction circulating solvent. The patent with publication number CN104910961A performs a first catalytic hydrogenation on coal direct liquefaction oil, fractionates the first liquid phase product to obtain light distillate oil, middle distillate oil and heavy distillate oil; performs a second catalytic hydrogenation on part or all of the heavy distillate oil to obtain a second liquid phase product; finally, mixes the second liquid phase product with part or all of the middle distillate oil to form a coal direct liquefaction circulating hydrogen supply solvent.
[0005] At present, the preparation method of circulating solvent for direct coal liquefaction has technical problems such as high hydrogen consumption, harsh reaction conditions, and difficulty in controlling the hydrogenation depth of solvent oils of different fractions. Therefore, research and improvement on the processing methods of existing circulating solvents and the preparation technology of hydrogenation catalysts remains a hot topic in this research field. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a method for preparing a circulating solvent for direct coal liquefaction. The preparation method of the present invention is used to carry out a hydrogenation reaction of a light fraction under the action of a first catalyst in a fixed bed reactor, and to carry out a hydrogenation reaction of a heavy fraction under the action of a second catalyst in an ebullating bed reactor with forced circulation, which is conducive to obtaining a circulating solvent with good hydrogen supply performance. During the hydrogenation process, the first catalyst used has good hydrogenation performance and high selectivity for hydrogenated aromatics; the second catalyst used has high denitrification, deoxygenation, and dearomatization performance, good mechanical properties, and strong resistance to metal deposition and coking, which is conducive to the long-term stable operation of the process.
[0007] To achieve the purpose, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a circulating solvent for direct coal liquefaction, comprising the following steps:
[0009] (1) subjecting a light fraction having a distillation range of 200 to 300° C. to a first hydrogenation reaction in a fixed bed reactor in the presence of a first catalyst to obtain a first hydrogenated stabilized oil;
[0010] subjecting the heavy fraction with a distillation range of more than 300° C. to a second hydrogenation reaction in an ebullating bed reactor with forced circulation in the presence of a second catalyst to obtain a second hydrogenated stable oil;
[0011] (2) mixing the first hydrogenated stabilized oil and the second hydrogenated stabilized oil, and separating and fractionating them to obtain a medium-temperature solvent and a high-temperature solvent;
[0012] (3) mixing the medium-temperature solvent and the high-temperature solvent to prepare the circulating solvent;
[0013] The first catalyst comprises a first carrier and a first active metal element, wherein the first active metal element comprises Ni and W; in the first catalyst, nickel oxide accounts for 0.1-10wt%, dextrin accounts for 5-40wt%, and the remainder is the first carrier; and the ratio of the amount of Ni element to the sum of the amounts of Ni element and W element is 0.1-0.4;
[0014] The second catalyst includes a second carrier and a second active metal element, wherein the second active metal element includes Ni and Mo, and optionally includes W; in the second catalyst, nickel oxide accounts for 0.1-10wt%, molybdenum oxide accounts for 10-40wt%, tungsten oxide accounts for 0-15wt%, and the balance is the second carrier.
[0015] Preferably, in the first catalyst, nickel oxide accounts for 1-6wt% (e.g., 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, etc.), and dock oxide accounts for 10-25wt% (e.g., 10wt%, 15wt%, 20wt%, 25wt%, etc.);
[0016] In the second catalyst, nickel oxide accounts for 2-6wt% (for example, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, etc.); molybdenum oxide accounts for 15-30wt% (for example, 15wt%, 20wt%, 25wt%, 30wt%, etc.); preferably, tungsten oxide accounts for 2-15wt% (for example, 2wt%, 8wt%, 10wt%, 15wt%, etc.).
[0017] Preferably, the first catalyst has a maximum pore size in the range of 5-20 nm, preferably 8-15 nm; and a specific surface area in the range of 200-400 m 2 / g, and the pore volume is preferably 0.35-0.9cm 3 / g;
[0018] The second catalyst has a bimodal pore structure, the most probable pore size range of the small pores is 2-15nm, preferably 5-10nm; the most probable pore size range of the large pores is 20-80nm, preferably 30-50nm; the specific surface area is 200-400m 2 / g, pore volume is 0.35-0.9cm 3 / g; the pore volume of small pores with a pore diameter of 5-10nm accounts for 20-60% of the total pore volume, and the pore volume of large pores with a pore diameter of 30-50nm accounts for 20-50% of the total pore volume.
[0019] Further, the first carrier is selected from one or more of alumina, silicon oxide, amorphous silica-alumina, SBA-15, preferably the first carrier is a carrier modified by a modifying metal; the modifying metal is selected from one or more of alkali metal elements and alkaline earth metal elements, preferably the modifying metal is selected from one or more of Li, K, Na, Mg, Ca;
[0020] Preferably, in the first carrier, the content of the modified metal oxide is 0.1-8wt%, for example, 0.1wt%, 0.5wt%, 1wt%, 3wt%, 5wt%, 8wt% and the like.
[0021] Preferably, the preparation step of the first catalyst comprises:
[0022] S1a: mixing the dry rubber powder, sesbania powder and citric acid uniformly, then adding nitric acid solution to knead uniformly and shape, drying and calcining, the calcination temperature is preferably 500-800° C., and the calcination time is preferably 3-10 hours, to obtain the first carrier; preferably, the solution of the modified metal salt is also added during the mixing process;
[0023] S2a: impregnating the precursor solution of the first active metal element onto the first carrier obtained in step S1a, drying and calcining, wherein the calcination temperature is preferably 500-600° C. and the calcination time is preferably 3-10 h, to obtain the first catalyst.
[0024] Further, the second carrier is selected from one or more of aluminum oxide, amorphous silicon aluminum, silicon oxide, zirconium oxide, magnesium oxide and titanium oxide;
[0025] Preferably, the second carrier is selected from alumina, and the alumina is selected from γ-AL 2 O 3,δ-AL 2 O 3 ,θ-AL 2 O 3 ,η-AL 2 O 3 One or more of;
[0026] Further preferably, the second carrier comprises γ-AL 2 O 3 , including δ-AL 2 O 3 and / or θ-AL 2 O 3 , the γ-AL 2 O 3 The mass of the δ-AL 2 O 3 and the θ-AL 2 O 3 The ratio of the sum of the masses of the two is 1:1-9:1, for example 1:1, 2:1, 4:1, 6:1, 7:1, 9:1, etc.
[0027] Preferably, the second carrier contains auxiliary elements, and the auxiliary elements include one or more of Si, P, B, Zr, and Ti;
[0028] Preferably, in the second carrier, the mass content of the oxide of the auxiliary element is 0.1-8wt%, for example, 0.1wt%, 0.5wt%, 1wt%, 3wt%, 5wt%, 8wt% and the like.
[0029] Preferably, the preparation step of the second catalyst comprises:
[0030] S1b: uniformly mixing the dry rubber powder with sesbania powder, citric acid and pore-enlarging agent, then adding nitric acid solution, kneading and forming, drying and calcining, the calcination temperature is preferably 500-1000° C., and the calcination time is preferably 3-10 hours, to obtain the second carrier; preferably, the precursor of the auxiliary element is also added during the uniform mixing process;
[0031] Preferably, after the drying, the dried material is divided into two parts with a mass ratio of 1:1-9:1, one part is calcined at 500-800°C for 3-10h, and the other part is calcined at >800°C and ≤1000°C for 3-10h, and then the two parts of the carrier obtained by calcination are mixed as the second carrier;
[0032] S2b: impregnating the impregnation solution on the second carrier, drying and calcining, the calcination temperature is preferably 500-600° C., and the calcination time is preferably 3-10 hours, to obtain the second catalyst; the impregnation solution is a solution including a salt of the second active metal element;
[0033] Preferably, in step S1b, the pore expanding agent is selected from one or more of carbon black, polyethylene glycol, ammonium carbonate, silica sol, and cellulose; the amount of the pore expanding agent is 0.5%-10% of the mass of the dry rubber powder, preferably 1%-5%.
[0034] Furthermore, the conditions of the first hydrogenation reaction include: pressure of 8-16 MPa, temperature of 300-360°C, hydrogen-to-oil ratio of 400-1000 v / v, reaction volume space velocity of 0.5-3.5 h -1 ;
[0035] And / or, the conditions of the second hydrogenation reaction include: pressure of 10-19 MPa, temperature of 320-380°C, hydrogen-to-oil ratio of 200-800 v / v, reaction volume space velocity of 1.0-3.5 h -1 ;
[0036] And / or, in step (1), the light fraction and the heavy fraction are obtained by fractionating the whole fraction oil obtained by direct coal liquefaction reaction.
[0037] Further, in step (2), the distillation range of the medium-temperature solvent is 220-320°C, and the distillation range of the high-temperature solvent is 320-500°C; or, the distillation range of the medium-temperature solvent is 200-300°C, and the distillation range of the high-temperature solvent is 300-480°C;
[0038] Preferably, in step (3), the mass ratio of the medium-temperature solvent to the high-temperature solvent is 5:1 to 4:2, for example, 5:1, 4:1, 3:1, 2:1, etc., preferably 4:1 to 6:2.
[0039] The technical solution provided by the present invention has the following beneficial effects:
[0040] (1) The preparation method of the present invention is used to hydrogenate the light fraction using a specific Ni-W catalyst and the heavy fraction using a specific Ni-Mo or Ni-Mo-W catalyst in a fixed bed reactor and an ebullating bed reactor with forced circulation, respectively. This is not only beneficial to avoid problems such as excessive hydrogenation of the light fraction and insufficient hydrogenation of the heavy fraction, but also beneficial to ultimately obtain a circulating solvent with good hydrogen supply performance.
[0041] (2) In the preferred embodiment, a first catalyst having specific pore structure and other apparent characteristics is used for the hydrogenation catalysis of light fractions in a fixed bed, and a second catalyst having specific pore structure and other apparent characteristics is used for the hydrogenation catalysis of heavy fractions in an ebullating bed reactor with forced circulation, which is ultimately conducive to obtaining a circulating solvent with better hydrogen supply performance, and the obtained circulating solvent has low N, O and S contents.
[0042] (3) In the preparation method of the present invention, the first catalyst used in the hydrogenation process has good hydrogenation performance and high selectivity for hydrogenated aromatics; the second catalyst used also has high denitrification, deoxygenation, and dearomatization performance, good mechanical properties, and strong resistance to metal deposition and coking, which is conducive to the long-term stable operation of the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 The present invention is a schematic diagram of a process flow for preparing a circulating solvent for direct coal liquefaction in one embodiment.
[0044] Figure 2 XRD patterns of carriers Z-3-1 and Z-3-2 prepared in Catalyst Preparation Example 9.
[0045] Explanation of reference numerals: buffer tank 20 , buffer tank 80 , first hydrogenation reactor 30 , high-temperature separator 40 , low-temperature separator 50 , fractionation tower 60 , circulating hydrogen compressor 70 , second hydrogenation reactor 90 . DETAILED DESCRIPTION
[0046] In order to facilitate the understanding of the present invention, the present invention will be further described below in conjunction with examples. It should be understood that the following examples are only for a better understanding of the present invention and do not mean that the present invention is limited to the following examples.
[0047] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The term "and / or" as may be used herein includes any and all combinations of one or more of the related listed items. The terms "first", "second", etc. are used for descriptive purposes only and are not to be construed as indicating or implying relative importance.
[0048] The present invention provides a method for preparing a circulating solvent for direct coal liquefaction, comprising the following steps:
[0049] (1) subjecting a light fraction having a distillation range of 200 to 300° C. to a first hydrogenation reaction in a fixed bed reactor in the presence of a first catalyst to obtain a first hydrogenated stabilized oil;
[0050] subjecting the heavy fraction with a distillation range of more than 300° C. to a second hydrogenation reaction in an ebullating bed reactor with forced circulation in the presence of a second catalyst to obtain a second hydrogenated stable oil;
[0051] (2) mixing the first hydrogenated stabilized oil and the second hydrogenated stabilized oil, and separating and fractionating them to obtain a medium-temperature solvent and a high-temperature solvent;
[0052] (3) mixing the medium-temperature solvent and the high-temperature solvent to prepare the circulating solvent;
[0053] The first catalyst comprises a first carrier and a first active metal element, wherein the first active metal element comprises Ni and W; in the first catalyst, nickel oxide accounts for 0.1-10wt%, dextrin accounts for 5-40wt%, and the remainder is the first carrier; and the ratio of the amount of Ni element to the sum of the amounts of Ni element and W element is 0.1-0.4;
[0054] The second catalyst includes a second carrier and a second active metal element, wherein the second active metal element includes Ni and Mo, and optionally includes W; in the second catalyst, nickel oxide accounts for 0.1-10wt%, molybdenum oxide accounts for 10-40wt%, tungsten oxide accounts for 0-15%, and the balance is the second carrier.
[0055] By adopting the preparation method of the present invention, the light fraction is subjected to hydrogenation reaction using a specific Ni-W catalyst, and the heavy fraction is subjected to hydrogenation reaction using a specific Ni-Mo or Ni-Mo-W catalyst in a fixed bed reactor and an ebullating bed reactor with forced circulation, respectively. This is not only beneficial to avoid excessive hydrogenation of the light fraction and insufficient hydrogenation of the heavy fraction, but also beneficial to ultimately obtaining a circulating solvent with improved hydrogen supply performance.
[0056] In the present invention, a Ni-W catalyst is used for hydrogenation of light fractions, and in the first catalyst, nickel oxide accounts for 0.1-10wt%, dock oxide accounts for 5-40wt%, and the ratio of the amount of Ni element to the sum of the amounts of Ni element and W element is 0.1-0.4; the catalyst is used for hydrogenation of light fractions, has partial hydrogenation saturation performance for polycyclic aromatic hydrocarbons, inhibits cracking of cycloalkyl groups of hydrogenated aromatic hydrocarbons, improves the selectivity of hydrogenated aromatic hydrocarbons, and improves the hydrogen supply performance of medium-temperature solvents.
[0057] In the present invention, the hydrogenation of the heavy fraction uses a Ni-Mo or Ni-Mo-W catalyst, preferably a Ni-Mo-W catalyst, and in the second catalyst, nickel oxide accounts for 0.1-10wt%; molybdenum oxide accounts for 10-40wt%, and tungsten oxide accounts for 0-15%. In the heavy fraction, the nitrogen content, oxygen content and metal content are relatively high. The inventors have found that the use of the above catalyst for hydrogenation of the heavy fraction has high denitrification, deoxygenation, and dearomatization performance, good mechanical properties, strong resistance to metal deposition and coking, and can simultaneously meet the aromatic hydrogenation saturation functions of removing heteroatoms and condensed aromatics.
[0058] In a preferred embodiment, in the first catalyst, nickel oxide accounts for 1-6wt%, and tungsten oxide accounts for 10-25wt%; in the second catalyst, nickel oxide accounts for 2-6wt%; molybdenum oxide accounts for 15-30wt%; preferably, tungsten oxide accounts for 2-15wt%.
[0059] In a preferred embodiment, the most probable pore size of the first catalyst is in the range of 5-20 nm, preferably 8-15 nm; the specific surface area is preferably 200-400 m 2 / g, and the pore volume is preferably 0.35-0.9cm 3 / g; the second catalyst has a bimodal pore structure, the most possible pore size range of the small pore is 2-15nm, preferably 5-10nm; the most possible pore size range of the large pore is 20-80nm, preferably 30-50nm, and the specific surface area is 200-400m 2 / g, pore volume is 0.35-0.9cm 3 / g; the pore volume of small pores with a pore size of 5-10nm accounts for 20-60% of the total pore volume, and the pore volume of large pores with a pore size of 30-50nm accounts for 20-50% of the total pore volume. The inventors have found that the first catalyst having the above-mentioned specific pore structure and other apparent characteristics is used for the hydrogenation catalysis of light fractions in a fixed bed, and the second catalyst having the above-mentioned specific pore structure and other apparent characteristics is used for the hydrogenation catalysis of heavy fractions in an ebullating bed reactor with forced circulation. The combination of the two is applied to the circulating solvent preparation method of the present invention, based on the light fraction (mainly containing dicyclic and tricyclic aromatic compounds) and the heavy fraction (mainly containing condensed aromatic hydrocarbons with four or more rings) are hydrogenated separately, which is ultimately conducive to obtaining a circulating solvent with better hydrogen supply performance, and the obtained circulating solvent has low N, O, and S contents.
[0060] Furthermore, the first carrier is selected from one or more of alumina, silicon oxide, amorphous silica-alumina, and SBA-15; preferably, the first carrier is a carrier modified by a modifying metal, and the modifying metal is selected from one or more of alkali metal elements and alkaline earth metal elements, and preferably, the modifying metal is selected from one or more of Li, K, Na, Mg, and Ca. The inventors have found that the use of the above-mentioned modifying metal to modify the first carrier plays a role in reducing strong acid; in the light fraction hydrogenation process, polycyclic aromatic hydrocarbons are hydrogenated into hydrogenated aromatic hydrocarbons, and the use of such a modified first carrier in the first catalyst avoids the cracking of the cycloalkyl groups of the hydrogenated aromatic hydrocarbons during the hydrogenation process, thereby preventing the reduction of hydrogen supply performance.
[0061] Preferably, in the first carrier, the content of the modified metal oxide is 0.1-8 wt %.
[0062] In a preferred embodiment, the preparation step of the first catalyst comprises:
[0063] S1a: Mix the dry rubber powder (pseudo-boehmite) with sesbania powder and citric acid evenly, then add nitric acid solution, knead evenly and shape, dry and calcine, the calcination temperature is preferably 500-800, the calcination time is preferably 3-10h, to obtain the first carrier; in this step, drying is, for example, drying at 100°C for 3h.
[0064] Specifically, based on the mass of the dry rubber powder used in step S1a, the amount of sesbania powder is, for example, 1-5wt%; the amount of citric acid is, for example, 1-8wt%; the nitric acid solution is, for example, a nitric acid solution with a volume fraction of 20%, and the amount of nitric acid solution is, for example, 0.5-1.5wt%. During the kneading process, an appropriate amount of water can be added according to the molding requirements.
[0065] Preferably, during the uniform mixing process in step S1a, a solution of a salt of the modified metal is also added, and the specific amount can be determined according to the content of the modified metal oxide in the first carrier. The salt of the modified metal is, for example, one or more of nitrates, chlorides, sulfates and carbonates of the corresponding alkali metal or alkaline earth metal element (preferably one or more of Li, K, Na, Mg and Ca).
[0066] S2a: Impregnate the precursor solution of the first active metal element on the first carrier obtained in step S1a, dry and calcine, the calcination temperature is preferably 500-600°C, and the calcination time is preferably 3-10h, to obtain the first catalyst. Specifically, the above-mentioned impregnation can be an equal volume impregnation. The precursor of the first active metal element is, for example, ammonium metatungstate, basic nickel carbonate, etc.; in some examples, the specific operation process of impregnation in step S2a is, for example: add ammonium metatungstate to ammonia water to dissolve and adjust the pH to 9, stir evenly (for example, stir for 0.5h), add basic nickel carbonate, dissolve, and perform ultrasonic dispersion (for example, ultrasonic for 0.5h). After all components are completely dissolved, the volume is fixed to the required volume to obtain an impregnation solution, which is then impregnated on the first carrier. In this step, drying is, for example, drying at 120°C for 3h.
[0067] By adopting the above preparation steps to prepare the first catalyst, a first catalyst having the above preferred pore size and other apparent characteristics can be obtained.
[0068] Further, the second carrier is selected from one or more of alumina, amorphous silica-alumina, silicon oxide, zirconium oxide, magnesium oxide and titanium oxide;
[0069] Preferably, the second carrier is selected from alumina, and the alumina is selected from γ-AL 2 O 3 ,δ-AL 2 O 3 ,θ-AL 2 O 3,η-AL 2 O 3 Further preferably, the second carrier comprises γ-AL 2 O 3 , including δ-AL 2 O 3 and / or θ-AL 2 O 3 , the γ-AL 2 O 3 The mass of the δ-AL 2 O 3 and the θ-AL 2 O 3 The ratio of the sum of the masses of the two is 1:1-9:1; the inventors have found that by using the preferred second carrier, the obtained second catalyst has higher mechanical strength, and is particularly suitable for hydrogenation of heavy fractions in an ebullating bed with forced internal circulation which has more stringent requirements on mechanical strength, and has a lower attrition rate.
[0070] In a preferred embodiment, the second carrier further contains an auxiliary element, and the auxiliary element includes one or more of Si, P, B, Zr, and Ti;
[0071] Preferably, in the second carrier, the mass content of the oxide of the auxiliary element is 0.1-8wt%.
[0072] In a preferred embodiment, the preparation step of the second catalyst comprises:
[0073] S1b: Mix the dry rubber powder (pseudo-boehmite) with sesbania powder, citric acid and pore-enlarging agent uniformly, then add nitric acid solution (preferably a precursor of the auxiliary element dissolved therein), knead uniformly and shape, dry and calcine, the calcination temperature is preferably 500-1000° C., and the calcination time is preferably 3-10 hours, to obtain the second carrier; in this step, drying is performed at 100° C. for 3 hours, for example;
[0074] Preferably, after the drying, the dried material is divided into two parts with a mass ratio of 1:1-9:1, one part is calcined at 500-800°C for 3-10h, and the other part is calcined at >800°C and ≤1000°C for 3-10h, and then the two parts of the calcined carriers are mixed as the second carrier to obtain γ-AL 2 O 3 With δ-AL 2 O 3 and / or θ-AL 2 O 3 A second carrier formed by the combination;
[0075] Specifically, based on the mass of the dry rubber powder used in step S1b, the amount of sesbania powder is, for example, 1-5wt%, the amount of citric acid is, for example, 1-8wt%, the amount of the pore expanding agent is, for example, 0.5%-10%, preferably 1%-5%; the nitric acid solution is, for example, a nitric acid solution with a volume fraction of 20%, and the amount of the nitric acid solution is, for example, 0.5-1.5wt%; the precursor of the auxiliary element is boric acid, phosphoric acid, etc.
[0076] S2b: impregnating the impregnation solution on the second carrier, drying and calcining, the calcination temperature is preferably 500-600° C., and the calcination time is preferably 3-10 hours, to obtain the second catalyst; the impregnation solution is a solution including a salt of the second active metal element.
[0077] Specifically, the salt of the second active metal element is, for example, ammonium molybdate, ammonium metatungstate, basic nickel carbonate, etc. In step S2b, the impregnation is, for example, equal volume impregnation. The specific preparation operation of the impregnation solution in step S2b can refer to the corresponding description of the preparation of the impregnation solution in step S2a in the above text, and will not be repeated here.
[0078] By adopting the above preparation steps to prepare the second catalyst, a second catalyst having the above preferred pore size and other apparent characteristics can be obtained.
[0079] The inventors have found that the bimodal pore structure of the second catalyst can take into account both the heteroatom removal function and the improvement of the PDQI value of condensed aromatic hydrocarbons. The small pores are suitable for the hydrogenation removal of heteroatoms, and the large pores are helpful for the hydrogenation saturation of condensed aromatic hydrocarbons, while at the same time improving the resistance to metal deposition. The addition of auxiliary elements can adjust the acid properties of the catalyst surface and improve the interaction between the metal and the carrier, thereby reducing the coking of the catalyst.
[0080] Preferably, in step S1b, the pore expanding agent is selected from one or more of carbon black, polyethylene glycol, ammonium carbonate, silica sol, and cellulose.
[0081] In some embodiments, the conditions of the first hydrogenation reaction include: pressure of 8-16 MPa, temperature of 300-360°C, hydrogen-to-oil ratio of 400-1000 v / v, reaction space velocity of 0.5-3.5 h -1 The conditions of the second hydrogenation reaction include: pressure of 10-19 MPa, temperature of 320-380°C, hydrogen-oil ratio of 200-800 v / v, reaction space velocity of 1.0-3.5 h -1 .
[0082] Further, in step (2), the distillation range of the medium temperature solvent is 220-320°C, and the distillation range of the high temperature solvent is 320-500°C; or, the distillation range of the medium temperature solvent is 200-300°C, and the distillation range of the high temperature solvent is 300-480°C. Specifically, step (2) can also fractionate to obtain low temperature oil, such as a distillation range of <220°C or <200°C; and can also fractionate to obtain heavy oil, such as a distillation range of >480°C or >500°C.
[0083] In a preferred embodiment, in step (3), the mass ratio of the intermediate temperature solvent to the high temperature solvent is 5:1 to 4:2, preferably 4:1 to 6:2.
[0084] Specifically, in some examples, Figure 1 The process system shown is used to prepare the circulating solvent for direct coal liquefaction in the present invention, and the system includes buffer tanks 20, 80, a first hydrogenation reactor 30, a high-temperature separator 40, a low-temperature separator 50, a fractionation tower 60, a circulating hydrogen compressor 70, and a second hydrogenation reactor 90. In step (1), the light fraction and the heavy fraction are obtained by fractionating the whole distillate oil obtained by the direct coal liquefaction reaction. The light fraction and the heavy fraction enter the buffer tanks 20 and 80 respectively as subsequent hydrogenation raw materials. The light fraction coming out of the bottom of the buffer tank 20 is mixed with hydrogen and then enters the first hydrogenation reactor 30 for hydrogenation reaction to obtain a first hydrogenated stable oil. The heavy fraction coming out of the bottom of the buffer tank 80 is mixed with hydrogen and then enters the second hydrogenation reactor 90 for hydrogenation reaction to obtain a second hydrogenated stable oil. In step (2), the first hydrogenated stable oil and the second hydrogenated stable oil are mixed and separated, for example, including: entering the high temperature separator 40 for separation, the separation pressure of the hot high separation is, for example, 10-21 MPa, and the separation temperature is, for example, 100-300°C, more preferably 200-250°C; liquid oil is obtained at the bottom of the high temperature separator 40, and the top material enters the low temperature separator 50 for product separation; a part of the top material of the low temperature separator 50 is compressed by the circulating gas compressor 70 and mixed with fresh hydrogen as a raw material for the hydrogenation reactor, and a part is used as a purge gas to the subsequent gas treatment device; the bottom discharge of the low temperature separator 50 and the liquid oil obtained at the bottom of the high temperature separator 40 enter the fractionation tower 60 for product separation, and the top discharge of the fractionation tower 60 is a low temperature oil product; the side discharge of the fractionation tower is used as a medium temperature solvent (i.e., medium temperature oil); the bottom discharge of the fractionation tower is used as a high temperature solvent (i.e., high temperature oil). In some examples, all high temperature solvents and part of the medium temperature solvents are mixed to form a coal direct liquefaction circulating solvent.
[0085] Where specific experimental steps or conditions are not specified in the examples, the corresponding conventional experimental steps or conditions in the art can be used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.
[0086] Description of some detection methods:
[0087] 1. Testing methods for specific surface area, pore volume, minimum pore diameter, etc. of catalysts: GB / T 21650.2-2008 and GB / T 21650.1-2008.
[0088] 2. Mechanical strength: HG / T 2782-2011.
[0089] 3. Wear loss rate: Q / TSH 3490 909-2006.
[0090] 4. Catalyst C content after reaction: NB / SH / T 6067-2022.
[0091] Catalyst Preparation Example 1
[0092] Preparation of the first catalyst C-1:
[0093] S1a: Dry rubber powder, sesbania powder and citric acid are mixed evenly; then a nitric acid solution with a volume fraction of 20% is added, and a magnesium nitrate aqueous solution is added to the nitric acid solution, and the mixture is kneaded evenly with the powder, and extruded on an extruder; after drying at 100°C for 3 hours, the aluminum oxide carrier is obtained after calcining at 550°C for 6 hours; wherein based on the mass of the dry rubber powder used, the mass fraction of sesbania powder is 2%, the mass fraction of citric acid is 3%, and the mass fraction of nitric acid is 1%. The mass content of magnesium oxide in the obtained carrier is 1%.
[0094] S2a: prepare active metal solution, and use equal volume impregnation method to impregnate active metal elements onto the carrier, specifically, add ammonium metatungstate into deionized water heated to 45°C, and add ammonia water to adjust the solution pH to 9, add basic nickel carbonate after stirring for 0.5h, and after the basic nickel carbonate is dissolved, put it into an ultrasonic device for ultrasonication for 0.5h, and after the metal compound is completely dissolved, adjust the volume to the required volume to obtain an impregnation solution; impregnate the impregnation solution onto the carrier, dry it at 120°C for 3h, and calcine it at 550°C for 3h to obtain a hydrorefining catalyst, named C-1; wherein the mass proportion of nickel oxide is 1.2%, the mass proportion of tungsten oxide is 15%, and the remainder is the carrier, and the molar ratio of Ni / (Ni+W) is 0.2.
[0095] Catalyst Preparation Example 2
[0096] Preparation of the first catalyst C-2:
[0097] S1a: The carrier is prepared by referring to step S1a in Catalyst Preparation Example 1, except that the mass content of magnesium oxide in the prepared carrier is 2%.
[0098] S2a: Active metal elements are loaded by referring to step S2a of catalyst preparation example 1, except that, in the prepared catalyst, the mass proportion of nickel oxide is 1.5%, the mass proportion of tungsten oxide is 15%, and the molar ratio Ni / (Ni+W)=0.25, recorded as catalyst C-2.
[0099] Catalyst Preparation Example 3
[0100] Preparation of the first catalyst C-3:
[0101] S1a: Prepare the carrier by referring to step S1a of Catalyst Preparation Example 2;
[0102] S2a: Active metal elements are loaded by referring to step S2a of catalyst preparation example 2, except that the mass proportion of nickel oxide in the prepared catalyst is 1.8%, the mass proportion of tungsten oxide is 15%, and the molar ratio Ni / (Ni+W)=0.3, recorded as catalyst C-3.
[0103] Catalyst Preparation Example 4
[0104] Preparation of the first catalyst C-4:
[0105] S1a: The carrier is prepared by referring to step S1a in Catalyst Preparation Example 1, except that the magnesium nitrate used in preparing the carrier is replaced by potassium nitrate; and the mass content of potassium oxide in the prepared carrier is 2%.
[0106] S2a: Active metal elements are loaded by referring to step S2a of catalyst preparation example 1, except that the mass proportion of nickel oxide is 1.5%, the mass proportion of tungsten oxide is 15%, and the molar ratio Ni / (Ni+W)=0.25, recorded as catalyst C-4.
[0107] Catalyst Preparation Example 5
[0108] Preparation of the first catalyst C-5:
[0109] Catalyst C-5 was prepared with reference to Catalyst Preparation Example 4, with the following differences: when preparing the carrier, the dry rubber powder used was replaced with dry rubber powder and amorphous silica-alumina in a mass ratio of 3:2, and the potassium nitrate used was replaced with magnesium nitrate; in the prepared carrier, the mass fraction of magnesium oxide was 2%.
[0110] The rest of the preparation process and active metal content were consistent with those of catalyst C-4.
[0111] Catalyst Preparation Example 6
[0112] Preparation of the first catalyst C-6:
[0113] Catalyst C-6 was prepared by referring to Catalyst Preparation Example 4, except that potassium nitrate was not added when preparing the carrier. The rest of the preparation process and active metal content were the same as those of Catalyst C-4.
[0114] Catalyst Preparation Example 7
[0115] The preparation steps of the second catalyst C-7 are:
[0116] S1b: dry rubber powder, sesbania powder, citric acid and polyethylene glycol 2000 are mixed evenly; then a nitric acid solution with a volume fraction of 20% is added, to which a phosphoric acid aqueous solution is added, and the mixture is kneaded evenly, and extruded on an extruder; after drying at 100°C for 3 hours, the mixture is calcined at 550°C for 6 hours to obtain a carrier Z-2; wherein based on the mass of the dry rubber powder used, the mass fraction of sesbania powder is 2%, the mass fraction of citric acid is 3%, the mass fraction of nitric acid is 1%, and the mass fraction of polyethylene glycol 2000 is 2%; in the obtained carrier, the mass fraction of phosphorus oxide is 2%;
[0117] S2b: Active metals are loaded by equal volume impregnation method, and the specific steps are as follows: ammonium molybdate is added to deionized water heated to 45°C, and ammonia water is added to adjust the solution pH to 9. After stirring for 0.5h, basic nickel carbonate is added. After dissolution, it is placed in an ultrasonic device for ultrasonication for 0.5h. After the metal compound is completely dissolved, the volume is fixed to the required volume to obtain an impregnation solution, and the impregnation solution is impregnated onto the carrier; after drying at 120°C for 3h, it is calcined at 550°C for 3h to obtain a hydrorefining catalyst, named C-7; wherein, the proportion of nickel oxide is 2.5%, the mass fraction of molybdenum oxide is 15%, and the remainder is the carrier.
[0118] Catalyst Preparation Example 8
[0119] Preparation of the second catalyst C-8:
[0120] S1b: Prepare the carrier by referring to step S1b of Catalyst Preparation Example 7, except that the phosphoric acid solution is replaced by an aqueous boric acid solution, and the mass content of boron oxide in the obtained carrier is 2%;
[0121] S2b: proceed as per step S2b of Catalyst Preparation Example 7, except that the proportion of nickel oxide in the obtained catalyst is 2.5%, and the mass fraction of molybdenum oxide is 20%. This catalyst is recorded as Catalyst C-8.
[0122] Catalyst Preparation Example 9
[0123] The preparation steps of the second catalyst C-9 are:
[0124] S1b: The carrier was prepared by referring to step S1b in Catalyst Preparation Example 7, except that: the phosphoric acid aqueous solution was replaced by the boric acid aqueous solution; and before calcination, the carrier obtained after extrusion and drying was divided into two parts with a mass ratio of 7:3, 70wt% was calcined at a calcination temperature of 550°C for 6h to obtain the carrier Z-3-1; 30wt% was calcined at a calcination temperature of 900°C for 6h to obtain the carrier Z-3-2; the XRD spectra of the carriers Z-3-1 and Z-3-2 are shown in Figure 2 , carrier Z-3-1 is γ-Al 2 O 3 , carrier Z-3-2 is δ-Al 2 O 3 .
[0125] Carriers Z-3-1 and Z-3-2 are mixed to form carrier Z-3, wherein the mass content of boron oxide is 2%;
[0126] S2b: Step S2b was performed with reference to Catalyst Preparation Example 8, and the active metal was loaded onto the carrier Z-3 by the equal volume impregnation method to obtain Catalyst C-9, the active metal content of which was consistent with that of Catalyst C-8.
[0127] Catalyst Preparation Example 10
[0128] The preparation steps of the second catalyst C-10 are:
[0129] S1b: Prepare the carrier by referring to step S1b of catalyst preparation example 9, except that: when preparing the carrier, before calcination, the carrier obtained after extrusion molding and drying is divided into two parts at a mass ratio of 5:5, one part is calcined at 550°C, and the other part is calcined at 900°C. After calcination, the two parts of the carrier are mixed to obtain carrier Z-4, in which the mass content of boron oxide is 2%;
[0130] S2b: Refer to step S2b of Catalyst Preparation Example 9, and the active metal content in the prepared catalyst is consistent with that of Catalyst C-9.
[0131] Catalyst Preparation Example 11
[0132] Preparation steps of the second catalyst C-11:
[0133] The preparation steps of catalyst C-9 are referred to, except that:
[0134] The impregnation solution in step S2b contains basic nickel carbonate, ammonium metatungstate and ammonium molybdate. In the obtained catalyst C-11, the mass fraction of nickel oxide is 2.5%, the mass fraction of molybdenum oxide is 15%, and the mass fraction of tungsten oxide is 5%.
[0135] Catalyst Preparation Example 12
[0136] Preparation steps of the second catalyst C-12:
[0137] S1b: The process is carried out in accordance with step S1b of catalyst preparation example 8, except that polyethylene glycol 2000 is not added during the preparation process; the mass content of boron oxide in the obtained carrier is 2%;
[0138] S2b: The catalyst was prepared by referring to step S2b of catalyst preparation example 8. In the obtained catalyst, the proportion of nickel oxide was 2.5%, and the mass fraction of molybdenum oxide was 20%.
[0139] Examples 1-8
[0140] Examples 1-8 use the first catalyst and the second catalyst (see Table 1 for the specific catalysts used in each example) to prepare the circulating solvent. Figure 1 As shown, the full-fraction oil from the direct coal liquefaction reaction is fractionated in a distillation tower at a pressure of 0.05MPa to separate low-temperature oil with a distillation range of <200°C, a light fraction with a distillation range of 200-300°C, and a heavy fraction with a distillation range of >300°C.
[0141] (1) Hydrogenation reaction
[0142] (1.1) After being stabilized in the buffer tank 20, the light fraction enters the first hydrogenation reactor 30 (fixed bed reactor) and undergoes hydrogenation reaction under the catalytic action of the first catalyst at a pressure of 13 MPa, a temperature of 340°C, a hydrogen-to-oil ratio of 800 v / v, and a reaction volume space velocity of 1.5 h -1 Hydrogenation stabilization is carried out under conditions of to obtain the first hydrogenation stabilized oil.
[0143] (1.2) After being stabilized in the buffer tank 80, the heavy fraction enters the second hydrogenation reactor (ebullating bed reactor with forced circulation) and undergoes hydrogenation reaction under the catalytic action of the second catalyst at a pressure of 16 MPa, a temperature of 360°C, a hydrogen-to-oil ratio of 300 v / v, and a reaction volume space velocity of 1.5 h -1 The oil is then hydrogenated and stabilized to obtain a second hydrogenated stabilized oil.
[0144] (2) The first and second hydrogenated stable oils obtained from the first hydrogenation reactor 30 and the second hydrogenation reactor 90 enter the high temperature separator 40 with a pressure of 16 MPa and a separation temperature of 250° C. for separation; the light oil product at the top of the high temperature separator 40 enters the low temperature separator 50 with a pressure of 16 MPa and a temperature of 20° C. for separation, and the oil product coming out of the bottom after separation and the bottom product of the high temperature separator enter the fractionation tower 60 for fractionation, and the oil product coming out of the top of the fractionation tower has a distillation range of <200° C., which is mixed with the low temperature oil obtained by fractionation of the whole fraction oil obtained by direct liquefaction reaction with coal, the oil product coming out of the side line (distillation range 200-300° C.) is used as the medium temperature solvent, the oil product coming out of the bottom (distillation range 300-480° C.) is used as the high temperature solvent, and the oil product with a distillation range greater than 480° C. is used as the heavy oil.
[0145] (3) All high-temperature solvent and part of medium-temperature solvent are prepared into coal direct liquefaction circulating solvent in a mass ratio of 2:3.
[0146] Table 1 The first catalyst and the second catalyst used in Examples 1-8
[0147]
[0148] Comparative Example 1:
[0149] The whole fraction oil from the direct coal liquefaction reaction enters the ebullating bed reactor and undergoes hydrogenation reaction under the catalytic action of the nickel-molybdenum series catalyst HRK-658 at a pressure of 19 MPa, a temperature of 360°C, a hydrogen-to-oil ratio of 300 v / v, and a reaction space velocity of 1.5 h -1 Hydrogenation stabilization is carried out under conditions to obtain hydrogenation stabilized oil.
[0150] The obtained hydrogenated stabilized oil is drawn out from the ebullating bed reactor and separated in a hot high fraction separator at a pressure of 19MPa and a separation temperature of 400°C to obtain high temperature oil. The material at the top of the hot high fraction separator enters a low temperature fraction separator at a pressure of 19MPa and a temperature of 20°C for separation. The material at the bottom of the low temperature separator and the high temperature oil enter a fractionation tower for fractionation. The pressure of the fractionation tower is controlled at 0.05MPa to separate low temperature oil less than 200°C, medium temperature oil of 200-350°C, and high temperature oil>350°C.
[0151] All the high-temperature oil and part of the medium-temperature oil obtained from the fractionation tower are prepared into a circulating solvent for direct coal liquefaction in a ratio of 2:7. The remaining medium-temperature oil and low-temperature oil are mixed as feedstock oil for the hydrogenation and reforming process.
[0152] The physical property analysis of the first catalyst obtained in each catalyst preparation example and the application effect (carbon content in the catalyst after the reaction) when preparing the first hydrogenated stable oil when preparing the circulating solvent in Examples 1-6 are shown in Table 2. The physical property analysis of the second catalyst obtained in each catalyst preparation example and the application effect (wear loss rate and carbon content in the catalyst after the reaction) when preparing the second hydrogenated stable oil when preparing the circulating solvent in Examples 1-6 are shown in Table 3.
[0153] Table 2 Physical properties analysis of the first catalyst
[0154]
[0155] Table 3 Physical properties analysis of the second catalyst
[0156]
[0157]
[0158] Note: In Table 3, the "small pore size / large pore size pore volume percentage in the total pore volume" refers to small pores with a pore diameter of 5-10 nm, and the "large pore size" refers to large pores with a pore diameter of 30-50 nm. Taking Example 1 as an example, the small pore size / large pore size pore volume percentage in the total pore volume is 47 / 40, where "47" means that the pore volume of small pores in the pore diameter range of 5-10 nm accounts for 47% of the total pore volume, and "40" means that the pore volume of large pores in the pore diameter range of 30-50 nm accounts for 40% of the total pore volume.
[0159] See Table 4 for the analytical data of the circulating solvents prepared in each embodiment and comparative example.
[0160] Table 4 Circulating solvent analysis data
[0161]
[0162]
[0163] Note: "Feedstock" in Table 4 refers to the whole distillate oil from direct coal liquefaction reaction.
[0164] It can be seen from the experimental results in Table 4 that, by adopting the preparation method of the present invention, the light fraction is hydrogenated in a fixed bed reactor using the first catalyst of the present invention, and the heavy fraction is hydrogenated in an ebullating bed reactor with forced circulation using the second catalyst of the present invention; and then the circulating solvent obtained by preparing the medium-temperature solvent and the high-temperature solvent obtained by fractionation has significantly improved hydrogen supply performance, and the N, S, and O contents are significantly lower.
[0165] From the comparison between Examples 6 and 8 and Example 1, it can be seen that the circulating solvent prepared in Example 1 using the first catalyst containing the modified metal has further improved hydrogen supply performance and lower N, S and O contents compared with Examples 6 and 8.
[0166] It can be seen from the comparison between Examples 3-5 and 7 and Examples 1-2 that the use of a preferred carrier in the second catalyst is conducive to further improving the hydrogen supply performance of the obtained circulating solvent, while taking into account the lower content of N, S, and O. Among them, the second catalyst in Example 5 further contains tungsten, and the obtained circulating solvent has better hydrogen supply performance and takes into account relatively lower content of N, S, and O.
[0167] It is easy to understand that the above embodiments are only examples for clear explanation and do not mean that the present invention is limited thereto. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the protection scope of the present invention.
Claims
1. A method for preparing a circulating solvent for direct coal liquefaction, It is characterized in that The steps include: (1) subjecting a light fraction having a distillation range of 200 to 300° C. to a first hydrogenation reaction in a fixed bed reactor in the presence of a first catalyst to obtain a first hydrogenated stabilized oil; subjecting the heavy fraction with a distillation range of more than 300° C. to a second hydrogenation reaction in an ebullating bed reactor with forced circulation in the presence of a second catalyst to obtain a second hydrogenated stable oil; (2) mixing the first hydrogenated stabilized oil and the second hydrogenated stabilized oil, and separating and fractionating them to obtain a medium-temperature solvent and a high-temperature solvent; (3) mixing the medium-temperature solvent and the high-temperature solvent to prepare the circulating solvent; The first catalyst comprises a first carrier and a first active metal element, wherein the first active metal element comprises Ni and W; in the first catalyst, nickel oxide accounts for 0.1-10wt%, dextrin accounts for 5-40wt%, and the remainder is the first carrier; and the ratio of the amount of Ni element to the sum of the amounts of Ni element and W element is 0.1-0.4; The second catalyst includes a second carrier and a second active metal element, wherein the second active metal element includes Ni and Mo, and optionally includes W; in the second catalyst, nickel oxide accounts for 0.1-10wt%, molybdenum oxide accounts for 10-40wt%, tungsten oxide accounts for 0-15wt%, and the balance is the second carrier.
2. The preparation method according to claim 1, It is characterized in that In the first catalyst, nickel oxide accounts for 1-6wt% and dock oxide accounts for 10-25wt%; In the second catalyst, nickel oxide accounts for 2-6wt%; molybdenum oxide accounts for 15-30wt%; and preferably tungsten oxide accounts for 2-15wt%.
3. The preparation method according to claim 1 or 2, It is characterized in that The most probable pore size of the first catalyst is in the range of 5-20 nm, preferably 8-15 nm; the specific surface area is preferably 200-400 m 2 / g, and the pore volume is preferably 0.35-0.9cm 3 / g; The second catalyst has a bimodal pore structure, the most probable pore size range of the small pores is 2-15nm, preferably 5-10nm; the most probable pore size range of the large pores is 20-80nm, preferably 30-50nm; the specific surface area is 200-400m 2 / g, pore volume is 0.35-0.9cm 3 / g; the pore volume of small pores with a pore diameter of 5-10nm accounts for 20-60% of the total pore volume, and the pore volume of large pores with a pore diameter of 30-50nm accounts for 20-50% of the total pore volume.
4. The preparation method according to claim 3, It is characterized in that The first carrier is selected from one or more of alumina, silicon oxide, amorphous silica-alumina, and SBA-15, and preferably the first carrier is a carrier modified by a modified metal; The modified metal is selected from one or more of alkali metal elements and alkaline earth metal elements, preferably the modified metal is selected from one or more of Li, K, Na, Mg, and Ca; Preferably, in the first carrier, the content of the modified metal oxide is 0.1-8 wt %.
5. The preparation method according to claim 4, It is characterized in that The preparation steps of the first catalyst include: S1a: mixing the dry rubber powder, sesbania powder and citric acid uniformly, then adding nitric acid solution to knead uniformly and shape, drying and calcining, the calcination temperature is preferably 500-800° C., and the calcination time is preferably 3-10 hours, to obtain the first carrier; preferably, the solution of the modified metal salt is also added during the mixing process; S2a: impregnating the precursor solution of the first active metal element onto the first carrier obtained in step S1a, drying and calcining, wherein the calcination temperature is preferably 500-600° C. and the calcination time is preferably 3-10 h, to obtain the first catalyst.
6. The preparation method according to any one of claims 3 to 5, It is characterized in that The second carrier is selected from one or more of alumina, amorphous silica-alumina, silicon oxide, zirconium oxide, magnesium oxide and titanium oxide; Preferably, the second carrier is selected from alumina, and the alumina is selected from γ-AL 2 O 3 ,δ-AL 2 O 3 ,θ-AL 2 O 3 ,η-AL 2 O 3 One or more of; Further preferably, the second carrier comprises γ-AL 2 O 3 , including δ-AL 2 O 3 and / or θ-AL 2 O 3 , the γ-AL 2 O 3 The mass of the δ-AL 2 O 3 and the θ-AL 2 O 3 The ratio of the sum of the masses of the two is 1:1-9:
1.
7. The preparation method according to claim 6, It is characterized in that The second carrier contains auxiliary elements, and the auxiliary elements include one or more of Si, P, B, Zr, and Ti; Preferably, in the second carrier, the mass content of the oxide of the auxiliary element is 0.1-8wt%.
8. The preparation method according to claim 7, It is characterized in that The preparation steps of the second catalyst include: S1b: uniformly mixing the dry rubber powder with sesbania powder, citric acid and pore-enlarging agent, then adding nitric acid solution, kneading and forming, drying and calcining, the calcination temperature is preferably 500-1000° C., and the calcination time is preferably 3-10 hours, to obtain the second carrier; preferably, the precursor of the auxiliary element is also added during the uniform mixing process; Preferably, after the drying, the dried material is divided into two parts with a mass ratio of 1:1-9:1, one part is calcined at 500-800°C for 3-10h, and the other part is calcined at >800°C and ≤1000°C for 3-10h, and then the two parts of the carrier obtained by calcination are mixed as the second carrier; S2b: impregnating the impregnation solution on the second carrier, drying and calcining, the calcination temperature is preferably 500-600° C., and the calcination time is preferably 3-10 hours, to obtain the second catalyst; the impregnation solution is a solution including a salt of the second active metal element; Preferably, in step S1b, the pore expanding agent is selected from one or more of carbon black, polyethylene glycol, ammonium carbonate, silica sol, and cellulose; the amount of the pore expanding agent is 0.5%-10% of the mass of the dry rubber powder, preferably 1%-5%.
9. The preparation method according to any one of claims 1 to 8, It is characterized in that The conditions of the first hydrogenation reaction include: pressure of 8-16 MPa, temperature of 300-360°C, hydrogen-to-oil ratio of 400-1000 v / v, reaction volume space velocity of 0.5-3.5 h -1 ; And / or, the conditions of the second hydrogenation reaction include: pressure of 10-19 MPa, temperature of 320-380°C, hydrogen-to-oil ratio of 200-800 v / v, reaction volume space velocity of 1.0-3.5 h -1 ; And / or, in step (1), the light fraction and the heavy fraction are obtained by fractionating the whole fraction oil obtained by direct coal liquefaction reaction.
10. The preparation method according to any one of claims 1 to 9, It is characterized in that In step (2), the distillation range of the medium-temperature solvent is 220-320° C., and the distillation range of the high-temperature solvent is 320-500° C.; or, the distillation range of the medium-temperature solvent is 200-300° C., and the distillation range of the high-temperature solvent is 300-480° C.; Preferably, in step (3), the mass ratio of the medium-temperature solvent to the high-temperature solvent is 5:1 to 4:2, preferably 4:1 to 6:2.
Citation Information
Patent Citations
Recycling solvent and preparation method thereof
CN106479564A
Direct coal liquefaction circulating hydrogen-donor solvent as well as preparation method and application thereof