Two-dimensional mesoporous single crystal gamma-alumina nano material and preparation method thereof

Through the high-pressure hydrothermal method without template agent, the problems of easy formation of three-dimensional structure and high production cost of mesoporous γ-alumina nanomaterials were solved, and two-dimensional mesoporous single crystal γ-alumina with high specific surface area and uniform morphology was successfully prepared. Alumina nanomaterials are suitable for large-scale industrial production.

CN118792736AActive Publication Date: 2024-10-18FUDAN UNIVERSITY

Patent Information

Application Number
CN202410845836.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-18
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

When the existing technology synthesizes mesoporous γ-alumina nanomaterials, it is easy to form a three-dimensional structure and mask the active sites, and most methods require template agents, which increases production costs and is difficult to be suitable for large-scale industrial production.

Method used

Using a template-free high-pressure hydrothermal method, two-dimensional mesoporous single crystal γ-alumina nanomaterials are prepared by dissolving inorganic aluminum salts and precipitating agents in deionized water, performing a hydrothermal reaction and then calcining, avoiding grain growth. And the mesoporous skeleton collapses, achieving the maintenance of the two-dimensional structure.

Benefits of technology

Successfully prepared two-dimensional mesoporous single crystal γ-alumina nanomaterials with high specific surface area and uniform morphology, which simplifies the process, reduces production costs, is suitable for large-scale industrial production, and maintains the high crystallinity and activity of the material. site.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118792736A_ABST
    Figure CN118792736A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of preparation of nano materials, and particularly relates to a two-dimensional mesoporous single crystal gamma-aluminum oxide nano material and a preparation method thereof. The preparation method comprises the following steps: dissolving an aluminum source and a precipitator in deionized water, carrying out a hydrothermal reaction at a specific temperature, centrifuging, washing and drying the product, and carrying out high-temperature roasting to obtain the blade-shaped two-dimensional mesoporous single crystal gamma-alumina nano material. The long edge of the two-dimensional mesoporous single crystal gamma-alumina nano material grows in an oriented manner along the crystal orientation (400), the wide edge of the two-dimensional mesoporous single crystal gamma-alumina nano material grows in an oriented manner along the crystal orientation (440), the specific surface area can reach 200 m < 2 > / g, and the two-dimensional mesoporous single crystal gamma-alumina nano material has the advantages of controllable morphology, uniform dispersion, high The method does not need a surfactant, is low in production cost, and is green and environment-friendly; the preparation process is simple, large-scale rapid preparation of the two-dimensional mesoporous single crystal gamma-alumina nano material can be realized, and the method has a wide industrial application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanomaterials, and specifically relates to a two-dimensional mesoporous single crystal gamma-alumina nanomaterial and a preparation method thereof. Background Art

[0002] Mesoporous metal oxides are not only endowed with the common properties of mesoporous materials such as high specific surface area and high mass transfer efficiency, but also maintain the intrinsic physical and chemical properties of metal oxides, showing strong advantages in the fields of catalysis, separation, gas sensing, etc. Among them, mesoporous γ-alumina is widely used as a functional carrier for catalytic conversion of small molecules and catalytic cracking of large molecules due to its excellent thermal stability, good mechanical properties, adjustable surface properties, and low production cost.

[0003] A classic method for synthesizing mesoporous γ-alumina mainly includes solvent evaporation induced self-assembly method, hydrothermal method, etc.; the main problem of solvent evaporation induced self-assembly method is that long-term high-temperature calcination in the subsequent crystallization process can easily cause grain growth and collapse of the mesoporous skeleton (RSC Adv.2015,5,49287). The hydrothermal method can more conveniently obtain single-crystalline mesoporous hydroxyalumina, and then obtain single-crystalline mesoporous alumina with preserved morphology after calcination. However, the mesoporous hydroxyalumina nanomaterials synthesized by the hydrothermal method are usually three-dimensional structures formed by the assembly of two-dimensional nanosheets (Nat.Commun.2019,10,1611; Patent CN107540007A), which masks a large number of active sites and is not conducive to mass transfer of macromolecules. In addition, most hydrothermal synthesis methods require templates such as sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, and polyvinylpyrrolidone, which increases the synthesis cost and is not suitable for large-scale industrial production. In view of the above problems, the present invention develops a method for synthesizing two-dimensional mesoporous single crystal γ-alumina nanomaterials without a template. Summary of the invention

[0004] The purpose of the present invention is to provide a two-dimensional mesoporous single crystal γ-alumina nanomaterial with uniform product morphology, green and environmental protection, simple preparation process and low production cost, and a preparation method thereof.

[0005] The method for preparing a two-dimensional mesoporous single crystal γ-alumina nanomaterial provided by the present invention comprises the following specific steps:

[0006] (1) adding an inorganic aluminum salt and a precipitant to deionized water, stirring and dissolving to obtain a clear and transparent precursor solution;

[0007] (2) transferring the precursor solution into a high-pressure hydrothermal autoclave and performing a hydrothermal reaction in an oven;

[0008] (3) The product is centrifuged, washed, dried, and then calcined to obtain the target product, a two-dimensional mesoporous single crystal γ-alumina nanomaterial. The nanomaterial has a two-dimensional blade-like morphology with a length of 1.1 to 1.3 μm, a width of 300 to 400 nm, and a thickness of 20 to 30 nm. Clear mesoporous channels are distributed on the two-dimensional γ-alumina sheet, and the channel orientation is parallel to the long side of the blade, with a pore size of 2 to 3 nm. The long edge of the two-dimensional mesoporous single crystal γ-alumina grows along the (400) crystal direction, and the wide edge grows along the (440) crystal direction. The specific surface area of ​​the material can reach 200 m 2 / g.

[0009] Preferably, the inorganic aluminum salt in step (1) is one or more of aluminum nitrate nonahydrate and anhydrous aluminum chloride.

[0010] Preferably, the precipitant in step (1) is one or more of urea, urotropine, and ammonia water; more preferably, urea and urotropine.

[0011] Preferably, the concentration of the inorganic aluminum salt in step (1) is 6.66 to 333 mmol / L. More preferably, the concentration of the inorganic aluminum salt is 33.3 mmol / L.

[0012] Preferably, if urea is used as a precipitant in step (1), the concentration of urea is 9.94-3330 mmol / L, and the molar ratio of aluminum salt to urea is 0.1-0.67. More preferably, the concentration of urea is 66.6 mmol / L, and the molar ratio of aluminum salt to urea is 0.5.

[0013] Preferably, if hexamethylenetetramine is used as a precipitant in step (1), the concentration of hexamethylenetetramine is 4.44-333 mmol / L, and the molar ratio of aluminum salt to urea is 1.0-1.5. More preferably, the concentration of hexamethylenetetramine is 25.0 mmol / L, and the molar ratio of aluminum salt to urea is 1.3.

[0014] Preferably, if concentrated ammonia water is used as a precipitant in step (1), the amount of concentrated ammonia water used is 0.6 mL.

[0015] Preferably, the stirring in step (1) has a stirring speed of 150 to 2000 rpm and a time of 0.25 to 36 h.

[0016] Preferably, the temperature of the hydrothermal reaction in step (2) is 120 to 200° C., and the time of the hydrothermal reaction is 4 to 72 hours.

[0017] Preferably, the centrifugal speed in step (3) is 7000 rpm; and the washing solvent is deionized water.

[0018] Preferably, the calcination temperature used in step (3) is 300-800° C., the calcination heating rate is 0.1-20° C. / min, and the holding time is more than 0.5 h.

[0019] The present invention also includes a two-dimensional mesoporous single crystal γ-alumina nanomaterial prepared by the above method, which has a two-dimensional blade-like morphology, a length of 1.1 to 1.3 μm, a width of 300 to 400 nm, and a thickness of 20 to 30 nm. Clear mesoporous channels are distributed on the two-dimensional γ-alumina sheet, and the channel orientation is parallel to the long side of the blade, and the pore size is 2 to 3 nm. The long side of the two-dimensional mesoporous single crystal γ-alumina grows along the (400) crystal direction, and the wide side grows along the (440) crystal direction; the specific surface area of ​​the material can reach 200 m 2 / g.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] (1) The present invention overcomes the problem that aluminum hydroxide easily self-assembles to construct a three-dimensional structure under hydrothermal / solvothermal conditions, and obtains a two-dimensional mesoporous single-crystal γ-alumina nanomaterial that has a high crystallinity and can maintain a high crystallinity of up to 200 m 2 / g specific surface area;

[0022] (2) The present invention proposes an in-situ decomposition and release strategy for the precipitant, which effectively slows down the hydrolysis rate of aluminum salt, regulates the process of aluminum source hydrolysis, colloid conversion, and nanoparticle assembly, and realizes the construction of two-dimensional mesoporous single crystal γ-alumina;

[0023] (3) The preparation process of the present invention is simple, the production cost is low, and it is green and environmentally friendly; except for inorganic aluminum salts and precipitants, no other additives such as surfactants are required to achieve large-scale rapid preparation of two-dimensional mesoporous single-crystal γ-alumina nanomaterials, which has broad industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a transmission electron microscope image of the two-dimensional mesoporous single crystal γ-alumina nanomaterial provided in Example 1, wherein the inset is the corresponding selected electron diffraction image.

[0025] Figure 2 This is a large-scale scanning electron microscope image of the two-dimensional mesoporous single-crystalline γ-alumina nanomaterial provided in Example 1.

[0026] Figure 3 This is the nitrogen adsorption-desorption isotherm of the two-dimensional mesoporous single crystal γ-alumina nanomaterial provided in Example 1.

[0027] Figure 4 This is the pore size distribution curve of the two-dimensional mesoporous single crystal γ-alumina nanomaterial provided in Example 1.

[0028] Figure 5 This is the X-ray diffraction pattern of the two-dimensional mesoporous single crystal γ-alumina nanomaterial provided in Example 1.

[0029] Figure 6 This is a transmission electron microscope image of the two-dimensional mesoporous single crystal γ-alumina nanomaterial provided in Example 2.

[0030] Figure 7 This is a transmission electron microscope image of the two-dimensional mesoporous single crystal γ-alumina nanomaterial obtained using urotropine as provided in Example 3.

[0031] Figure 8 This is a scanning electron microscope image of the sample obtained using ammonia water provided in Example 4. DETAILED DESCRIPTION

[0032] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0033] Example 1, preparation of a two-dimensional mesoporous single crystal γ-alumina nanomaterial:

[0034] Dissolve 750mg aluminum nitrate nine hydrate (2.0mmol) and 240mg urea (4.0mmol, aluminum salt to precipitant molar ratio of 0.5) in 60mL deionized water, at which the aluminum ion concentration is 33.3mmol / L and the urea concentration is 66.6mmol / L; stir at 500rpm and 1h during dissolution. Transfer the precursor solution into a 100mL hydrothermal reactor, put it into an oven, react at 120℃ for 48h, and cool naturally to room temperature; centrifuge the obtained product at a speed of 7000rpm, wash it with deionized water 3 times, and put it into a 60℃ oven to dry overnight; the dried product is heated to 450℃ at 2℃ / min in a muffle furnace, kept warm for 2h, and then cooled naturally, and the obtained white powder is a two-dimensional mesoporous single crystal γ-alumina nanomaterial.

[0035] Figure 1 The transmission electron microscope image of the two-dimensional mesoporous single crystal γ-alumina nanomaterial provided in Example 1 shows that the material has a two-dimensional blade-like morphology, with clear mesoporous channels distributed on the sheet. The channels are oriented parallel to the long side of the blade, and the pore diameter is 2 to 3 nm. Figure 1 The small figure in the figure is the corresponding selected area electron diffraction pattern, which shows that the two-dimensional mesoporous γ-alumina has a high crystallinity of a single crystal. The long edge of the material grows in an oriented direction along the (400) direction, and the wide edge grows in an oriented direction along the (440) direction.

[0036] Figure 2A large-scale scanning electron microscope image of the two-dimensional mesoporous single-crystalline γ-alumina nanomaterial provided in Example 1 shows that the material morphology is uniform and has not been assembled to form a three-dimensional structure; the two-dimensional mesoporous single-crystalline γ-alumina nanomaterial has a length of 1.1 to 1.3 μm, a width of 300 to 400 nm, and a thickness of 20 to 30 nm.

[0037] Figure 3 The nitrogen adsorption-desorption isotherm of the two-dimensional mesoporous single crystal γ-alumina nanomaterial provided in Example 1 is shown as curve II. A hysteresis loop appears at a partial pressure of 0.9 to 0.99, showing the adsorption-desorption characteristics of stacked pores. The specific surface area is 200 m 2 / g.

[0038] Figure 4 The pore size distribution curve of the two-dimensional mesoporous single crystal γ-alumina nanomaterial provided in Example 1 shows that the pore size is concentrated at 3 nm.

[0039] Figure 5 This is an X-ray diffraction pattern of the two-dimensional mesoporous single crystal γ-alumina nanomaterial provided in Example 1. The diffraction peak corresponds to the crystal diffraction peak of γ-alumina, and the corresponding crystal library number is 10-0425.

[0040] Example 2, preparation of a two-dimensional mesoporous single crystal γ-alumina nanomaterial:

[0041] 1.34g of anhydrous aluminum chloride (10.0mmol) and 900mg of urea (15.0mmol, aluminum salt to precipitant molar ratio of 0.67) were dissolved in 60mL of deionized water, at which the aluminum ion concentration was 166mmol / L and the urea concentration was 250mmol / L; the stirring speed was 1500rpm and the stirring time was 30h during dissolution. The precursor solution was transferred into a 100mL hydrothermal reactor, placed in an oven, reacted at 180℃ for 4h, and naturally cooled to room temperature; the obtained product was centrifuged at a speed of 7000rpm, washed with deionized water 3 times, and placed in a 60℃ oven to dry overnight; the dried product was heated to 350℃ in a muffle furnace at 0.5℃ / min, kept warm for 4h, and then cooled naturally, and the obtained white powder was a two-dimensional mesoporous single crystal γ-alumina nanomaterial.

[0042] Figure 6 The transmission electron micrograph of the two-dimensional mesoporous single crystal γ-alumina nanomaterial provided in Example 2 shows that the shape of the alumina nanosheets is partially incomplete, but it still proves that the method is simple to synthesize, has strong universality and high repeatability.

[0043] Example 3, preparation of a two-dimensional mesoporous single crystal γ-alumina nanomaterial:

[0044] Compared with Example 1, most of the conditions are the same, except that the precipitant is replaced by 215 mg of hexamethylenetetramine (1.5 mmol) instead of 240 mg of urea.

[0045] Figure 7 The transmission electron microscope image of the sample obtained using urotropine provided in Example 3; it can be seen that using another precipitant that slowly decomposes and releases ammonia under hydrothermal conditions can also obtain a two-dimensional mesoporous single-crystalline γ-alumina nanomaterial, which is mainly in the shape of long strips. However, compared with using urea as a precipitant, the mesoporous channels are not clear enough.

[0046] Example 4, preparation of a two-dimensional mesoporous single crystal γ-alumina nanomaterial:

[0047] Compared with Example 1, most of the steps are the same, except that the precipitant is replaced by 0.6 mL of concentrated aqueous ammonia instead of 240 mg of urea.

[0048] Figure 8 From the scanning electron microscope image of the sample obtained using ammonia water provided in Example 4, it can be seen that the sample does not show independently dispersed two-dimensional lamellar morphology, but is adhered together to form a bulk structure, indicating that the selection of a precipitant that releases alkali in situ by thermal decomposition is the key to synthesizing two-dimensional mesoporous single-crystalline γ-alumina nanomaterials.

[0049] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a two-dimensional mesoporous single-crystal γ-alumina nanomaterial, characterized in that: The specific steps are: (1) adding an inorganic aluminum salt and a precipitant to deionized water, stirring and dissolving to obtain a clear and transparent precursor solution; (2) transferring the precursor solution into a high-pressure hydrothermal autoclave and performing a hydrothermal reaction in an oven; (3) The product is centrifuged, washed, dried, and then calcined to obtain the target product, a two-dimensional mesoporous single-crystalline γ-alumina nanomaterial; the two-dimensional mesoporous single-crystalline γ-alumina nanomaterial has a two-dimensional blade-like morphology, a length of 1.1 to 1.3 μm, a width of 300 to 400 nm, and a thickness of 20 to 30 nm; clear mesoporous channels are distributed on the two-dimensional sheet, the channel orientation is parallel to the long side of the blade, the pore diameter is 2 to 3 nm, and the specific surface area can reach 200 m 2 / g; the long edges of the two-dimensional mesoporous single crystal γ-alumina nanomaterial grow in an oriented direction (400) and the wide edges grow in an oriented direction (440).

2. The preparation method according to claim 1, characterized in that: In step (1), the inorganic aluminum salt is one or more of aluminum nitrate nonahydrate and anhydrous aluminum chloride; the precipitant is one or more of urea, hexamethylenetetramine and concentrated ammonia water.

3. The preparation method according to claim 2, characterized in that: In step (1), when urea is used as the precipitant, the concentration of the aluminum salt is 6.66-333 mmol / L, and the molar ratio of the aluminum salt to the urea is 0.1-0.67; when urotropine is used as the precipitant, the concentration of the aluminum salt is 6.66-333 mmol / L, and the molar ratio of the aluminum salt to the urea is 1.0-1.5; when concentrated aqueous ammonia is used as the precipitant, the concentration of the aluminum salt is 6.66-333 mmol / L, and the amount of concentrated aqueous ammonia used is 0.6 mL.

4. The preparation method according to claim 4, characterized in that: In step (2), the hydrothermal reaction temperature is 120 to 200° C., and the hydrothermal reaction time is 4 to 72 hours.

5. The second preparation method according to claim 2, characterized in that: In step (3), the calcination temperature is 300-800°C, and the heating rate is 0.1-20°C / min.

6. A two-dimensional mesoporous single crystal γ-alumina nanomaterial obtained by the preparation method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • A preparing method of nanometer flake-shaped mesoporous alumina

    CN107540007A

  • Hydrothermal method for preparing gamma-AL2O3 hollow microsphere polishing material without mould plate

    CN101367535A

  • Preparation method of mesoporous alumina catalyst

    CN101829552A

  • Preparation method of micron gamma aluminum oxide with controllable morphology and mesoporous structure

    CN103359765A

  • Preparation method of alumina carrier

    CN103787394A

Cited By

  • Adsorption coupling catalyst, preparation method thereof and application of adsorption coupling catalyst in catalytic adsorption of methyl mercaptan and carbon dioxide

    CN120393990A

  • Adsorptive coupling catalyst, its preparation method and application in catalytic adsorption of methanethiol and carbon dioxide

    CN120393990B

  • Flaky aluminum oxide nano-particles, preparation method and application of flaky aluminum oxide nano-particles in geothermal circulation medium

    CN120589769A

  • A platelet-shaped alumina nanoparticle, a method of preparation and use thereof in geothermal circulating media

    CN120589769B

  • Plate-shaped boehmite aggregate and method for manufacturing the same

    JP7845731B1