Modified graphene antistatic viscose fiber as well as preparation method and application thereof

By grafting poly(2-vinylpyridine) on polysiloxane and compounding it with graphene, the problem of compatibility and dispersion of graphene and viscose fiber is solved, and the antistatic effect of modified graphene viscose fiber is improved. The antistatic and antibacterial properties make the material washable and high-strength.

CN118792745APending Publication Date: 2024-10-18SHENZHEN HUANENG GRAPHENE TECH CO LTD

Patent Information

Application Number
CN202411165395.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In the existing technology, graphene has poor compatibility and dispersion with viscose fibers, resulting in insufficient antistatic properties and poor functionality against washing, which affects the performance and application of the material.

Method used

By grafting poly(2-vinylpyridine) on polysiloxane and compounding it with graphene, its dispersion effect and compatibility in viscose fiber is improved, combined with silicone antistatic agent, and wet spinning is used Process for preparing modified graphene antistatic viscose fiber.

Benefits of technology

It significantly improves the antistatic and antibacterial properties of the fiber, enhances the dispersion and mechanical properties of graphene, makes the fiber washable, and improves the overall strength and performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007721980000101
    Figure BDA0005007721980000101
  • Figure BDA0005007721980000102
    Figure BDA0005007721980000102
Patent Text Reader

Abstract

The invention relates to the technical field of viscose fibers, in particular to a modified graphene antistatic viscose fiber as well as a preparation method and application thereof. According to the invention, poly (2-vinylpyridine) is grafted on polysiloxane, and then graphene is compounded, so that the antistatic capability of the modified graphene antistatic viscose fiber can be greatly enhanced, the modified graphene antistatic viscose fiber is good in antistatic effect and strong in antibacterial property, the dispersion effect of graphene in the fiber is specifically improved, and the obtained fiber is washable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of viscose fibers, and in particular to a modified graphene antistatic viscose fiber and a preparation method and application thereof. Background Art

[0002] Viscose fiber, also known as viscose fiber or cellulose fiber, is a cellulose fiber obtained by extracting and reshaping fiber molecules from natural wood cellulose. The hygroscopicity of viscose fiber meets the physiological requirements of human skin. It is smooth and cool, breathable, anti-static, UV-proof, colorful, and has good dyeing fastness. It is an authentic plant fiber that has the essence of cotton and the quality of silk. It is often used in the field of clothing and non-woven fabrics. However, there is currently a problem that viscose fiber has poor antistatic properties and is not functional. Traditional functional viscose fibers are mainly achieved by adding additives to viscose fibers or by modifying the fibers. The viscose fibers prepared by this method are not resistant to water washing, and the pollution caused by post-processing is relatively serious, which limits the application of viscose fibers.

[0003] As a new type of two-dimensional nanocarbon material, graphene has excellent properties such as high electrical conductivity, high thermal conductivity, high specific surface area, and excellent mechanical properties. As an ultra-light material, technicians in the textile field are studying how to compound graphene into textile fibers such as viscose fibers to develop new properties and new uses for viscose fibers. Studies have found that adding graphene to polypropylene can give polypropylene good antibacterial and antistatic effects. However, due to the ultra-light properties of graphene, it is difficult to achieve good compatibility and dispersion of graphene with viscose fibers through general mixing processes.

[0004] Silicone antistatic agents can improve the antistatic properties of viscose fibers. The principle of increasing the conductivity of viscose is mainly based on its special chemical structure and properties. First, the organosilicon compounds in silicone antistatic agents contain special polar groups. These groups are easily polarized and adsorb charges with opposite signs under the action of an electric field, which helps to form a conductive film on the surface of the viscose, thereby improving its conductivity. Secondly, the siloxane segments in silicone antistatic agents have excellent flexibility and mobility, which can improve the surface morphology of viscose fibers and make them smoother. This smooth surface helps to reduce friction and reduce the static charge generated by friction. In addition, silicone antistatic agents may also improve the conductivity of viscose fibers by increasing the ion concentration in viscose fibers or improving the distribution of ions in viscose fibers. These ions can migrate and neutralize static charges under the action of an electric field, thereby reducing the accumulation of static electricity.

[0005] Although silicone antistatic agents can exhibit the above-mentioned antistatic effects, there are still many defects in their combination with graphene in the fiber system, such as (1) compatibility issues: the compatibility between graphene and silicone antistatic agents and fiber matrix is ​​poor, resulting in the inability to evenly disperse graphene, affecting the performance of the final composite material. The flake structure of graphene is prone to agglomeration at the interface between silicone and fiber materials; (2) uneven dispersion: Although silicone antistatic agents can provide a certain electrostatic repulsion to help graphene disperse, if the dispersion process is not properly controlled, it may still lead to the agglomeration of graphene and the formation of micro- (3) Interface bonding strength: The interface bonding strength between graphene and the fiber matrix may be weakened due to the intervention of the organosilicon antistatic agent. If the antistatic agent forms a weak boundary layer at the interface, the overall strength and durability of the composite material may be reduced. (4) Processing performance: The addition of organosilicon may affect the rheological properties of the fiber during processing, such as viscosity changes, which may have an adverse effect on processing techniques such as spinning and coating, resulting in increased processing difficulty or unstable product quality.

[0006] It can be seen that the above technical problems in the prior art need to be solved urgently, and a fiber product with good dispersibility and high mechanical properties is needed. Summary of the invention

[0007] The first aspect of the present invention provides a method for preparing a modified graphene antistatic viscose fiber, comprising the following steps:

[0008] S1. Adding a polyether to polymethyl hydrogen siloxane, heating and stirring and adding a catalyst, continuing heating and stirring, cooling and dissolving the crude product in excess toluene, washing with sodium carbonate solution and deionized water, distilling off the solvent, and drying the solid substance in vacuo to obtain a polyether-modified polysiloxane;

[0009] S2. The polyether-modified polysiloxane is added to toluene, triethylamine and 4-dimethylaminopyridine are added, 2-bromoisobutyl bromide dissolved in toluene is added, stirred evenly, the residue is concentrated, precipitated in cold ether, and the precipitate is dried in vacuo to obtain a bromine-containing polyether-modified polysiloxane;

[0010] S3. The bromine-containing polyether-modified polysiloxane, CuBr, CuBr2 and ligand 5,5,7,12,12,14-hexamethyl-1,4,8,11-tetraazacyclotetradecane are uniformly mixed, 2-vinylpyridine, graphene and toluene are added to carry out polymerization reaction, the obtained reactant is precipitated in cold ether, and the precipitate is vacuum dried to obtain polysiloxane-grafted poly(2-vinylpyridine) modified graphene;

[0011] S4. The polysiloxane-grafted poly (2-vinylpyridine) modified graphene is mixed with the viscose fiber spinning solution, and the spun fibers are obtained by wet spinning. The spun fibers are stretched and then cut and post-treated in sequence to obtain modified graphene antistatic viscose fibers.

[0012] In some embodiments, the preparation method comprises the following steps:

[0013] S1. Add polyether to polymethyl hydrogen siloxane, heat to 60-120°C, stir at 100-1000rpm for 10-60min and add catalyst, continue to heat to 60-120°C, stir at 100-1000rpm for 1-6h, and after cooling, dissolve the crude product in excess toluene, wash with sodium carbonate solution and deionized water, distill to remove the solvent, and dry the solid at 40-100°C in vacuum to obtain polyether-modified polysiloxane;

[0014] S2. The polyether-modified polysiloxane is added to toluene, stirred at 100-1000 rpm for 10-120 min, triethylamine and 4-dimethylaminopyridine are added, 2-bromoisobutyl bromide dissolved in toluene is added, and stirred at 20-50 ° C and 100-1000 rpm for 1-48 h. The residue is concentrated and precipitated in cold ether. The precipitate is dried in vacuum at 30-100 ° C to obtain a bromine-containing polyether-modified polysiloxane;

[0015] S3. The bromine-containing polyether-modified polysiloxane, CuBr, CuBr2 and ligand 5,5,7,12,12,14-hexamethyl-1,4,8,11-tetraazacyclotetradecane are uniformly mixed, 2-vinylpyridine, graphene and toluene are added to carry out polymerization reaction at 50-100° C. for 1-24 h, the obtained reactant is precipitated in cold ether, and the precipitate is vacuum dried at 40-100° C. to obtain polysiloxane-grafted poly(2-vinylpyridine) modified graphene;

[0016] S4. The polysiloxane-grafted poly (2-vinylpyridine) modified graphene is mixed with the viscose fiber spinning solution, and the spun fibers are obtained by wet spinning. The spun fibers are stretched and then cut and post-treated in sequence to obtain modified graphene antistatic viscose fibers.

[0017] In some embodiments, the mass ratio of the polymethylhydrogensiloxane to the polyether is 1:(0.5-5).

[0018] In some embodiments, the polyether is allyl alcohol polyoxyalkyl ether.

[0019] In some embodiments, the allyl alcohol polyoxyalkyl ether has a hydroxyl value of 37-53 mgKOH / g, an acid value of 0.1-1.0 mgKOH / g, and a double bond value of 0.1-1.0 mmol / g.

[0020] Furthermore, the hydroxyl value of the allyl alcohol polyoxyalkyl ether is 45 mgKOH / g, the acid value is 0.5 mgKOH / g, and the double bond value is 0.5 mgKOH / g.

[0021] In some embodiments, the catalyst is a solution of chloroplatinic acid dissolved in isopropanol with a mass concentration of 1-20%.

[0022] In some embodiments, the mass concentration of the sodium carbonate solution is 0.1-5%.

[0023] In some embodiments, in S2, the mass ratio of the polyether-modified polysiloxane to toluene is 1:(2-10).

[0024] In some embodiments, in S2, the mass ratio of the polyether-modified polysiloxane to triethylamine is (1-60):1; the mass ratio of the polyether-modified polysiloxane to 4-dimethylaminopyridine is (1-1000):1.

[0025] In some embodiments, in S2, the mass ratio of toluene to 2-bromoisobutyl bromide is (10-100):1.

[0026] In some embodiments, in S2, the mass ratio of the polyether-modified polysiloxane to 2-bromoisobutyl bromide is (1-50):1.

[0027] In some embodiments, in S3, the mass ratio of the bromine-containing polyether modified polysiloxane, CuBr, CuBr2, ligand 5,5,7,12,12,14-hexamethyl-1,4,8,11-tetraazacyclotetradecane, 2-vinylpyridine, graphene and toluene is 1:(0.01-1):(0.001-0.1):(0.1-1):(0.1-5):(0.1-5):(0.1-5).

[0028] In some embodiments, in S4, the mass ratio of the polysiloxane-grafted poly(2-vinylpyridine) modified graphene to the viscose fiber spinning solution is 1:(10-100).

[0029] In some embodiments, in S4, the post-treatment includes sequentially subjecting the cut spun fibers to water washing, desulfurization, acid washing, oiling and drying steps.

[0030] In some embodiments, the method for preparing the viscose fiber spinning solution comprises: pulp is sequentially subjected to impregnation, pressing, crushing, aging, yellowing, dissolution, maturation, filtering, and degassing to obtain the viscose fiber spinning solution.

[0031] The present invention does not impose any special limitation on the preparation method of viscose fiber spinning solution, which can be prepared with reference to the prior art. The specific process includes: the pulp is impregnated with a sodium hydroxide aqueous solution with a concentration of about 18% to convert cellulose into alkali cellulose, dissolve hemicellulose, and partially reduce the degree of polymerization; and then the excess alkali solution is removed by squeezing. The blocky alkali cellulose is crushed on a pulverizer to become a loose flocculent body, and the uniformity of subsequent chemical reactions is improved due to the increase in surface area. Alkali cellulose undergoes oxidative cleavage under the action of oxygen to reduce the average degree of polymerization. This process is called aging. After aging, the alkali cellulose is reacted with carbon disulfide to form cellulose xanthate, which is called xanthation, which further weakens the hydrogen bonds between macromolecules. Due to the hydrophilicity of the xanthate group, the solubility of cellulose xanthate in dilute alkali solution is greatly improved. Dissolving solid cellulose xanthate in dilute alkali solution is viscose. The newly made viscose is difficult to shape due to its high viscosity and salt value. It must be placed at a certain temperature for a certain period of time, which is called ripening, so that the sodium cellulose xanthate in the viscose fiber is gradually hydrolyzed and saponified, the esterification degree is reduced, and the viscosity and stability to electrolytes also change. During ripening, degassing and filtration should be carried out to remove bubbles and impurities.

[0032] The second aspect of the present invention provides a modified graphene antistatic viscose fiber obtained by the above preparation method.

[0033] The third aspect of the present invention provides the application of modified graphene antistatic viscose fiber in textile materials.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. The modified graphene antistatic viscose fiber prepared by the present invention has good antistatic effect and strong antibacterial property, specifically improves the dispersion effect of graphene in the fiber, and the obtained fiber is resistant to water washing.

[0036] 2. The present invention can greatly enhance the antistatic ability of polysiloxane by grafting poly(2-vinylpyridine) on the composite graphene. Polysiloxane, as an organosilicon antistatic agent, has an antistatic effect brought by its structure. Poly(2-vinylpyridine) improves the conductivity of the fiber by introducing the nitrogen-containing functional group of pyridine. These functional groups can interact with the polar groups on the surface of the fiber to form a conductive channel and reduce the generation of static electricity. In addition, pyridine is an aromatic compound and can produce π-π conjugation with graphene, so that graphene and polysiloxane grafted poly(2-vinylpyridine) are closely combined to prevent the agglomeration of graphene on viscose fiber, which can greatly enhance the dispersibility of graphene. Graphene has extremely high conductivity and electrons can flow freely on its surface. Therefore, when static charges are generated, these charges will be evenly distributed on the surface of graphene to avoid the concentration of charges in one area, thereby effectively preventing the generation of static discharge.

[0037] 3. The applicant found that the antistatic performance of the antibacterial material can be greatly enhanced after polysiloxane grafted poly (2-vinylpyridine) modified graphene, and the problem of graphene being easily agglomerated in viscose fiber is solved. This may be because polysiloxane grafted poly (2-vinylpyridine) has good compatibility in viscose fiber, resulting in polysiloxane grafted poly (2-vinylpyridine) modified graphene interacting with the molecular structure of viscose fiber, improving the compatibility between the two, and improving the problems of easy fiber breakage, low fiber strength, and uneven performance caused by uneven dispersion of graphene. It can also significantly improve the compatibility and dispersion stability of polysiloxane grafted poly (2-vinylpyridine) modified graphene with the viscose fiber matrix, thereby ensuring that the corresponding functional effects can be exerted for a long time and stably, and can be washed with water. In addition, the addition of graphene can also make the fiber have certain antibacterial properties.

[0038] 4. The applicant has found that adding polysiloxane to the system of the present invention can also improve the breaking strength of viscose fiber. The silicon-oxygen bond in the polysiloxane molecular chain has a high bond energy, which gives the polysiloxane excellent heat resistance, cold resistance and weather resistance. At the same time, the molecular chain of polysiloxane has good flexibility and is easy to form a uniform dispersion system in the viscose fiber, thereby enhancing the strength and toughness of the viscose fiber. Adding polysiloxane to the system of the present invention can interact with other components in the viscose fiber through physical or chemical effects to form a tighter network structure and improve the breaking strength of the viscose fiber. In addition, polysiloxane can also improve the wettability and fluidity of viscose fiber, making the viscose fiber easier to process and apply, thereby improving the performance and scope of application of the viscose fiber.

[0039] 5. The applicant found that the addition of graphene to viscose can also greatly improve its physical properties. When graphene is added to viscose fiber, it can form a solid support structure inside the material, thereby effectively preventing the expansion of cracks and the occurrence of tearing. Secondly, the lamellar structure of graphene gives it a large specific surface area and excellent interface interaction, allowing it to form a tight bond with other components in the viscose fiber, thereby improving the cohesion of the entire material. When subjected to external forces, these tight bonds can effectively transmit and disperse stress, thereby reducing the risk of local stress concentration and tearing. Further, the polysiloxane grafted poly (2-vinyl pyridine) modified graphene can greatly improve its physical properties in viscose fiber. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The parameters and sources of the substances in the examples and comparative examples of the present invention are as follows:

[0042] Polymethylhydrogensiloxane, purchased from Merck 176206.

[0043] Polyether was purchased from Haian Petrochemical Plant in Jiangsu Province with the brand name of polyether F-6.

[0044] Graphene was purchased from Yuanfeng Chemical Products Company in Zhongyuan District, Zhengzhou City, with brand number 196.

[0045] 5,5,7,12,12,14-hexamethyl 1,4,8,11-tetraazacyclotetradecane is homemade. The preparation method is as follows: add 100 mL of acetone to 11.1 g of 1,2-diaminoethane, stir the mixture and heat it at 45 ° C for about 45 minutes, cool the solution, filter, wash with ice-cold acetone, then wash with ether, and vacuum dry. Dissolve 16 g of the previously vacuum-dried product in 200 mL of methanol, and add 3 g of sodium borohydride to the heated solution, and then heat it in a water bath until the foam stops. Then add potassium hydroxide solution until the pH value of the mixture is about 12, and cool the solution to room temperature and filter. About 50% of the methanol is evaporated, and the resulting solution is cooled in an ice bath. Wash with water. After drying, 5,5,7,12,12,14-hexamethyl 1,4,8,11-tetraazacyclotetradecane is obtained. 1,2-Diaminoethane CAS: 107-15-3,

[0046] The method for preparing viscose fiber spinning stock solution comprises: pulp is sequentially subjected to impregnation, pressing, crushing, aging, yellowing, dissolving, maturing, filtering and degassing to obtain viscose fiber spinning stock solution.

[0047] Example 1

[0048] This embodiment provides a modified graphene antistatic viscose fiber, and the preparation method includes the following steps:

[0049] S1. Add polyether to polymethyl hydrogen siloxane, heat to 70°C, stir at 600rpm for 30min and add catalyst, continue to heat to 95°C, stir at 600rpm for 3h, and after cooling, dissolve the crude product in excess toluene, wash with 0.5% sodium carbonate solution and deionized water, distill to remove the solvent, and dry the solid at 50°C in vacuum to obtain polyether-modified polysiloxane;

[0050] The mass ratio of polymethylhydrogensiloxane to polyether is 1:2;

[0051] The allyl alcohol polyoxyalkyl ether has a hydroxyl value of 45 mgKOH / g, an acid value of 0.5 mgKOH / g, and a double bond value of 0.5 mgKOH / g.

[0052] The catalyst is a chloroplatinic acid solution dissolved in isopropanol, with a mass concentration of 10%, and a mass ratio of the catalyst to hydrogen siloxane of 1:250;

[0053] S2. The polyether-modified polysiloxane was added to toluene, stirred at 600 rpm for 30 min, triethylamine and 4-dimethylaminopyridine were added, 2-bromoisobutyl bromide dissolved in toluene was added, and the mixture was stirred at 25 ° C and 600 rpm for 24 h. The residue was concentrated and precipitated in cold ether. The precipitate was dried in vacuum at 40 ° C to obtain a bromine-containing polyether-modified polysiloxane;

[0054] The mass ratio of polyether-modified polysiloxane to toluene is 1:6;

[0055] The mass ratio of the polyether-modified polysiloxane to triethylamine is 43:1; the mass ratio of the polyether-modified polysiloxane to 4-dimethylaminopyridine is 860:1;

[0056] The mass ratio of toluene to 2-bromoisobutyl bromide is 45:1; the mass ratio of polyether-modified polysiloxane to 2-bromoisobutyl bromide is 20:1;

[0057] S3. The bromine-containing polyether-modified polysiloxane, CuBr, CuBr2 and ligand 5,5,7,12,12,14-hexamethyl-1,4,8,11-tetraazacyclotetradecane were mixed uniformly, 2-vinylpyridine, graphene and toluene were added to carry out polymerization reaction at 70° C. for 12 h, the obtained reactant was precipitated in cold ether, and the precipitate was vacuum dried at 50° C. to obtain polysiloxane-grafted poly(2-vinylpyridine)-modified graphene;

[0058] The mass ratio of bromine-containing polyether modified polysiloxane, CuBr, CuBr2, ligand 5,5,7,12,12,14-hexamethyl-1,4,8,11-tetraazacyclotetradecane, 2-vinylpyridine, graphene and toluene is 1:0.3:0.03:0.18:3:1:2;

[0059] S4. The polysiloxane-grafted poly (2-vinylpyridine) modified graphene is mixed with the viscose fiber spinning solution, and the spun fibers are obtained by wet spinning. The spun fibers are stretched and then cut and post-treated in sequence to obtain modified graphene antistatic viscose fibers.

[0060] The mass ratio of polysiloxane grafted poly (2-vinylpyridine) modified graphene to viscose fiber spinning solution is 1:90.

[0061] The post-treatment includes washing, desulfurization, acid washing, oiling and drying the cut raw fibers in sequence.

[0062] Example 2

[0063] This embodiment provides a modified graphene antistatic viscose fiber, and the preparation method includes the following steps:

[0064] S1. Add polyether to polymethyl hydrogen siloxane, heat to 120°C, stir at 1000rpm for 60min and add catalyst, keep at 120°C, stir at 1000rpm for 6h, cool and dissolve the crude product in excess toluene, wash with 0.5% sodium carbonate solution and deionized water, distill to remove the solvent, and dry the solid at 50°C in vacuum to obtain polyether-modified polysiloxane;

[0065] The mass ratio of polymethyl hydrogen siloxane to polyether is 1:5;

[0066] The allyl alcohol polyoxyalkyl ether has a hydroxyl value of 45 mgKOH / g, an acid value of 0.5 mgKOH / g, and a double bond value of 0.5 mgKOH / g.

[0067] The catalyst is a chloroplatinic acid solution dissolved in isopropanol, with a mass concentration of 20%, and a mass ratio of the catalyst to hydrogen siloxane of 1:20;

[0068] S2. The polyether-modified polysiloxane was added to toluene, stirred at 1000 rpm for 120 min, triethylamine and 4-dimethylaminopyridine were added, 2-bromoisobutyl bromide dissolved in toluene was added, and stirred at 50 ° C and 1000 rpm for 48 h. The residue was concentrated and precipitated in cold ether. The precipitate was dried in vacuum at 100 ° C to obtain a bromine-containing polyether-modified polysiloxane;

[0069] The mass ratio of polyether-modified polysiloxane to toluene is 1:10;

[0070] The mass ratio of the polyether-modified polysiloxane to triethylamine is 1:1; the mass ratio of the polyether-modified polysiloxane to 4-dimethylaminopyridine is 10:1;

[0071] The mass ratio of toluene to 2-bromoisobutyl bromide is 10:1; the mass ratio of polyether-modified polysiloxane to 2-bromoisobutyl bromide is 10:1;

[0072] S3. The bromine-containing polyether-modified polysiloxane, CuBr, CuBr2 and ligand 5,5,7,12,12,14-hexamethyl-1,4,8,11-tetraazacyclotetradecane were mixed evenly, 2-vinylpyridine, graphene and toluene were added to carry out polymerization reaction at 100° C. for 24 h, the obtained reactant was precipitated in cold ether, and the precipitate was vacuum dried at 100° C. to obtain polysiloxane-grafted poly(2-vinylpyridine) modified graphene;

[0073] The mass ratio of bromine-containing polyether-modified polysiloxane, CuBr, CuBr2, ligand 5,5,7,12,12,14-hexamethyl-1,4,8,11-tetraazacyclotetradecane, 2-vinylpyridine, graphene and toluene is 1:0.1:0.01:1:5:5:5;

[0074] S4. The polysiloxane-grafted poly (2-vinylpyridine) modified graphene is mixed with the viscose fiber spinning solution, and the spun fibers are obtained by wet spinning. The spun fibers are stretched and then cut and post-treated in sequence to obtain modified graphene antistatic viscose fibers.

[0075] The mass ratio of polysiloxane grafted poly (2-vinylpyridine) modified graphene to viscose fiber spinning solution is 1:10.

[0076] The post-treatment includes washing, desulfurization, acid washing, oiling and drying the cut raw fibers in sequence.

[0077] Example 3

[0078] The preparation method of this embodiment is the same as that of embodiment 1, except that step S3 does not contain graphene;

[0079] S3. The bromine-containing polyether-modified polysiloxane, CuBr, CuBr2 and ligand 5,5,7,12,12,14-hexamethyl-1,4,8,11-tetraazacyclotetradecane were mixed uniformly, 2-vinylpyridine and toluene were added to carry out polymerization reaction at 70° C. for 12 h, the obtained reactant was precipitated in cold ether, and the precipitate was vacuum dried at 50° C. to obtain polysiloxane-grafted poly(2-vinylpyridine);

[0080] The mass ratio of bromine-containing polyether modified polysiloxane, CuBr, CuBr2, ligand 5,5,7,12,12,14-hexamethyl-1,4,8,11-tetraazacyclotetradecane, 2-vinylpyridine, graphene and toluene is 1:0.3:0.03:0.18:3:2;

[0081] Comparative Example 1

[0082] This comparative example provides a graphene antistatic viscose fiber, the preparation method of which includes: mixing graphene with viscose fiber spinning stock solution, the mass ratio of graphene to viscose fiber spinning stock solution is 1:90. Through wet spinning, primary fibers are obtained, and the primary fibers are cut, washed, desulfurized, pickled, oiled and dried in sequence after being drawn to obtain modified graphene antistatic viscose fibers.

[0083] Comparative Example 2

[0084] The present comparative example provides an antistatic viscose fiber, and the preparation method comprises: subjecting the viscose fiber spinning stock solution to wet spinning to obtain spun fibers, and then subjecting the obtained spun fibers to subsequent cutting, water washing, desulfurization, acid washing, oiling and drying to obtain modified graphene antistatic viscose fibers.

[0085] Comparative Example 3

[0086] The specific implementation of this comparative example is the same as that of Example 1, except that the mass ratio of polymethyl hydrogen siloxane to polyether is 1:4.

[0087] Performance Testing

[0088] The viscose fibers prepared in the above examples and comparative examples were subjected to the following tests:

[0089] Referring to GB / T20944.3-2008 "Oscillating method for evaluating antibacterial properties of textiles", the antibacterial rates of the fibers prepared in the examples and comparative examples after washing for 10, 30 and 50 times were examined. Washing conditions: The fiber samples were immersed and shaken in a 0.2% washing powder solution for 8 minutes each time.

[0090] Resistance: Use a DC resistance meter to test the resistance.

[0091] Dry breaking strength: Use a fiber strength testing machine to test the fiber tensile strength.

[0092] The results of Examples 1-3 are shown in Table 1, and the results of Comparative Examples 1-3 are shown in Table 2.

[0093] Table 1

[0094]

[0095] Table 2

[0096]

[0097] In Example 1, due to the use of polysiloxane grafted poly (2-vinyl pyridine) modified graphene material in viscose fiber, its antistatic ability is greatly enhanced, and the resistance is significantly improved compared with Examples 2-3, and because the modified graphene material is well dispersed in viscose, polysiloxane grafted poly (2-vinyl pyridine) has good compatibility in viscose, resulting in polysiloxane grafted poly (2-vinyl pyridine) modified graphene can interact with the molecular structure of viscose fiber, improving the compatibility of the two, so that the highest resistance and the lowest resistance of the same fiber in Example 1 are slightly different, and the antistatic performance is the strongest. In addition, both graphene and pyridine have strong antibacterial properties, so that the antibacterial effect of Example 1 and the antibacterial effect after multiple washings are better.

[0098] In terms of breaking strength, both graphene and polysiloxane can improve the interaction between viscose and other components through physical or chemical effects, so that viscose fibers form a tighter mesh structure, which greatly improves its breaking strength. In Example 2, due to excessive addition of graphene, a large amount of graphene agglomerates, and the dispersion effect is significantly reduced compared to Example 1, resulting in a significant decrease in its resistance, the difference between the highest and lowest resistances, antibacterial properties, and breaking strength. In Example 3, polysiloxane can improve its antistatic effect as an antistatic agent, but due to the absence of composite graphene, its antistatic effect is significantly different from that of Example 1.

[0099] In Comparative Example 1, graphene was added directly, but it was difficult for the graphene to be completely dispersed in the viscose fiber, resulting in a decrease in its resistance, antibacterial and breaking strength. In Example 5, no additives were added, resulting in poor performance in all aspects.

[0100] In Comparative Example 3, since the mass ratio of polymethylhydrogensiloxane to polyether is 1:4, the polyether is already in great excess, and the reaction can be completed when the mass ratio of polymethylhydrogensiloxane to polyether is 1:2. At this time, increasing the amount of polyether has almost no effect on its resistance, antibacterial and breaking strength.

[0101] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing modified graphene antistatic viscose fiber, characterized in that: The steps include: S1. Adding a polyether to polymethyl hydrogen siloxane, heating and stirring and adding a catalyst, continuing heating and stirring, cooling and dissolving the crude product in excess toluene, washing with sodium carbonate solution and deionized water, distilling off the solvent, and drying the solid substance in vacuo to obtain a polyether-modified polysiloxane; S2. The polyether-modified polysiloxane is added to toluene, triethylamine and 4-dimethylaminopyridine are added, 2-bromoisobutyl bromide dissolved in toluene is added, stirred evenly, the residue is concentrated, precipitated in cold ether, and the precipitate is dried in vacuo to obtain a bromine-containing polyether-modified polysiloxane; S3. The bromine-containing polyether-modified polysiloxane, CuBr, CuBr2 and ligand 5,5,7,12,12,14-hexamethyl-1,4,8,11-tetraazacyclotetradecane are uniformly mixed, 2-vinylpyridine, graphene and toluene are added to carry out polymerization reaction, the obtained reactant is precipitated in cold ether, and the precipitate is vacuum dried to obtain polysiloxane-grafted poly(2-vinylpyridine) modified graphene; S4. The polysiloxane-grafted poly (2-vinylpyridine) modified graphene is mixed with the viscose fiber spinning solution, and the spun fibers are obtained by wet spinning. The spun fibers are stretched and then cut and post-treated in sequence to obtain modified graphene antistatic viscose fibers.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the polymethyl hydrogen siloxane to the polyether is 1:(0.5-5).

3. The preparation method according to claim 2, characterized in that: The polyether is allyl alcohol polyoxyalkyl ether.

4. The preparation method according to claim 3, characterized in that: The allyl alcohol polyoxyalkyl ether has a hydroxyl value of 37-53 mgKOH / g, an acid value of 0.1-1.0 mgKOH / g, and a double bond value of 0.1-1.0 mmol / g.

5. The preparation method according to claim 4, characterized in that: In S2, the mass ratio of the polyether-modified polysiloxane to triethylamine is (1-60):1; the mass ratio of the polyether-modified polysiloxane to 4-dimethylaminopyridine is (1-1000):

1.

6. The preparation method according to claim 5, characterized in that: In S2, the mass ratio of the polyether-modified polysiloxane to 2-bromoisobutyl bromide is (1-50):

1.

7. The preparation method according to claim 6, characterized in that: In S3, the mass ratio of the bromine-containing polyether modified polysiloxane, CuBr, CuBr2, ligand 5,5,7,12,12,14-hexamethyl-1,4,8,11-tetraazacyclotetradecane, 2-vinylpyridine, graphene and toluene is 1:(0.01-1):(0.001-0.1):(0.1-1):(0.1-5):(0.1-5):(0.1-5).

8. The preparation method according to claim 7, characterized in that: In S4, the mass ratio of the polysiloxane-grafted poly(2-vinylpyridine) modified graphene to the viscose fiber spinning solution is 1:(10-100).

9. A modified graphene antistatic viscose fiber, characterized in that: Obtained by the preparation method according to any one of claims 1 to 8.

10. Application of the modified graphene antistatic viscose fiber according to claim 9 in textile materials.

Citation Information

Patent Citations

  • Grapheme-containing viscose fiber and preparation method thereof

    CN104328523A

  • Tetraazacyclo tetradecane derived ligand complex and its synthesis process

    CN1706856A

  • Initiator Integrated Poly (Dimethylsiloxane) and Methods for Making the Same and Its Application

    US20120283394A1

Cited By

  • Graphene conductive adhesive and preparation method thereof

    CN119979085A