Method for stabilizing ferroelectric phase in high-quality epitaxial Hf0. 5Zr0. 5O2 single crystal film

By preheating the YSZ (001) single crystal substrate and pulse laser deposition technology to grow Hf0.5Zr0.5O2 single crystal thin films and performing rapid annealing, the problem of ferroelectric instability of HfO2-based thin films was solved and high-performance The growth of quality epitaxial films and the stabilization of the ferroelectric phase promote the development of high-performance memory devices.

CN118800643APending Publication Date: 2024-10-18SONGSHAN LAKE MATERIALS LAB +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410936582.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing HfO2-based films generally have polycrystalline and multiphase structures, which lead to ferroelectric instability and limit their large-scale and stable application in semiconductor devices.

Method used

YSZ (001) single crystal substrate is used for preheating treatment, and a 50nm-150nm thick Hf0.5Zr0.5O2 single crystal film is grown by pulse laser deposition method, followed by rapid annealing to obtain Hf0.5Zr0 with stable polar state. .5O2 single crystal film.

Benefits of technology

The growth of high-quality epitaxial Hf0.5Zr0.5O2 single crystal thin film is achieved. The ferroelectric phase is stabilized at the anti-phase domain boundary in the film, which improves the macroscopic ferroelectricity and performance of the film and promotes high-performance and stable ferroelectric memory devices. development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118800643A_ABST
    Figure CN118800643A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor films, in particular to a method for stabilizing a ferroelectric phase in a high-quality epitaxial Hf0. 5Zr0. 5O2 single crystal film. The method comprises the following steps: step S1, carrying out preheating treatment on a YSZ (001) single crystal substrate; s2, epitaxially growing a thin film with the thickness of 50nm to 150nm on the preheated YSZ (001) single crystal substrate by adopting a pulse laser deposition method; and S3, carrying out rapid annealing treatment on the thin film at an annealing rate of 20 DEG C / min to 30 DEG C / min to obtain the Hf0. 5Zr0. 5O2 single crystal thin film with a stable ferroelectric phase. The Hf < 0.5 > Zr < 0.5 > O < 2 > thin film prepared by the method is a single-crystal thin film and has extremely high epitaxy in the [001] direction, and the Hf < 0.5 > Zr < 0.5 > O < 2 > thin film / substrate interface is of a completely coherent structure without dislocation; based on interface engineering, the stability of a novel ferroelectric phase is realized at an anti-phase domain boundary in the Hf < 0.5 > Zr < 0.5 > O < 2 > thin film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor thin films, and in particular to a method for producing high-quality epitaxial Hf 0.5 Zr 0.5 Methods for stabilizing the ferroelectric phase in O2 single crystal thin films. Background Art

[0002] The rapid development of big data, the Internet of Things, and artificial intelligence has put forward higher and higher requirements on the performance of memory chips, logic chips, and other electronic components. Storage materials are the medium of data, and high-performance storage materials are the key to determining the performance of electronic components. Ferroelectric thin films have spontaneous ferroelectric polarization that can be flipped under an external field and are a storage material with great application potential. Since the ferroelectricity of hafnium oxide (HfO2)-based thin films was discovered in 2011, it has become a current research hotspot due to its high compatibility with complementary metal oxide semiconductor (CMOS) processes and anti-critical size effect. Researchers have made outstanding progress in the growth and preparation of HfO2-based thin films and the regulation of ferroelectricity. However, the HfO2-based thin films currently studied are generally polycrystalline and multi-phase structures, and there are many complex grain boundaries, interfaces, and defects in the film, which have an adverse effect on the macroscopic properties of the film, such as ferroelectricity, fatigue, and retention, which greatly limits the large-scale and stable application of HfO2-based thin films in semiconductor devices.

[0003] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a high-quality epitaxial Hf 0.5 Zr 0.5 The method of stabilizing the ferroelectric phase in O2 single crystal thin films is aimed at solving the problem of unstable ferroelectricity of existing HfO2-based thin films.

[0005] The technical solution of the present invention is as follows:

[0006] The first aspect of the present invention provides a method for producing a high quality epitaxial Hf 0.5 Zr 0.5 A method for stabilizing a ferroelectric phase in an O2 single crystal thin film, comprising:

[0007] Step S1, preheating the YSZ (001) single crystal substrate;

[0008] Step S2, epitaxially growing a thin film with a thickness of 50 nm to 150 nm on the preheated YSZ (001) single crystal substrate by a pulsed laser deposition method;

[0009] Step S3, performing rapid annealing treatment on the film at an annealing rate of 20°C / min-30°C / min to obtain Hf 0.5 Zr 0.5 O2 single crystal thin film.

[0010] Optionally, before step S1, the method further includes: immersing the YSZ (001) single crystal substrate in alcohol for 2 hours to 4 hours.

[0011] Optionally, the step S1 specifically includes: placing a YSZ (001) single crystal substrate into a pulsed laser deposition system chamber, heating it to 850-900° C. and then maintaining the temperature for 0.5 h-1 h.

[0012] Optionally, the temperature is increased to 850-900° C. at a heating rate of 10-15° C. / min and then maintained at that temperature for 0.5 h-1 h.

[0013] Optionally, the step S2 specifically includes:

[0014] A 50nm-150nm thick film is epitaxially grown on a preheated YSZ (001) single crystal substrate at a temperature of 830-850°C and an oxygen pressure of 90mTorr-120mTorr at a sputtering rate of 2Hz-4Hz.

[0015] Optionally, the step S2 specifically includes:

[0016] The temperature is kept at 830-850°C for 10-30 minutes, and then a 50nm-150nm thick film is epitaxially grown on a YSZ (001) single crystal substrate at a temperature of 830-850°C and an oxygen pressure of 90mTorr-120mTorr at a sputtering rate of 2Hz-4Hz.

[0017] Optionally, the step S3 specifically includes:

[0018] Before annealing, the film is kept warm for 20-30 minutes, and then the film is rapidly annealed under the conditions of 120-200 Torr oxygen partial pressure in the pulse laser deposition system chamber and 20-30 ° C / min annealing rate, and cooled to room temperature to obtain ferroelectric phase-stable Hf 0.5 Zr 0.5 O2 single crystal thin film.

[0019] Optionally, the Hf 0.5 Zr 0.5 There is a stable ferroelectric phase at the antiphase domain boundary in O2 single crystal film.

[0020] Optionally, the high quality epitaxial Hf 0.5 Zr 0.5The method for stabilizing the ferroelectric phase in an O2 single crystal thin film comprises the following specific steps:

[0021] Soak the YSZ (001) single crystal substrate in alcohol for 2h-4h, put the taken-out YSZ (001) single crystal substrate into the pulse laser deposition system chamber, heat it to 850-900℃ and keep it warm for 0.5h-1h;

[0022] The temperature is lowered from 850-900°C to 830-850°C, and kept at 830-850°C for 10-30 minutes, and then a 50nm-150nm thick film is epitaxially grown on a YSZ (001) single crystal substrate at a temperature of 830-850°C and an oxygen pressure of 90mTorr-120mTorr at a sputtering rate of 2Hz-4Hz;

[0023] Before annealing, the film is kept warm for 20-30 minutes, and then the film is rapidly annealed under the conditions of 120-200 Torr oxygen partial pressure in the pulse laser deposition system chamber and 20-30 ° C / min annealing rate, and cooled to room temperature to obtain ferroelectric phase-stable Hf 0.5 Zr 0.5 O2 single crystal thin film.

[0024] The second aspect of the present invention provides a ferroelectric phase-stable Hf 0.5 Zr 0.5 O2 single crystal thin film, wherein it is prepared by the method described in the present invention.

[0025] Beneficial effect: The present invention provides a high-quality epitaxial Hf 0.5 Zr 0.5 The method of stabilizing the ferroelectric phase in the O2 single crystal film is to use a specific commercial single crystal substrate, preheat the single crystal substrate, use pulsed laser deposition technology to deposit a film of a specific thickness, and after rapid annealing, obtain a high-quality HZO single crystal film with high crystallinity and epitaxy, and no defects at the interface; the ferroelectric phase is stabilized at the high-density antiphase domain boundary in the HZO single crystal film. From a social and economic perspective, the growth of high-quality epitaxial HZO single crystal films and the stabilization of the ferroelectric phase at the antiphase domain boundary are of great significance for understanding the structural origin of the ferroelectricity of HZO films, improving the macroscopic ferroelectricity of films, and obtaining high-performance and stable ferroelectric memory devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the θ-2θ curve of the X-ray diffraction of the epitaxial HZO film in Example 1.

[0027] Figure 2This is the rocking curve of the (001) peak of the X-ray diffraction of the epitaxial HZO thin film in Example 1.

[0028] Figure 3 This is a high-resolution X-ray diffraction reciprocal space scan of the epitaxial HZO film in Example 1.

[0029] Figure 4 This is the atomic force microscope morphology image of the epitaxial HZO film in Example 1.

[0030] Figure 5 This is the selected area electron diffraction pattern of the epitaxial HZO film of Example 1 along the

[100] crystal zone axis.

[0031] Figure 6 For example 1, epitaxial HZO thin film is grown along Selected area electron diffraction pattern of the crystal zone axis.

[0032] Figure 7 This is the selected area electron diffraction pattern of the epitaxial HZO film of Example 1 along the

[001] crystal zone axis.

[0033] Figure 8 This is a low-magnification TEM bright-field image of the epitaxial HZO film in Example 1.

[0034] Fig. 9 This is a low-magnification HAADF-STEM high-resolution image of the epitaxial HZO film in Example 1.

[0035] Fig.10 These are the atomic scale HAADF-STEM high-resolution images and iDPC-STEM high-resolution images of the epitaxial HZO film in Example 1.

[0036] Fig.11 A is the atomic scale HAADF-STEM high-resolution image of the epitaxial HZO film in Example 1, B is the two-dimensional intensity distribution diagram of the Hf element in the epitaxial HZO film in Example 1 at the atomic scale, and C is the two-dimensional intensity distribution diagram of the Zr element in the epitaxial HZO film in Example 1 at the atomic scale.

[0037] Fig.12 This is the atomic scale HAADF-STEM high-resolution image of the epitaxial HZO film in comparison with Example 1.

[0038] Fig.13 This is the atomic scale HAADF-STEM high-resolution image of the epitaxial HZO film in comparative example 2.

[0039] Fig.14 This is a low-magnification HAADF-STEM image of the TEM plane sample of the epitaxial HZO film in Example 1.

[0040] Fig.15These are the atomic-scale HAADF-STEM high-resolution images and iDPC-STEM high-resolution images at the antiphase domain boundary in the epitaxial HZO film in Example 1.

[0041] Fig.16 The local butterfly curve (amplitude-voltage curve) and hysteresis loop (phase-voltage curve) of the epitaxial HZO film of Example 1 measured by piezoelectric force microscope.

[0042] Fig.17 This is an atomic scale HAADF-STEM high-resolution image of a TEM cross-section sample of the epitaxial HZO thin film of comparative example 3.

[0043] Fig.18 This is the atomic scale iDPC-STEM high-resolution image of the TEM plane sample of the epitaxial HZO film in comparative example 3. DETAILED DESCRIPTION

[0044] The present invention provides a high-quality epitaxial Hf 0.5 Zr 0.5 Method for stabilizing ferroelectric phase in O2 single crystal thin film, in order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0045] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0046] The embodiment of the present invention provides a method for high-quality epitaxial Hf 0.5 Zr 0.5 A method for stabilizing a ferroelectric phase in an O2 (HZO) single crystal thin film, comprising the steps of:

[0047] Step S1, preheating the YSZ (001) single crystal substrate;

[0048] Step S2, epitaxially growing a thin film with a thickness of 50 nm to 150 nm on the preheated YSZ (001) single crystal substrate by a pulsed laser deposition method;

[0049] Step S3, performing rapid annealing treatment on the film at an annealing rate of 20°C / min-30°C / min to obtain a ferroelectric phase-stable Hf 0.5 Zr 0.5O2 single crystal thin film (Zr-doped HfO2 thin film, abbreviated as HZO thin film).

[0050] In an embodiment of the present invention, by selecting a specific YSZ (001) single crystal substrate, which has a fluorite structure similar to that of the HZO film, the epitaxial growth of the HZO film and the acquisition of a single crystal structure can be ensured; and the YSZ (001) single crystal substrate is subjected to a high-temperature preheating treatment, the potential defects and contaminants on the surface of the YSZ (001) single crystal substrate can be reduced, and a high-quality, atomically flat YSZ (001) single crystal substrate surface is obtained, thereby improving the epitaxy and growth quality of the HZO single crystal film. In addition, by using a high-precision pulsed laser deposition technique, the physical deposition method can further ensure the epitaxy and growth quality of the HZO single crystal film. In addition, by growing a HZO single crystal film of a specific thickness, it is ensured that a high-density antiphase domain boundary structure exists in the HZO single crystal film, and the existence of the antiphase domain boundary can ensure the stability of the polarity state at the domain boundary.

[0051] It is also important to emphasize that the research found that high temperature preheating of the YSZ (001) single crystal substrate before HZO single crystal film deposition and rapid annealing after deposition are beneficial to improving the epitaxial coherence of HZO single crystal films. Moreover, compared with slow annealing of thin HZO single crystal films, rapid annealing of thick HZO single crystal films is more conducive to the formation of antiphase boundaries, thereby stabilizing the ferroelectric phase at the antiphase boundaries.

[0052] By using the preparation method of the embodiment of the present invention, a high-quality HZO single crystal film is prepared with high-density antiphase boundaries, thereby stabilizing the ferroelectric phase at the antiphase boundaries. From a social and economic perspective, the preparation of the HZO single crystal film is of great significance for clarifying the structural mechanism of the ferroelectricity of HfO2-based films and further designing high-performance, stable silicon-based semiconductor memory devices.

[0053] Furthermore, before step S1, the process further includes: immersing the YSZ (001) single crystal substrate in alcohol for 2 hours to 4 hours, such as 2 hours, 3 hours or 4 hours, but not limited thereto. YSZ (001) refers to yttrium-stabilized zirconia with a

[001] orientation.

[0054] Further, the step S1 specifically includes: placing the YSZ (001) single crystal substrate into a pulsed laser deposition system chamber, heating it to 850-900°C (such as 900°C), and then keeping it warm for 0.5h-1h, such as 0.5h, 0.8h or 1h, but not limited thereto. The temperature is raised to 850-900°C at a heating rate of 10-15°C / min (such as 15°C / min).

[0055] Furthermore, the step S2 specifically includes:

[0056] A 50nm-150nm thick film is epitaxially grown on a preheated YSZ (001) single crystal substrate at a temperature of 830-850°C (eg 830°C) and an oxygen pressure of 90mTorr-120mTorr at a sputtering rate of 2Hz-4Hz.

[0057] Furthermore, the step S2 specifically includes:

[0058] Keep the temperature at 830-850℃ for 10-30min, then epitaxially grow a 50nm-150nm thick film on a YSZ (001) single crystal substrate at a temperature of 830-850℃ and an oxygen pressure of 90mTorr-120mTorr at a sputtering rate of 2Hz-4Hz. The sputtering target is Hf 0.5 Zr 0.5 O2, the sputtering atmosphere is an oxygen pressure atmosphere of 90mTorr-120mTorr.

[0059] Furthermore, the step S3 specifically includes:

[0060] Before annealing, the film is kept warm for 20-30 minutes, and then the film is rapidly annealed under the condition that the oxygen partial pressure environment of the pulse laser deposition system chamber is 120-200 Torr (such as 200 Torr, etc.) and the annealing rate is 20°C / min-30°C / min, and the temperature is cooled to room temperature (such as 15°C-25°C) to obtain a ferroelectric phase-stable Hf 0.5 Zr 0.5 O2 single crystal thin film.

[0061] In a specific embodiment, the high-quality epitaxial Hf 0.5 Zr 0.5 The method for stabilizing the ferroelectric phase in an O2 single crystal thin film comprises the following specific steps:

[0062] Soak the YSZ (001) single crystal substrate in alcohol for 2h-4h, put the taken-out YSZ (001) single crystal substrate into the pulse laser deposition system chamber, heat it to 850-900℃ and keep it warm for 0.5h-1h;

[0063] The temperature is lowered from 850-900°C to 830-850°C, and kept at 830-850°C for 10-30 minutes, and then a 50nm-150nm thick film is epitaxially grown on a YSZ (001) single crystal substrate at a temperature of 830-850°C and an oxygen pressure of 90mTorr-120mTorr at a sputtering rate of 2Hz-4Hz;

[0064] Before annealing, the film is kept warm for 20-30 minutes, and then the film is rapidly annealed under the conditions of 120-200 Torr oxygen partial pressure in the pulse laser deposition system chamber and 20-30 ° C / min annealing rate, and cooled to room temperature to obtain ferroelectric phase-stable Hf 0.5 Zr 0.5 O2 single crystal thin film.

[0065] The embodiment of the present invention also provides a ferroelectric phase-stable Hf 0.5 Zr 0.5 O2 single crystal thin film, wherein it is prepared by the method described in the embodiment of the present invention.

[0066] The embodiment of the present invention uses

[001] oriented yttrium-stabilized zirconium oxide as a substrate, removes pollutants and defects on the substrate surface by preheating the substrate in a pulsed laser deposition chamber, then deposits a Zr-doped HfO2 film of a specific thickness under a specific oxygen atmosphere and deposition rate, and then performs a rapid annealing process to obtain a high-quality single crystal Zr-doped HfO2 epitaxial film. The high-density antiphase boundary in the film promotes the stability of the ferroelectric phase in the film.

[0067] The present invention will be further described below by means of specific examples.

[0068] Example 1

[0069] A high-quality epitaxial Hf 0.5 Zr 0.5 O2 single crystal thin film, wherein the polar state is stabilized at the high-density antiphase domain boundary, and the preparation method comprises the following steps:

[0070] S1: Soak the commercial YSZ (001) single crystal substrate in alcohol for 2 hours, then put the taken-out YSZ (001) single crystal substrate into the pulsed laser deposition system chamber, heat it to 900 °C at a heating rate of 15 °C / min and keep it at that temperature for 1 hour.

[0071] S2: The temperature was lowered from 900°C to the deposition temperature of 830°C at a cooling rate of 10°C / min and kept at this temperature for 10 minutes. Subsequently, a 50 nm thick HZO film was epitaxially deposited on a YSZ (001) single crystal substrate at a temperature of 830°C and an oxygen pressure of 90 mTorr at a sputtering rate of 2 Hz using pulsed laser deposition technology.

[0072] S3: After the HZO film deposition is completed, the temperature is kept for 30 minutes, and then the temperature is cooled to room temperature under the conditions of a chamber oxygen partial pressure environment of 200 Torr and an annealing rate of 30°C / min to obtain a high-quality epitaxial HZO single crystal film.

[0073] Comparative Example 1

[0074] S1: Soak the commercial YSZ (001) single crystal substrate in alcohol for 2 hours, and then put the taken out YSZ (001) single crystal substrate into the pulsed laser deposition system chamber.

[0075] S2: The temperature was raised from room temperature to the deposition temperature of 830°C at a rate of 15°C / min and kept at this temperature for 10 minutes. Subsequently, a 50 nm thick HZO film was epitaxially deposited on a YSZ (001) single crystal substrate at a temperature of 830°C and an oxygen pressure of 90 mTorr at a sputtering rate of 2 Hz using pulsed laser deposition technology.

[0076] S3: After the HZO film deposition is completed, the temperature is kept for 30 minutes, and then the temperature is cooled to room temperature under the conditions of a chamber oxygen partial pressure environment of 200 Torr and an annealing rate of 5°C / min to obtain a high-quality epitaxial HZO single crystal film.

[0077] Comparative Example 2

[0078] S1: Soak the commercial KTaO3 (KTO) (001) single crystal substrate in alcohol for 2 hours, then put the taken out KTO (001) single crystal substrate into the pulsed laser deposition system chamber, heat it to 900°C at a heating rate of 15°C / min and keep it at that temperature for 1 hour.

[0079] S2: The temperature was lowered from 900°C to the deposition temperature of 830°C at a cooling rate of 10°C / min and kept at this temperature for 10 minutes. Subsequently, a 50 nm thick HZO film was epitaxially deposited on a YSZ (001) single crystal substrate at a temperature of 830°C and an oxygen pressure of 90 mTorr at a sputtering rate of 2 Hz using pulsed laser deposition technology.

[0080] S3: After the HZO film deposition is completed, the temperature is kept for 30 minutes, and then the temperature is cooled to room temperature under the conditions of a chamber oxygen partial pressure environment of 200 Torr and an annealing rate of 30°C / min to obtain a high-quality epitaxial HZO single crystal film.

[0081] Comparative Example 3

[0082] S1: Soak the commercial YSZ (001) single crystal substrate in alcohol for 2 hours, then put the taken-out YSZ (001) single crystal substrate into the pulsed laser deposition system chamber, heat it to 900 °C at a heating rate of 15 °C / min and keep it at that temperature for 1 hour.

[0083] S2: The temperature was lowered from 900°C to the deposition temperature of 830°C at a cooling rate of 10°C / min and kept at this temperature for 10 minutes. Subsequently, a 11 nm thick HZO film was epitaxially deposited on a YSZ (001) single crystal substrate using pulsed laser deposition technology at a temperature of 830°C and an oxygen pressure of 90 mTorr at a sputtering rate of 2 Hz.

[0084] S3: After the HZO film deposition is completed, the temperature is kept for 30 minutes, and then the temperature is cooled to room temperature under the conditions of a chamber oxygen partial pressure environment of 200 Torr and an annealing rate of 5°C / min to obtain a high-quality epitaxial HZO single crystal film.

[0085] Test equipment: X-ray diffraction θ-2θ curves, rocking curves and high-resolution reciprocal space scans were measured by X'Pert3 MRD XRD equipment from Malvern Panalytical, UK; TEM bright field images were characterized by a transmission electron microscope, model JEM-F200, from JEOL, Japan;

[0086] HAADF-STEM and iDPC-STEM were measured using a Spectra 300 double-aberration-corrected transmission electron microscope from ThermoFisher, USA.

[0087] Test results:

[0088] Figure 1-Figure 3 The X-ray diffraction characterization result of Example 1 shows that the HZO film is a high-quality epitaxial single crystal film with extremely low defect density.

[0089] Figure 4 This is an atomic force microscope morphology image of Example 1. The average roughness of the HZO film is 762 pm, indicating that the surface of the grown HZO film has high flatness.

[0090] Figure 5 , Figure 6 and Figure 7 They are respectively along the film of Example 1

[100] , The selected area electron diffraction patterns of the

[001] and

[001] zone axes indicate the single crystal nature and high epitaxial quality of the HZO film.

[0091] Figure 8 , Fig. 9 They are the TEM bright field image and HAADF-STEM high-resolution image of the film in Example 1, which show that the film has a smooth interface, high epitaxy and no defects.

[0092] Fig.10 These are the atomic scale HAADF-STEM high-resolution images and iDPC-STEM high-resolution images of the film in Example 1. Fig.11 A is an atomic scale HAADF-STEM high-resolution image of the thin film of Example 1, B is a two-dimensional intensity distribution diagram of the Hf element in the thin film of Example 1 at the atomic scale, and C is a two-dimensional intensity distribution diagram of the Zr element in the thin film of Example 1 at the atomic scale. Figure 10-11 Displays the crystal structure and element distribution of the film.

[0093] Fig.12 For the atomic scale HAADF-STEM high resolution image of Example 1, there is a black contrast between the YSZ (001) single crystal substrate and the HZO film, indicating that the epitaxial coherence of the HZO film is low. Fig. 9 ) and Comparative Example 1 ( Fig.12 ), both are HZO films epitaxially grown on commercial YSZ (001) single crystal substrates. High-temperature preheating of the YSZ (001) single crystal substrate before film deposition and rapid annealing after deposition are beneficial to improving the epitaxial coherence of the HZO films.

[0094] Fig.13 For the atomic scale HAADF-STEM high-resolution image of the film in Example 2, multiple grains can be clearly seen inside the film, there are many defects in the film, and the epitaxy of the HZO film and the KTO (001) single crystal substrate is poor. By comparing Example 1 ( Fig. 9 ) and Comparative Example 2 ( Fig.13 ), the commercial single crystal substrate was also preheated before deposition. Compared with the KTO (001) single crystal substrate, the YSZ (001) single crystal substrate was more conducive to the growth of high-quality single crystal HZO epitaxial thin films.

[0095] Fig.14 , Fig.15 They are respectively the low-magnification HAADF-STEM image of the TEM plane sample of the film in Example 1, the atomic-scale HAADF-STEM high-resolution image at the antiphase domain boundary, and the iDPC-STEM high-resolution image, indicating the existence of high-density antiphase domain boundaries in the HZO film; the crystal structure and atomic distribution at the antiphase domain boundary are different from those of the HZO film on both sides of the boundary, and have polarity.

[0096] Fig.16 The local butterfly curve (A) and hysteresis loop (B) measured for the thin film sample of Example 1 show the ferroelectric properties of the local area of ​​the film.

[0097] Fig.17 , Fig.18 The atomic scale HAADF-STEM high resolution images and iDPC-STEM high resolution images of the TEM cross-section sample and TEM plane sample of the film of Comparative Example 3 are shown respectively. By comparing Example 1 and Comparative Example 3, both are HZO films epitaxially grown on commercial YSZ (001) single crystal substrates, and both are the same substrate pretreatment process. Compared with the thin HZO film annealed at a slow rate, the thick HZO film annealed at a fast rate is more conducive to the formation of antiphase domain boundaries, thereby stabilizing the ferroelectric phase at the antiphase domain boundaries.

[0098] In summary, the present invention provides a method for growing high-quality epitaxial Hf 0.5 Zr 0.5 Method for stabilizing ferroelectric phase in O2 single crystal thin film, Hf 0.5 Zr 0.5 O2 thin film is a single crystal thin film with extremely high epitaxiality along the

[001] direction. 0.5 Zr 0.5 The O2 film / substrate interface is a completely coherent structure with no dislocations. Based on interface engineering, the Hf 0.5 Zr 0.5 The stability of a new ferroelectric phase is achieved at the antiphase domain boundaries within the O2 film.

[0099] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A method for high-quality epitaxial Hf 0.5 Zr 0.5 A method for stabilizing a ferroelectric phase in an O2 single crystal thin film, characterized in that: include: Step S1, preheating the YSZ (001) single crystal substrate; Step S2, epitaxially growing a thin film with a thickness of 50 nm to 150 nm on the preheated YSZ (001) single crystal substrate by a pulsed laser deposition method; Step S3, performing rapid annealing treatment on the film at an annealing rate of 20°C / min-30°C / min to obtain a ferroelectric phase-stable Hf 0.5 Zr 0.5 O2 single crystal thin film.

2. The high quality epitaxial Hf according to claim 1 0.5 Zr 0.5 A method for stabilizing a ferroelectric phase in an O2 single crystal thin film, characterized in that: Before step S1, the method further includes: immersing the YSZ (001) single crystal substrate in alcohol for 2 hours to 4 hours.

3. The method according to claim 1 or 2 for high quality epitaxial Hf 0.5 Zr 0.5 A method for stabilizing a ferroelectric phase in an O2 single crystal thin film, characterized in that: The step S1 specifically includes: placing a YSZ (001) single crystal substrate into a pulsed laser deposition system chamber, heating it to 850-900° C. and then maintaining the temperature for 0.5 h to 1 h.

4. The high quality epitaxial Hf according to claim 3 0.5 Zr 0.5 A method for stabilizing a ferroelectric phase in an O2 single crystal thin film, characterized in that: Heat to 850-900°C at a heating rate of 10-15°C / min and keep warm for 0.5h-1h.

5. The high quality epitaxial Hf according to claim 1 0.5 Zr 0.5 A method for stabilizing a ferroelectric phase in an O2 single crystal thin film, characterized in that: The step S2 specifically includes: A 50nm-150nm thick film is epitaxially grown on a preheated YSZ (001) single crystal substrate at a temperature of 830-850°C and an oxygen pressure of 90mTorr-120mTorr at a sputtering rate of 2Hz-4Hz.

6. The method according to claim 1 or 5 for high quality epitaxial Hf 0.5 Zr 0.5 A method for stabilizing a ferroelectric phase in an O2 single crystal thin film, characterized in that: The step S2 specifically includes: The temperature is kept at 830-850°C for 10-30 minutes, and then a 50nm-150nm thick film is epitaxially grown on a YSZ (001) single crystal substrate at a temperature of 830-850°C and an oxygen pressure of 90mTorr-120mTorr at a sputtering rate of 2Hz-4Hz.

7. The high quality epitaxial Hf according to claim 1 0.5 Zr 0.5 A method for stabilizing a ferroelectric phase in an O2 single crystal thin film, characterized in that: The step S3 specifically includes: Before annealing, the film is kept warm for 20-30 minutes, and then the film is rapidly annealed under the conditions of 120-200 Torr oxygen partial pressure in the pulse laser deposition system chamber and 20-30 ° C / min annealing rate, and cooled to room temperature to obtain ferroelectric phase-stable Hf 0.5 Zr 0.5 O2 single crystal thin film.

8. The high quality epitaxial Hf according to claim 1 0.5 Zr 0.5 A method for stabilizing a ferroelectric phase in an O2 single crystal thin film, characterized in that: The Hf 0.5 Zr 0.5 There is a stable ferroelectric phase at the antiphase domain boundary in O2 single crystal film.

9. The high quality epitaxial Hf according to claim 1 0.5 Zr 0.5 A method for stabilizing a ferroelectric phase in an O2 single crystal thin film, characterized in that: The specific steps are: Soak the YSZ (001) single crystal substrate in alcohol for 2h-4h, put the taken-out YSZ (001) single crystal substrate into the pulse laser deposition system chamber, heat it to 850-900℃ and keep it warm for 0.5h-1h; The temperature is lowered from 850-900°C to 830-850°C, and kept at 830-850°C for 10-30 minutes, and then a 50nm-150nm thick film is epitaxially grown on a YSZ (001) single crystal substrate at a temperature of 830-850°C and an oxygen pressure of 90mTorr-120mTorr at a sputtering rate of 2Hz-4Hz; Before annealing, the film is kept warm for 20-30 minutes, and then the film is rapidly annealed under the conditions of 120-200 Torr oxygen partial pressure in the pulse laser deposition system chamber and 20-30 ° C / min annealing rate, and cooled to room temperature to obtain ferroelectric phase-stable Hf 0.5 Zr 0.5 O2 single crystal thin film.

10. A ferroelectric phase-stabilized Hf 0.5 Zr 0.5 O2 single crystal thin film, characterized in that The method is prepared by any one of claims 1 to 9.

Citation Information

Cited By

  • Gadolinium oxide single crystal film with ultra-wide bandgap and preparation method and application thereof

    CN119571456B