Synthesis of * MRE framework type molecular sieves

By using 1-ethylpyridinium cation as an organic structure directing agent and combining silicon and aluminum atom sources, the *MRE framework molecular sieve was successfully synthesized, which solved the problem of *MRE framework molecular sieve synthesis in the existing technology and realized the synthesis of catalyst components. Efficient preparation and stable catalytic performance.

CN118804893APending Publication Date: 2024-10-18CHEVRON USA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024818.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-02-15
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

It is difficult to effectively synthesize a disordered *MRE framework molecular sieve with one-dimensional 10-ring channels using existing technology, and the synthesis methods of catalyst components are limited.

Method used

Using an organic structure directing agent containing 1-ethylpyridinium cation, combined with a silicon atom source, an aluminum atom source, an alkali metal source and a hydroxide ion source, the *MRE skeleton type is formed by preparing the reaction mixture and subjecting it to crystallization conditions Molecular sieve and contains 1-ethylpyridinium cation in its pores.

Benefits of technology

The molecular sieve with *MRE skeleton topology was successfully synthesized, achieving efficient preparation of catalyst components, with stable catalytic activity and good catalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118804893A_ABST
    Figure CN118804893A_ABST
Patent Text Reader

Abstract

A method of synthesizing a * MRE molecular sieve using an organic structure directing agent comprising a 1-ethylpyridinium cation is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to methods for preparing molecular sieves having a *MRE framework topology. Background Art

[0002] Molecular sieves are a commercially important class of materials that possess a unique crystal structure with a defined pore structure as evidenced by a unique X-ray diffraction (XRD) pattern and have a specific chemical composition.

[0003] Molecular sieves are classified by the International Zeolite Association Structure Commission according to the rules of the IUPAC Zeolite Nomenclature Commission. According to this classification, framework zeolites and other crystalline microporous crystalline materials of defined structure are assigned a unique three-letter code and are described, for example, in "Atlas of Zeolite Framework Types" (Elsevier, Sixth Revised Edition, 2007).

[0004] *MRE framework type molecular sieve is a disordered material with one-dimensional 10-ring channels. *MRE framework type molecular sieve shows attractive properties as a catalyst or catalyst component for dewaxing hydrocarbon feedstocks. *Examples of MRE framework type molecular sieves include COK-8, EU-2, EU-11, IZM-1, SSZ-91, ZBM-30 and ZSM-48.

[0005] Many organic compounds have been shown to be able to direct the synthesis of *MRE framework-type molecular sieves, including organic linear amines and polyamine compounds, diquaternary ammonium alkyl ammonium compounds, and diols.

[0006] According to the present disclosure, it has been discovered that an organic structure directing agent comprising a 1-ethylpyridinium cation can be used to synthesize a *MRE framework-type molecular sieve. Summary of the invention

[0007] In one aspect, a method for synthesizing a *MRE framework-type molecular sieve is provided, the method comprising: (1) preparing a reaction mixture, the reaction mixture comprising: (a) a silicon atom source; (b) an aluminum atom source; (c) an organic structure directing agent [Q], the organic structure directing agent [Q] comprising a 1-ethylpyridinium cation; (d) an alkali metal source [M]; (e) a hydroxide ion source; and (f) water; and (2) subjecting the reaction mixture to crystallization conditions sufficient to form crystals of the molecular sieve.

[0008] In another aspect, a *MRE framework-type molecular sieve in as-synthesized form is provided, the molecular sieve comprising 1-ethylpyridinium cations in its pores. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1The powder X-ray diffraction (XRD) pattern of the as-synthesized *MRE framework-type material according to Example 1 is shown.

[0010] Figure 2 A scanning electron microscope (SEM) image of the as-synthesized *MRE framework-type material according to Example 1 is shown. DETAILED DESCRIPTION

[0011] definition

[0012] The term "framework type" is used in the sense described in "Atlas of Zeolite Framework Types," by Ch. Baerlocher, LB McCusker, and DH Olson (Elsevier, 6th revised edition, 2007).

[0013] The terms "backbone type" and "backbone topology" are to be understood as synonyms.

[0014] As used herein, the term "as-synthesized" refers to the form of the molecular sieve after crystallization and before removal of the organic structure directing agent used in the synthesis of the molecular sieve.

[0015] Reaction mixture

[0016] Generally speaking, *MRE framework-type molecular sieves can be synthesized by the following steps: (1) preparing a reaction mixture comprising (a) a silicon atom source; (b) an aluminum atom source; (c) an organic structure directing agent [Q], wherein the organic structure directing agent [Q] comprises a 1-ethylpyridinium cation; (d) an alkali metal source [M]; (e) a hydroxide ion source; and (f) water; and (2) subjecting the reaction mixture to crystallization conditions sufficient to form crystals of the molecular sieve.

[0017] The reaction mixture may have a composition in terms of molar ratio within the range shown in Table 1.

[0018] Table 1

[0019]

[0020] wherein Q is an organic structure directing agent and M is an alkali metal.

[0021] Examples of silicon atom sources include colloidal suspensions of silica, precipitated silica, fumed silica, alkali metal silicates, tetraalkylorthosilicates, and mixtures thereof.

[0022] Examples of the aluminum atom source include hydrated aluminum oxide, aluminum hydroxide, alkali metal aluminates, aluminum alkoxides, and water-soluble aluminum salts (eg, aluminum nitrate), and mixtures thereof.

[0023] A combined source of silicon atoms and aluminum atoms, such as aluminosilicate zeolites (e.g., Y-type zeolites), may also be used. Aluminosilicate zeolites may be used as the sole or primary source of both silicon and aluminum. The term "primarily" means greater than 50 mol%, suitably greater than 75 mol%, and preferably greater than 90 mol%.

[0024] The alkali metal [M] can be selected from lithium, sodium, potassium, rubidium, cesium or mixtures thereof. In some aspects, the alkali metal is selected from sodium and / or potassium. The alkali metal is typically introduced into the reaction mixture together with a source of hydroxide ions.

[0025] The organic structure directing agent [Q] comprises a 1-ethylpyridinium cation represented by the following structure (1):

[0026]

[0027] Suitable sources of Q are hydroxides, chlorides, bromides and / or other salts of quaternary ammonium compounds.

[0028] The reaction mixture may additionally contain seeds from a previously synthesized crystalline material (such as ZSM-48), ideally in an amount of 0.01 to 10,000 ppm by weight (e.g., 100 to 5000 ppm by weight) of the reaction mixture. Adding seeds may be beneficial in reducing the time required to complete crystallization. In addition, adding seeds may increase the purity of the product by promoting nucleation and / or formation of the desired molecular sieve on any undesirable phase.

[0029] The reaction mixture components can be provided by multiple sources. In addition, two or more reaction mixture components can be provided by one source.

[0030] The reaction mixture can be prepared by any conceivable means, wherein mixing by shaking is preferred, preferably mixing by means of stirring.The reaction mixture can be prepared in batch, continuous or semi-continuous mode.

[0031] The reaction mixture may be in the form of a solution, a colloidal dispersion (colloidal sol), a gel or a paste, with gels being preferred.

[0032] Crystallization and post-synthesis processing

[0033] Crystallization of the molecular sieve from the reaction mixture can be carried out under static or stirred conditions in a suitable reactor vessel, such as a polypropylene jar or a Teflon-lined autoclave or a stainless steel autoclave, placed in a convection oven maintained at a temperature of 100° C. to 200° C. for a period of time sufficient for crystallization to occur (e.g., about 1 day to 21 days, or 1 day to 14 days, or 1 day to 7 days).

[0034] Once the desired molecular sieve crystals are formed, the solid product can be separated from the reaction mixture by standard mechanical separation techniques such as centrifugation or filtration. The recovered crystals are washed with water and then dried for a few seconds to a few minutes (e.g., 5 seconds to 10 minutes for rapid drying) or a few hours (e.g., 4 hours to 24 hours for oven drying at 75° C. to 150° C.) to obtain the molecular sieve crystals as they were after synthesis. The drying step can be carried out under vacuum or atmospheric pressure.

[0035] As a result of the crystallization process, the recovered as-synthesized crystalline molecular sieve product contains within its pore structure at least a portion of the organic structure directing agent (eg, 1-ethylpyridinium cation) used in the synthesis.

[0036] The organic structure directing agent can be removed by calcination, wherein the as-synthesized molecular sieve is heated under an oxidizing atmosphere (such as air or oxygen), a neutral atmosphere (such as nitrogen or other inert gases), or a reducing atmosphere (such as hydrogen). The atmosphere can be dry or contain water.

[0037] The temperature used for calcination depends on the composition of the material to be calcined and is generally 400° C. to 900° C. for a duration of about 1 to 8 hours. In some cases, calcination can be carried out at a temperature as high as 1200° C. In applications involving the methods described herein, calcination is generally carried out at a temperature of 400° C. to 700° C. for about 1 to 8 hours, preferably at a temperature of 400° C. to 650° C. for about 1 to 4 hours.

[0038] The molecular sieve synthesized by this method may contain one or more extra-framework alkali metals. Generally, it is desirable to remove alkali metal cations by ion exchange and replace alkali metal cations with hydrogen, ammonium or any desired metal ions. Typical ion exchange techniques involve contacting the synthetic molecular sieve with a solution containing a desired replacement cation or a salt of a cation. Although a variety of salts can be used, chlorides and other halides, nitrates, sulfates and carbonates are particularly preferred. Representative ion exchange techniques are well known in the art. Ion exchange occurs after synthesis and can be performed before or after the molecular sieve is calcined. After contact with the desired salt solution of the replacement cation, the molecular sieve is typically washed with water and dried at a temperature of 65°C to 200°C (e.g., 80°C to 150°C). After washing, the molecular sieve can be calcined at a temperature in the range of 400°C to 900°C in an inert gas and / or air for a period of 1 to 48 hours or longer to produce a catalytically active and stable product.

[0039] Characterization of Molecular Sieve

[0040] The *MRE framework-type molecular sieve synthesized by the method described herein may have SiO 2 / Al 2 O 3 The molar ratio (SAR) is at least 60 (e.g., 60 to 150, or 60 to 140, or 60 to 130, or 65 to 150, or 65 to 140, or 65 to 130, or 70 to 150, or 70 to 140, or 70 to 130).

[0041] The *MRE framework type molecular sieve may contain less than 5 wt % (e.g., less than 4 wt %, or less than 3 wt %, or less than 2 wt %, or less than 1 wt %) of non-*MRE materials. Examples of non-*MRE materials may include amorphous materials, undissolved FAU, hydrochloric acid sodium silicate, and ZSM-50. In some aspects, the *MRE framework type molecular sieve may be free of non-*MRE materials. The so-called "free of non-*MRE materials" means that the amount of non-*MRE solid materials (if any) cannot be detected by X-ray diffraction.

[0042] The X-ray powder diffraction pattern is determined by standard techniques. The radiation is K-alpha / doublet of copper. Minor variations in the diffraction pattern values ​​in the table or figure may also result from variations in the organic compounds used in the preparation and variations in the silica to alumina molar ratio between samples. Despite these minor perturbations, the basic crystal structure of the as-synthesized and calcined material remains essentially unchanged.

[0043] Example

[0044] The following illustrative examples are intended to be non-limiting.

[0045] Example 1

[0046] 0.24 g of 50% NaOH solution, 7.86 g of deionized water, 0.56 g of 1-ethylpyridinium bromide (TCI America) and 0.03 g of Reheis F-2000 hydrated alumina (53% Al 2 O 3 47% H 2 O) were mixed together in a Teflon liner. Then, 4.00 g of LUDOX® HS-30 colloidal silica was added to the liner. The resulting gel was stirred until uniform. The liner was then capped and placed in a Parr Steel autoclave reactor. The autoclave was then placed in an oven heated at 160°C for 4 days. The solid product was recovered from the cooled reactor by centrifugation, washed with deionized water and dried at 95°C.

[0047] Powder XRD analysis of the dried product ( Figure 1) indicates that the product has an *MRE backbone topology. Figure 2 Depicted is a SEM image of the product showing a uniform crystal field.

[0048] According to ICP elemental analysis, the product has SiO 2 / Al 2 O 3 The molar ratio is 126.06.

[0049] Example 2

[0050] 0.20 g of 50% NaOH solution, 8.90 g of deionized water, 0.63 g of 1-ethylpyridinium bromide and 0.02 g of sodium aluminate (Thermo Scientific) were mixed together in a Teflon liner. Then, 1.00 g of CAB-O-SIL® M-5 fumed silica was added to the liner. The resulting gel was stirred until uniform. The liner was then covered and placed in a Parr Steel autoclave reactor. The autoclave was then placed in an oven heated at 160°C for 4 days. The solid product was recovered from the cooled reactor by centrifugation, washed with deionized water and dried at 95°C.

[0051] Powder XRD and SEM analysis of the dried product showed that the product had an *MRE framework topology.

[0052] According to ICP elemental analysis, the product has SiO 2 / Al 2 O 3 The molar ratio is 118.43.

[0053] Example 3

[0054] 0.26 g of 50% NaOH solution, 11.47 g of deionized water and 1.00 g of CBV780 Y-type zeolite (SAR=80) powder were mixed together in a Teflon liner. Then, 0.91 g of 1-ethylpyridinium bromide was added to the liner. The resulting gel was stirred until uniform. The liner was then covered and placed in a Parr Steel autoclave reactor. The autoclave was then placed in an oven heated at 150°C for 4 days. The solid product was recovered from the cooled reactor by centrifugation, washed with deionized water and dried at 95°C.

[0055] Powder XRD and SEM analysis of the dried product showed that the product had an *MRE framework topology.

[0056] According to ICP elemental analysis, the product has SiO 2 / Al2 O 3 The molar ratio is 83.70.

[0057] Example 4

[0058] 0.39 g of 50% NaOH solution, 11.41 g of deionized water, 1.00 g of CBV760 Y-type zeolite (SAR=60) powder were mixed together in a Teflon liner. Then, 0.91 g of 1-ethylpyridinium bromide was added to the liner. The resulting gel was stirred until uniform. The liner was then covered and placed in a Parr Steel autoclave reactor. The autoclave was then placed in an oven heated at 160°C for 6 days. The solid product was recovered from the cooled reactor by centrifugation, washed with deionized water and dried at 95°C.

[0059] Powder XRD and SEM analysis of the dried product showed that the product had an *MRE framework topology.

[0060] According to ICP elemental analysis, the product has SiO 2 / Al 2 O 3 The molar ratio is 71.72.

[0061] Example 5

[0062] Calcination

[0063] The as-synthesized product of Example 1 was calcined in a muffle furnace under air flow, heated to 540°C at a rate of 1°C / min, and maintained at 540°C for 5 hours, cooled, and then analyzed by powder XRD. Powder XRD analysis of the dried product showed that the product was still stable after calcination to remove the organic structure directing agent.

[0064] Example 6

[0065] Ammonium ion exchange

[0066] The calcined material of Example 5 was treated with 10 mL (per gram of molecular sieve) of 1 N ammonium nitrate solution at 90°C for 2 hours. The solution was cooled, decanted and the same process was repeated. After drying, the product (NH 4 Micropore volume analysis was performed using N 2 As adsorbate and by BET method, the molecular sieve showed a micropore volume of 0.07 cm 3 / g.

[0067] Example 7

[0068] Palladium ion exchange

[0069] The ammonium exchanged samples of Examples 1 and 2 were each subjected to palladium ion exchange using tetraammine palladium (II) nitrate (0.5 wt % Pd). After ion exchange, the samples were dried at 95°C and then calcined in air at 482°C for 3 hours to convert the tetraammine palladium (II) nitrate into palladium oxide.

[0070] Example 8

[0071] Hydrogenation conversion of n-hexadecane (n-C16)

[0072] 0.5 g of each palladium exchanged sample of Example 7 was added to the center of a 23 inch long x 0.25 inch outer diameter stainless steel reaction tube, and corundum was added upstream of the catalyst to preheat the feed (total pressure was 1200 psig; the downward flowing hydrogen rate was 160 mL / min (measured at 1 atmosphere and 25°C); the downward flowing liquid feed rate was 1 mL / h). All materials were first reduced in flowing hydrogen at about 315°C for 1 hour. The products were analyzed once every thirty minutes by online capillary gas chromatography (GC). The raw data from the GC was collected by an automatic data collection / processing system, and the hydrocarbon conversion was calculated from the raw data.

[0073] The catalyst was initially tested at about 260°C to determine the temperature range for the next set of measurements. The total temperature range will provide a wide range of n-hexadecane conversions, with maximum conversions slightly less than and greater than 96%. At least five online GC injections were collected for each temperature. Conversion is defined as the amount of n-hexadecane that reacts to form other products (including iso-nC16 isomers). Yields are expressed as wt% of products other than n-C16, and iso-C16 is included in the yield product. The results are shown in Table 2.

[0074] Table 2

[0075] Results at 96% n-hexadecane conversion

[0076]

[0077] Good catalytic performance depends on the synergy between isomerization selectivity and temperature at 96% conversion, while minimizing undesirable catalytic cracking. These catalysts exhibit desirable isomerization selectivity at 96% conversion. The catalysts also exhibit very desirable temperature at 96% conversion, while still maintaining very good isomerization selectivity. In addition, undesirable catalytic cracking and the resulting high gas production are very low, which is reflected in acceptable levels of C4− cracking.

Claims

1. A method for synthesizing a *MRE framework type molecular sieve, the method comprising: (1) preparing a reaction mixture, the reaction mixture comprising: (a) Silicon atom source; (b) Aluminum atom source; (c) an organic structure directing agent [Q], the organic structure directing agent [Q] comprising a 1-ethylpyridinium cation; (d) alkali metal source [M]; (e) a source of hydroxide ions; and (f) water; and (2) subjecting the reaction mixture to crystallization conditions sufficient to form crystals of the molecular sieve.

2. The method of claim 1, wherein the reaction mixture has the following composition in molar ratio:

3. The method of claim 1, wherein the reaction mixture has the following composition in molar ratio:

4. The method of claim 1, wherein the silicon atom source is selected from a colloidal suspension of silica, precipitated silica, fumed silica, an alkali metal silicate, a tetraalkyl orthosilicate, or a mixture thereof.

5. The method of claim 1, wherein the aluminum atom source is selected from hydrated aluminum oxide, aluminum hydroxide, alkali metal aluminates, aluminum alkoxides and water-soluble aluminum salts or mixtures thereof.

6. The method of claim 1, wherein both the silicon atom source and the aluminum atom source are Y-type zeolites.

7. The method of claim 1, wherein the crystallization conditions include a temperature of 100°C to 200°C, and a crystallization time of about 1 day to 21 days.

8. An *MRE framework-type molecular sieve, which is in its as-synthesized form and contains 1-ethylpyridinium cations in its pores.

9. The molecular sieve of claim 8, having a SiO2 / Al2O3 molar ratio of at least 60.

10. The molecular sieve of claim 8, having a SiO2 / Al2O3 molar ratio in the range of 60 to 150.