Modified ethylene-vinyl alcohol copolymer composition, particles, multilayer structure, method for producing modified ethylene-vinyl alcohol copolymer composition, and method for producing multilayer structure

By adding a trace amount of titanium compound to the modified EVOH resin to form a titanium ion chelate, the problem of thermal degradation of the modified EVOH resin during heating and elongation is solved, the mechanical strength and barrier properties of the molded article are improved, and it is suitable for complex shapes. Manufacture of containers.

CN118804948APending Publication Date: 2024-10-18MITSUBISHI CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380025062.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-30
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing modified EVOH resins are prone to thermal deterioration during the heating and stretching process, resulting in insufficient mechanical strength and barrier properties of the molded products, making it difficult to meet the needs of complex-shaped containers.

Method used

A specific trace amount of titanium compound is added to the modified EVOH resin with primary hydroxyl structural units in the side chain, and a chelate is formed through the reaction of titanium ions and the main chain of the modified EVOH resin to inhibit thermal degradation.

Benefits of technology

It effectively suppresses the thermal degradation of modified EVOH resin during heating, improves the mechanical strength and barrier properties of the molded product, and is suitable for the manufacture of complex-shaped containers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005023198640000021
    Figure BDA0005023198640000021
  • Figure BDA0005023198640000041
    Figure BDA0005023198640000041
  • Figure BDA0005023198640000071
    Figure BDA0005023198640000071
Patent Text Reader

Abstract

Provided is a modified ethylene-vinyl alcohol copolymer composition in which thermal deterioration during heating such as melt kneading and melt molding is suppressed. A modified ethylene-vinyl alcohol copolymer composition containing a modified ethylene-vinyl alcohol copolymer having a primary hydroxyl group structural unit in a side chain, and a titanium compound, the content of the titanium compound in terms of metal is 0.001 ppm or more and less than 5 ppm relative to the unit mass of the modified ethylene-vinyl alcohol copolymer composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a modified ethylene-vinyl alcohol copolymer composition, particles, a multilayer structure, a method for producing the modified ethylene-vinyl alcohol copolymer composition, and a method for producing the multilayer structure. Background Art

[0002] Ethylene-vinyl alcohol copolymers (hereinafter sometimes referred to as "EVOH resins") have excellent transparency, gas barrier properties such as oxygen, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and are formed into films, sheets, bottles, etc., and are widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0003] In addition, EVOH resin is often subjected to heat stretching treatment for the purpose of deforming it into practical containers and improving its mechanical strength. In recent years, when multilayer sheets containing EVOH resin are formed into containers, deep-bottomed containers have begun to be manufactured due to the diversity and design of container shapes. In the case of forming such deep-bottomed containers, EVOH resin with excellent heat stretchability and good appearance, barrier properties and strength of the formed container is also required.

[0004] To address the above problems, for example, Patent Document 1 discloses a modified EVOH resin having a specific structural unit as an EVOH resin having excellent heat stretchability.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2004-359965 Summary of the invention

[0008] Problems to be solved by the invention

[0009] However, with regard to the modified EVOH resin disclosed in the above-mentioned Patent Document 1, the improvement effect related to long-term operation formability, such as suppression of deterioration products during heating during melt kneading, melt molding, etc., is not sufficient, and a modified EVOH resin composition that is not easily thermally degraded during heating and can produce high-quality molded products is sought.

[0010] Therefore, under such background, the present invention provides a modified EVOH resin composition which is suppressed from thermal degradation during heating such as melt kneading and melt molding.

[0011] Means for solving problems

[0012] However, in view of this situation, the present inventors have found that a modified EVOH resin composition with suppressed thermal degradation can be obtained by adding a specific trace amount of a titanium compound to a modified EVOH resin having a primary hydroxyl structural unit in a side chain.

[0013] That is, the present invention has the following aspects.

[0014] [1] A modified EVOH resin composition comprising a modified EVOH resin having a primary hydroxyl structural unit in a side chain and a titanium compound,

[0015] The metal-equivalent content of the titanium compound is 0.001 ppm or more and less than 5 ppm based on the unit mass of the modified EVOH resin composition.

[0016] [2] The modified EVOH resin composition according to [1], wherein the content of the ethylene structural unit in the modified EVOH resin is 20 to 60 mol%.

[0017] [3] The modified EVOH resin composition according to [1] or [2], wherein the modification rate of the primary hydroxyl structural unit in the side chain of the modified EVOH resin is 0.1 to 30 mol%.

[0018] [4] The modified EVOH resin composition according to any one of [1] to [3], wherein the primary hydroxyl structural unit in the side chain of the modified EVOH resin is represented by the following general formula (1).

[0019]

[0020] In the formula, R 1 ~R 3 Each independently represents a hydrogen atom or an organic group, and X represents a single bond or a bond chain.

[0021] [5] A pellet comprising the modified EVOH resin composition according to any one of [1] to [4].

[0022] [6] A multilayer structure comprising at least one layer comprising the modified EVOH resin composition according to any one of [1] to [4].

[0023] [7] A method for producing a modified EVOH resin composition, which is a method for producing the modified EVOH resin composition described in any one of [1] to [4],

[0024] The method comprises the step of melt-mixing a composition raw material containing the modified EVOH resin and a titanium compound.

[0025] [8]A method for manufacturing a multilayer structure, which is a method for manufacturing the multilayer structure described in [6],

[0026] comprises a step of melt-molding a layer composed of the above-mentioned modified EVOH resin composition.

[0027] Advantages of the Invention

[0028] The modified EVOH resin composition of the present invention can suppress thermal degradation during heating such as melt-kneading and melt-molding. Detailed Description of the Invention

[0029] Hereinafter, the present invention will be described in further detail based on examples of embodiments of the present invention, but the present invention is not limited to these embodiments.

[0030] It should be noted that in the present invention, when expressed as "X to Y" (X and Y are arbitrary numbers), unless otherwise specified, it means "X or more and Y or less", and also includes the meaning of "preferably greater than X" or "preferably less than Y".

[0031] In addition, when expressed as "X or more" (X is an arbitrary number) or "Y or less" (Y is an arbitrary number), it also includes the meaning of "preferably greater than X" or "preferably less than Y".

[0032] Furthermore, in the present invention, the so-called "x and / or y (x and y are arbitrary components or ingredients)" means only x, only y, and the three combinations of x and y.

[0033] <EVOH Resin Composition>

[0034] The modified EVOH resin composition of one embodiment of the present invention (hereinafter referred to as "the present modified EVOH resin composition") uses a modified EVOH resin having a primary hydroxyl group structural unit in the side chain as the main component and contains a specific trace amount of a titanium compound.

[0035] That is, in the present modified EVOH resin composition, the base resin is a modified EVOH resin, and the content of the modified EVOH resin in the present modified EVOH resin composition is usually 70% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0036] Hereinafter, each component will be described.

[0037] [Modified EVOH Resin]

[0038] The above-mentioned modified EVOH resin composition is an EVOH resin composition having a primary hydroxyl group in the side chain. Specifically, it is preferably a modified EVOH-based resin having a structural unit represented by the following general formula (1).

[0039] [Chemistry 1]

[0040]

[0041] In the formula, R 1 ~R 3 Each independently represents a hydrogen atom or an organic group, and X represents a single bond or a bond chain.

[0042] In the above general formula (1), R 1 ~R 3 There are no particular limitations as long as it is a hydrogen atom or an organic group. Examples of the organic group include hydrocarbon groups such as alkyl, alkenyl, alkynyl, phenyl, and naphthyl (these hydrocarbon groups may have a hydroxyl group, fluorine, chlorine, bromine, or the like as a substituent).

[0043] The bonding chain (X) bonding the polymer main chain to the primary hydroxyl structure is not particularly limited, and examples thereof include hydrocarbons such as alkylene, alkenylene, alkynylene, phenylene, and naphthylene (these hydrocarbons may also have hydroxyl, fluorine, chlorine, and bromine as substituents), and hydrocarbons such as oxyalkylene, oxyalkenylene, oxyalkynylene, oxyphenylene, and oxynaphthylene bonded to the polymer main chain via an ether bond (these hydrocarbons may also have hydroxyl, fluorine, chlorine, and bromine as substituents), and -CO-, -CO(CH2) m CO-, -CO(CH2) m COR 4 -、-NR 5 -、-CONR 5 - etc. 4 , R 5 (where m represents a natural number) is independently an arbitrary substituent, preferably a hydrogen atom or an alkyl group.

[0044] In order to obtain the above-mentioned modified EVOH resin, for example:

[0045] (I) a method in which a monomer having a primary hydroxyl structural unit in a side chain or a monomer in which the primary hydroxyl structural unit in the side chain is protected by ester or the like is copolymerized with ethylene and a vinyl ester monomer, and then deprotected by saponification or the like;

[0046] (II) A method of obtaining an EVOH resin by saponifying a copolymer of ethylene and a vinyl ester monomer, and then post-modifying the EVOH resin to produce a primary hydroxyl structural unit in the side chain. Among them, the method (I) is preferred from the viewpoint of productivity.

[0047] Hereinafter, a method for producing a modified EVOH-based resin will be described.

[0048] First, in the case of the method (I) described above, ethylene, a vinyl ester monomer, and a monomer having a primary hydroxyl structural unit in a side chain or a monomer in which the hydroxyl structural unit is protected by an ester or the like are copolymerized.

[0049] Examples of the vinyl ester monomers include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl versatate, vinyl trifluoroacetate, etc. Among these, vinyl acetate is preferred from the viewpoint of economic efficiency.

[0050] Examples of monomers having a primary hydroxyl structural unit in the side chain of the method (I) include monomers containing monohydroxyalkyl groups such as allyl alcohol, 3-butene-1-ol, 4-pentene-1-ol, 5-hexene-1-ol, 6-heptene-1-ol, and methylallyl alcohol; and monomers containing dihydroxyalkyl groups such as 2-methylene-1,3-propanediol, 3,4-diol-1-butene, 4,5-diol-1-pentene, 4,5-diol-3-methyl-1-pentene, 5,6-diol-1-hexene, and glycerol monoallyl ether. These monomers may be used alone or in combination of two or more.

[0051] In addition, as the monomers in which the primary hydroxyl structural unit of the side chain is protected by esters or the like in the method (I) above (hereinafter, sometimes referred to as "monomers in which the hydroxyl structural unit is protected by esters or the like"), examples thereof include acetates of the monomers having primary hydroxyl structural units in the side chains mentioned above. Specifically, examples thereof include monomers containing monoacetoxyalkyl groups such as allyl acetate, 3-butenyl acetate, 4-pentenyl acetate, 5-hexenyl acetate, 6-heptenyl acetate, and methyl allyl acetate; monomers containing diacetoxyalkyl groups such as 2-methylene-1,3-propanediol diacetate, 3,4-diacetoxy-1-butene, 4,5-diacetoxy-1-pentene, 4,5-diacetoxy-3-methyl-1-pentene, 5,6-diacetoxy-1-hexene, and 3-allyloxy-1,2-propanediol diacetate. These monomers may be used alone or in combination of two or more.

[0052] In the above method (I), a monomer having a primary hydroxyl structural unit in a side chain and a monomer in which the hydroxyl structural unit is protected by an ester or the like may be used in combination and copolymerized with ethylene or a vinyl ester monomer.

[0053] Among them, from the viewpoint of productivity, monomers in which the hydroxy structural unit is protected by an ester or the like are preferred, monomers containing a diacetoxyalkyl group are more preferred, 3,4-diacetoxy-1-butene and 2-methylene-1,3-propanediol diacetate are more preferred, and 3,4-diacetoxy-1-butene is particularly preferred.

[0054] Furthermore, a copolymerizable ethylenically unsaturated monomer may be copolymerized within a range not impairing the effects of the present invention.

[0055] Examples of the ethylenically unsaturated monomer include olefins such as propylene, 1-butene, and isobutylene; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, phthalic acid (anhydride), maleic acid (anhydride), and itaconic acid (anhydride), or salts thereof, or mono- or di-alkyl esters having an alkyl group with 1 to 18 carbon atoms; acrylamide, N-alkylmethacrylamide having an alkyl group with 1 to 18 carbon atoms, N,N-dimethylacrylamide, 2-acrylamidepropanesulfonic acid or salts thereof; acrylamidepropyldimethylamine or its acid salts or quaternary salts thereof; methacrylamide, alkyl carbon atoms; Methacrylamides such as N-alkylmethacrylamide with carbon number of 1 to 18, N,N-dimethylmethacrylamide, 2-methacrylamidepropanesulfonic acid or its salt; N-vinylamides such as N-vinylpyrrolidone, N-vinylformamide, N-vinylacetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl ethers such as alkylvinyl ether with carbon number of 1 to 18, hydroxyalkylvinyl ether, alkoxyalkylvinyl ether; vinyl halides such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, vinyl bromide; vinyl silanes, etc. These may be used alone or in combination of two or more.

[0056] For the copolymerization reaction, for example, a known method such as bulk polymerization, solution polymerization, suspension polymerization, dispersion polymerization or emulsion polymerization can be used. Among them, solution polymerization can be preferably used because the copolymerization is easily controlled.

[0057] As the solvent used when implementing the copolymerization by solution polymerization, for example, ketones such as lower alcohols with 1 to 5 carbon numbers such as methanol, ethanol, propanol, 2-propanol, butanol, acetone, and 2-butanone can be cited. They can be used alone or in combination of two or more. Among them, methanol can be suitably used from the ease of control of the polymerization reaction. In addition, in the case of synthesizing a copolymer with a low degree of polymerization, 2-propanol can be suitably used.

[0058] The amount of the solvent used can be appropriately selected in consideration of the polymerization degree of the target modified EVOH resin and the chain transfer constant of the solvent. When the solvent is methanol or 2-propanol, preferably S (solvent) / M (monomer) = 0.01 to 10 (weight ratio), more preferably 0.05 to 7 (weight ratio).

[0059] As a method for charging the copolymerization components in solution polymerization, any method may be adopted, such as initial all-in-one charging, batch charging, or continuous charging such as the Hanna method taking the reactivity ratio of the monomers into consideration.

[0060] A polymerization initiator may be used in the above copolymerization. Examples of the polymerization initiator include azo initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile); and peroxide initiators such as acetyl peroxide, benzoyl peroxide, lauroyl peroxide, tert-butyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, diisopropyl peroxydicarbonate, and di-2-ethylhexyl peroxydicarbonate.

[0061] The amount of the polymerization catalyst used varies depending on the type of polymerization catalyst and cannot be generalized, but can be arbitrarily selected according to the polymerization rate. For example, when 2,2'-azobisisobutyronitrile or tert-butyl peroxyneodecanoate is used, the amount is usually 10 to 2000 ppm, preferably 50 to 1000 ppm, relative to the vinyl ester monomer.

[0062] The polymerization temperature of the copolymerization is preferably selected from the range of 40°C to the boiling point depending on the solvent used and the ethylene pressure.

[0063] In addition, during the copolymerization, the copolymerization may be carried out in the presence of a chain transfer agent within the range that does not hinder the effect of the present invention. As the chain transfer agent, for example, aldehydes such as acetaldehyde, propionaldehyde, crotonaldehyde, and thiols such as 2-hydroxyethanethiol can be cited. They can be used alone or in combination of two or more. Among them, aldehydes can be used appropriately. The amount of chain transfer agent added during the copolymerization is determined according to the chain transfer constant of the chain transfer agent and the degree of polymerization of the target modified EVOH-based resin, but in general, it is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the vinyl ester monomer.

[0064] By saponifying the ethylene-vinyl ester copolymer thus obtained, a modified EVOH resin can be obtained.

[0065] The saponification method can be carried out by a known method, for example, by dissolving the ethylene-vinyl ester copolymer obtained above in alcohol or aqueous alcohol and using a saponification catalyst.

[0066] Examples of the alcohol include lower alcohols having 1 to 5 carbon atoms, such as methanol, ethanol, and propanol. These alcohols may be used alone or in combination of two or more. Among them, methanol is preferred.

[0067] The concentration of the ethylene-vinyl ester copolymer in the alcohol is appropriately selected depending on the viscosity and is usually 5 to 60% by mass.

[0068] Examples of the saponification catalyst include base catalysts such as hydroxides and alcoholates of alkali metals such as sodium hydroxide, potassium hydroxide, sodium methoxide, sodium ethoxide, potassium methoxide, and potassium ethoxide; and acid catalysts such as sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, zeolite, and cation exchange resins.

[0069] The temperature for saponification is not limited, but is preferably in the range of 20 to 140°C. As saponification proceeds, particulate matter is generated, indicating that the reaction has proceeded. At this time, when a gel-like product gradually precipitates, the product can be crushed. The generated particulate matter is washed and dried to obtain a modified EVOH-based resin.

[0070] In order to increase the degree of saponification, the generated particulate matter may be washed once and then dispersed again in alcohol or the like, and an alkali catalyst may be added to further react.

[0071] By the saponification, the vinyl ester units in the ethylene-vinyl ester copolymer are converted into vinyl alcohol units.

[0072] Furthermore, when a monomer in which a hydroxyl structural unit is protected by an ester or the like is copolymerized, the ester or the like of the protected monomer is also deprotected by saponification to convert it into a side chain primary hydroxyl structure.

[0073] In the above method (I), when 3,4-diacetoxy-1-butene is used as a copolymerization component, the modified EVOH-based resin obtained by deprotection by saponification or the like has a primary hydroxyl group represented by the following general formula (2) in the side chain.

[0074] [Chemistry 2]

[0075]

[0076] In the method (I) above, when 2-methylene-1,3-propanediol diacetate is used as a copolymerization component, the obtained modified EVOH-based resin has a primary hydroxyl group represented by the following general formula (3) in the side chain.

[0077] [Chemistry 3]

[0078]

[0079] When the modified EVOH resin is produced by the method (II) above, for example, ethylene and the vinyl ester monomers exemplified in the method (I) above, and the copolymerizable ethylenically unsaturated monomers exemplified in the method (I) above as needed, are copolymerized according to the method (I) above to produce the EVOH resin, and the obtained EVOH resin is reacted with a compound containing a monovalent epoxy group. The above reaction method is not particularly limited, and suitable methods include, for example, a method of reacting the resin in a solution, a method of reacting the resin in an extruder, and the like. In addition, when the method of reacting the resin in an extruder is adopted, it is also preferred to use a catalyst containing ions of metals belonging to Groups 3 to 12 of the periodic table.

[0080] Examples of the monovalent epoxy group-containing compound include propylene oxide, butylene oxide, glycidol, etc. These may be used alone or in combination of two or more. Among them, propylene oxide is preferred.

[0081] When propylene oxide is used as the monovalent epoxy group-containing compound, for example, the obtained modified EVOH-based resin has a primary hydroxyl structural unit represented by the following general formula (4) in the side chain.

[0082] [Chemistry 4]

[0083]

[0084] By the method (I) or (II), a modified EVOH resin having a structural unit of the following general formula (1) can be obtained. In addition, the modified EVOH resin may have a primary hydroxyl structural unit in the side chain, or may have other hydroxyl structures (secondary hydroxyl, tertiary hydroxyl) in the side chain. In addition, the EVOH resin may not be completely deprotected and a small amount of ester may remain.

[0085] [Chemistry 5]

[0086]

[0087] In the formula, R 1 ~R 3 Each independently represents a hydrogen atom or an organic group, and X represents a single bond or a bond chain.

[0088] In the above general formula (1), R 1 ~R 3 There are no particular limitations as long as it is a hydrogen atom or an organic group. Examples of the organic group include hydrocarbon groups such as alkyl, alkenyl, alkynyl, phenyl, and naphthyl (these hydrocarbon groups may also have a hydroxyl group, fluorine, chlorine, or bromine as a substituent).

[0089] The bonding chain (X) bonding the polymer main chain to the primary hydroxyl structure is not particularly limited, and examples thereof include hydrocarbons such as alkylene, alkenylene, alkynylene, phenylene, and naphthylene (these hydrocarbons may also have hydroxyl, fluorine, chlorine, and bromine as substituents), oxyalkylene, oxyalkenylene, oxyalkynylene, oxyphenylene, and oxynaphthylene bonded to the polymer main chain via an ether bond (these hydrocarbons may also have hydroxyl, fluorine, chlorine, and bromine as substituents), and -CO-, -CO(CH2)-, and -CO(CH3)-. m CO-, -CO(CH2) m COR 4 -、-NR 5 -、-CONR 5 - etc. 4 , R 5 (where m represents a natural number) is independently an arbitrary substituent, preferably a hydrogen atom or an alkyl group.

[0090] The content of the ethylene structural unit in the modified EVOH resin is usually 20 to 60 mol%, preferably 25 to 50 mol%, and particularly preferably 25 to 35 mol%. The content of the ethylene structural unit can be controlled by the ethylene pressure when the vinyl ester monomer and ethylene are copolymerized. When the content is too low, the gas barrier properties and melt moldability under high humidity tend to decrease. On the contrary, when the content is too high, the gas barrier properties tend to decrease.

[0091] In addition, the content of the ethylene structural unit can be measured based on ISO14663.

[0092] The modification rate of the primary hydroxyl structural unit in the side chain of the modified EVOH-based resin is preferably 0.1 to 30 mol %, more preferably 0.5 to 10 mol %, particularly preferably 1 to 5 mol %.

[0093] If the modification rate of the primary hydroxyl structural unit is too low, the hydrophilicity of the modified EVOH-based resin is insufficient and the biodegradability tends to be low. In addition, if the modification rate of the primary hydroxyl structural unit is too high, the production cost increases and tends to be economically disadvantageous.

[0094] In the case of the method (I) above, the modification rate of the primary hydroxyl structural unit can be controlled by the amount of the monomer having the primary hydroxyl structural unit in the side chain or the monomer protected by ester etc. used as the comonomer. In addition, in the case of the method (II) above, it can be controlled by the amount of the monovalent epoxy group-containing compound used for modification.

[0095] In addition, the melt flow rate (MFR) of the modified EVOH resin [210°C, load 2160g] is usually 0.1 to 100 g / 10 minutes, preferably 1 to 50 g / 10 minutes, and particularly preferably 3 to 35 g / 10 minutes. When the MFR is too large, thickness control during melt molding tends to become difficult, and when it is too small, a high load tends to be applied to the molding machine during melt molding.

[0096] This MFR is an index of the degree of polymerization of the modified EVOH-based resin, and can be adjusted by the amount of the polymerization catalyst and the amount of the solvent when copolymerizing the copolymerization components.

[0097] The saponification degree of the modified EVOH-based resin is usually 90 mol% or more, preferably 95 mol% or more, and particularly preferably 99 mol% or more. If the saponification degree is too low, the gas barrier properties tend to decrease.

[0098] [Titanium compounds]

[0099] Examples of the titanium compound include inorganic titanium compounds and organic titanium compounds. The titanium compound may be used alone or in combination of two or more. Among them, inorganic titanium compounds are preferred.

[0100] Examples of the inorganic titanium compound include titanium oxide, titanium hydroxide, titanium chloride, and inorganic titanium salts.

[0101] Examples of the titanium oxide include titanium (II) oxide, titanium (III) oxide, titanium (IV) oxide, and titanium oxyoxide.

[0102] Examples of the titanium hydroxide include titanium (III) hydroxide and titanium (IV) hydroxide.

[0103] Examples of the titanium chloride include titanium (III) chloride and titanium (IV) chloride.

[0104] Examples of the inorganic salt of titanium include titanium phosphate and titanium sulfate.

[0105] Among them, titanium oxide is preferred, titanium (IV) oxide is more preferred, and rutile titanium (IV) oxide is particularly preferred.

[0106] Examples of the organic titanium compound include titanium acetate, titanium butyrate, titanium stearate and other titanium carboxylates.

[0107] Furthermore, the titanium compound may be present in the modified EVOH resin composition in the form of a titanium compound or in the form of an ionized state or in the form of a complex interacting with the modified EVOH resin or other ligands.

[0108] The average particle size of the titanium compound is usually 0.001 to 100 μm, preferably 0.01 to 50 μm, and more preferably 0.015 to 20 μm. When the average particle size of the titanium compound is within the above range, the coloration suppression effect tends to be excellent.

[0109] The metal conversion content of the above-mentioned titanium compound is 0.001ppm or more and less than 5ppm relative to the unit mass of the modified EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By making the content of the titanium compound within the above range, thermal degradation during melt molding can be suppressed. In addition, if the content of the titanium compound is too little, it becomes easy to thermally degrade, and if the content is too much, it is easy to cause thermal decomposition of the EVOH resin and become easy to color.

[0110] The metal conversion content of the above-mentioned titanium compound can be quantified by weighing the EVOH resin composition into a platinum crucible, ashing it with a burner and an electric furnace in sequence, heating and decomposing the ashed material with nitric acid and hydrofluoric acid, and using an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800) to treat the mixed acid with dilute nitric acid and dilute hydrofluoric acid and then fix the volume to obtain the titanium in the fixed volume solution using ICP mass spectrometry.

[0111] Generally, modified EVOH resin deteriorates due to heat. This is believed to be because the heat-induced degradation of the modified EVOH resin generates free radicals, which dehydrate the hydroxyl groups of the modified EVOH resin, thereby generating double bonds in the main chain of the modified EVOH resin. This site becomes the starting point of the reaction, further promoting dehydration, so that a conjugated polyene structure is formed in the main chain of the modified EVOH resin.

[0112] In contrast, the modified EVOH resin composition of the present invention can suppress the degradation of the modified EVOH resin due to heat by containing a specific trace amount of a titanium compound.

[0113] Generally, when a titanium compound is contained in a modified EVOH resin composition, it is believed that the modified EVOH resin composition will be colored by titanium ions, so it is common knowledge for those skilled in the art to avoid the use of titanium compounds. However, the present invention has found that when a specific trace amount of a titanium compound is used in violation of such common knowledge, a modified EVOH resin composition in which thermal deterioration is suppressed can be obtained.

[0114] That is, it is presumed that titanium is stable as a tetravalent ion and coordinates to the double bonds of the main chain of the modified EVOH resin described above even in a trace amount to stabilize by forming a chelate or the like, thereby suppressing the formation of a polyene structure.

[0115] On the other hand, if the content of the titanium compound is too large, it is considered that thermal decomposition of the modified EVOH resin by the titanium compound may occur.

[0116] [Other thermoplastic resins]

[0117] The modified EVOH resin composition may contain a thermoplastic resin other than the modified EVOH resin within a range that does not hinder the effects of the present invention (e.g., usually 30% by mass or less, preferably 20% by mass or less, and particularly preferably 10% by mass or less of the modified EVOH resin composition).

[0118] As other thermoplastic resins, known thermoplastic resins can be used, for example, EVOH resin, polyester resin, polystyrene resin, polyvinyl chloride resin, polycarbonate resin, ionomer, polyvinylidene chloride, polyester elastomer, polyurethane elastomer, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0119] [Other compounding ingredients]

[0120] In addition, the modified EVOH resin composition may contain a compounding agent generally used in EVOH resin within the range that does not hinder the effect of the present invention. As the above-mentioned compounding agent, for example, an inorganic complex salt (such as hydrotalcite), a plasticizer (such as aliphatic polyols such as ethylene glycol, glycerol, hexylene glycol, etc.), an oxygen absorber [such as inorganic oxygen absorbers such as aluminum powder and potassium sulfite; ascorbic acid and its fatty acid esters, metal salts, etc., gallic acid, polyphenols such as phenolic resin containing hydroxyl groups, terpene compounds, a mixture of a resin containing tertiary hydrogen and a transition metal (such as a combination of polypropylene and cobalt), a mixture of a resin containing a carbon-carbon unsaturated bond and a transition metal (such as Combination of polybutadiene and cobalt), photo-oxidative degradable resins (e.g., polyketones), anthraquinone polymers (e.g., polyvinyl anthraquinone), etc., and the like ...

[0121] [Method for producing modified EVOH resin composition]

[0122] The modified EVOH resin composition can be produced, for example, by mixing the modified EVOH resin and the titanium compound using a known method, such as a dry blending method, a melt blending method, a solution blending method, an impregnation method, etc. Among these, it is preferably produced by a process of melt blending the composition raw materials containing the modified EVOH resin and the titanium compound. In addition, these production methods can also be arbitrarily combined.

[0123] Examples of the dry blending method include (i) a method of dry blending a pelletized modified EVOH resin and a titanium compound using a tumbler or the like.

[0124] Examples of the melt mixing method include: (ii) a method of melt kneading a dry blend obtained by dry-blending a pelletized modified EVOH resin and a titanium compound; and (iii) a method of adding a titanium compound to a molten EVOH resin and melt kneading the mixture.

[0125] Examples of the solution mixing method include: (iv) a method in which a solution is prepared using a commercially available modified EVOH resin, a titanium compound is added to the solution, the solution is solidified and formed, and then the solution is separated from the solid by a known method and dried; (v) a method in which, during the manufacturing process of the modified EVOH resin, a titanium compound is added to an ethylene-vinyl ester copolymer solution before saponification or a uniform solution of EVOH resin (water / alcohol solution, etc.), the solution is solidified and formed, and then the solution is separated from the solid by a known method and dried.

[0126] Examples of the impregnation method include (vi) a method in which a granular modified EVOH resin is brought into contact with an aqueous solution containing a titanium compound to allow the modified EVOH resin to contain the titanium compound and then dry the solution.

[0127] As the aqueous solution containing a titanium compound, an aqueous solution of a titanium compound or an aqueous solution obtained by immersing a titanium compound in water containing various chemicals to dissolve titanium ions can be used.

[0128] In the above-mentioned impregnation method, the content (metal conversion) of the titanium compound can be controlled by the concentration of the titanium compound in the aqueous solution in which the modified EVOH resin is impregnated, the impregnation temperature, the impregnation time, and the like.

[0129] The immersion temperature and immersion time are usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.

[0130] As the drying method in each of the above-mentioned production methods, various drying methods can be adopted, and any of static drying and fluidized drying can be adopted. In addition, these methods can also be combined.

[0131] As described above, in the present invention, the above different methods can be combined. Among them, from the perspective of obtaining a resin composition with higher productivity and the effect of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when using the above other thermoplastic resins and other compounding agents, they can be compounded by conventional methods according to the above manufacturing method.

[0132] The modified EVOH resin composition obtained by the above-mentioned production methods may be in any shape, but is preferably in the form of pellets.

[0133] As the above-mentioned particles, for example, there are spherical, elliptical, cylindrical, cubic, rectangular parallelepiped, etc., usually elliptical or cylindrical, and its size is considered from the perspective of convenience when used as a molding material later. In the case of an elliptical shape, the short diameter is usually 1 to 10 mm, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm, and the long diameter is usually 1.5 to 30 mm, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm. In addition, in the case of a cylindrical shape, the diameter of the bottom surface is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.

[0134] Furthermore, the shape and size of the pelletized modified EVOH resin used in the above-mentioned production methods are also preferably the same.

[0135] The modified EVOH resin composition can suppress thermal degradation during heating, and the 5% weight loss temperature of the modified EVOH resin composition is usually 371° C. or higher, preferably 372° C. or higher, and particularly preferably 373° C. or higher.

[0136] The 10% weight loss temperature of the modified EVOH resin composition is usually 383° C. or higher, preferably 384° C. or higher.

[0137] The upper limits of the 5% weight loss temperature and the 10% weight loss temperature are preferably as high as possible and are usually 450°C.

[0138] In addition, a difference of 1° C. in the weight loss temperature described above manifests as a large difference in yield in actual production, and thus the difference is very large.

[0139] The above-mentioned 5% weight loss temperature and 10% weight loss temperature refer to the temperature (5% weight loss temperature) at which the weight is reduced to 95% of the weight before measurement and the temperature (10% weight loss temperature) at which the weight is reduced to 90% of the weight before measurement, using a thermogravimetric measuring apparatus (manufactured by Perkin Elmer, Pyris 1TGA) for 5 mg of the modified EVOH resin composition in a nitrogen atmosphere at an air flow rate of 20 mL / min, a heating rate of 10°C / min, and a temperature range of 30 to 550°C.

[0140] The water content of the modified EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0141] In addition, the water content of the modified EVOH resin composition is measured and calculated by the following method.

[0142] The mass (W1) of the modified EVOH resin composition before drying was weighed with an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and weighed after cooling in the dryer for 30 minutes (W2), and the mass was calculated by the following formula.

[0143] Water content (mass %) = [(W1-W2) / W1] × 100

[0144] In addition, when the modified EVOH resin composition is in the form of pellets, it is also preferred to attach a known lubricant to the surface of the pellets from the perspective of stabilizing the feeding property during melt molding. Examples of lubricants include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters, etc. of higher fatty acids), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauramide, myristic acid, palmitic acid, stearic acid, behenic acid amide; unsaturated higher fatty acid amides such as oleamide and erucic acid amide, bis-higher fatty acid amides such as ethylene bisstearamide, ethylene bisoleamide, ethylene biserucic acid amide, ethylene bislauric acid amide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene having a molecular weight of about 500 to 10,000, or low molecular weight polypropylene, etc., or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluoroethylene resins, etc. These compounds may be used alone or in combination of two or more. The content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less, of the modified EVOH resin composition. The lower limit is usually 0% by mass.

[0145] The modified EVOH resin composition thus obtained can be modulated into various forms such as granules, powders, and liquids, and provided as a molding material for various molded products. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to more effectively obtain the effects of the present invention, and therefore it is preferred.

[0146] It should be noted that the modified EVOH resin composition of the present invention also includes a resin composition obtained by mixing a resin other than the modified EVOH resin used in the modified EVOH resin composition of the present invention.

[0147] Examples of the molded product include a multilayer structure having a layer composed of the present modified EVOH resin composition, typified by a single-layer film molded from the present modified EVOH resin composition.

[0148] [Multilayer structure]

[0149] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present modified EVOH resin composition. The layer composed of the present modified EVOH resin composition (hereinafter referred to as "the present modified EVOH resin composition layer") can be further provided with strength, or the present modified EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating the layer composed of the present modified EVOH resin composition (hereinafter referred to as "the present modified EVOH resin composition layer") with another substrate having a thermoplastic resin other than the present modified EVOH resin composition as a main component (hereinafter, the resin used for the substrate is sometimes referred to as "substrate resin").

[0150] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers and ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, (unmodified) polyolefin resins such as polybutene, polypentene, and polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and polyolefin resins such as polypropylene resins modified with unsaturated carboxylic acids or The esters thereof include polyolefin resins in a broad sense, such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft-modifying these polyolefins, ionomer resins, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, halogenated polyolefins such as chlorinated polyethylene and chlorinated polypropylene, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0151] Among them, preferred are polyamide resins, polyolefin resins, polyester resins, and polystyrene resins as hydrophobic resins, and more preferred are polyolefin resins such as polyethylene resins, polypropylene resins, polycyclic olefin resins, and unsaturated carboxylic acid-modified polyolefin resins thereof.

[0152] When the modified EVOH resin composition layer is a (a1, a2, ...) and the base resin layer is b (b1, b2, ...), the layer structure of the multilayer structure may be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the regenerated layer obtained by remelting and molding the end portion, defective product, etc. generated in the process of manufacturing the multilayer structure and comprising a mixture of the modified EVOH resin composition and a thermoplastic resin other than the modified EVOH resin composition is R, it may also be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is generally 2 to 15, preferably 3 to 10 in total. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be interposed between the layers as necessary.

[0153] As the above-mentioned adhesive resin, known substances can be used, as long as they are appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include: modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins through addition reactions, grafting reactions, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. can be listed. They can be used alone or in combination of two or more.

[0154] In the present multilayer structure, when an adhesive resin layer is used between the present modified EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present modified EVOH resin composition layer, it is preferable to use an adhesive resin with excellent hydrophobicity.

[0155] The above-mentioned base resin and adhesive resin may contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating materials, antiblocking agents, waxes, etc. within a range that does not impair the gist of the present invention (e.g., 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These may be used alone or in combination of two or more.

[0156] The lamination of the modified EVOH resin composition layer and the substrate resin layer (including the case where an adhesive resin layer is interposed) can be carried out by a known method. For example, there can be listed: a method of melt-extrusion laminating the substrate resin on a film, sheet, etc. of the modified EVOH resin composition; a method of melt-extrusion laminating the modified EVOH resin composition on the substrate resin layer; a method of co-extruding the modified EVOH resin composition and the substrate resin; a method of dry laminating the modified EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc.; a method of removing the solvent after applying a solution of the modified EVOH resin composition on the substrate resin, etc. Among these, from the perspective of cost and environment, it is preferred to manufacture by a process of melt-molding the modified EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0157] The present multilayer structure can be subjected to (heating) stretching treatment as required. The stretching treatment can be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, it can be stretched simultaneously or successively. In addition, as a stretching method, a method with a high stretching ratio such as a roller stretching method, a tenter stretching method, a tubular stretching method, a stretch blow molding method, and a vacuum pressure forming method can be adopted. The stretching temperature is a temperature near the melting point of the multilayer structure, usually 40 to 170°C, preferably selected from the range of about 60 to 160°C. When the stretching temperature is too low, the stretchability becomes poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0158] In addition, the stretched multilayer structure may be heat-fixed for the purpose of imparting dimensional stability. Heat-fixing may be performed in a known manner, for example, by heat-treating the stretched multilayer structure for about 2 to 600 seconds at a temperature of usually 80 to 180° C., preferably 100 to 165° C., while maintaining the stretched multilayer structure in a tensioned state.

[0159] When the present multilayer structure after the stretching treatment is used as a shrink film, in order to impart heat shrinkage, the present multilayer structure after the stretching treatment may be cooled and fixed by blowing cold air instead of the heat setting.

[0160] The thickness of the present multilayer structure (including the stretched multilayer structure), the thickness of the present modified EVOH resin composition layer, the base resin layer and the adhesive resin layer further constituting the multilayer structure cannot be generalized due to the differences in layer constitution, type of base resin, type of adhesive resin, application, packaging method, required physical properties, etc., but the thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present modified EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0161] Furthermore, regarding the thickness ratio of the modified EVOH resin composition layer to the substrate resin layer in the present multilayer structure (the present modified EVOH resin composition layer / the substrate resin layer), when there are multiple layers, the ratio between the thickest layers is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60. In addition, regarding the thickness ratio of the modified EVOH resin composition layer to the adhesive resin layer in the present multilayer structure (the present modified EVOH resin composition layer / the adhesive resin layer), when there are multiple layers, the ratio between the thickest layers is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10.

[0162] In addition, the present multilayer structure can also be used to obtain a multilayer container in the shape of a cup or a tray. In this case, a deep drawing method is usually used, and specifically, vacuum forming, pressure forming, vacuum pressure forming, plunger-assisted vacuum pressure forming, etc. can be listed. Furthermore, in the case of obtaining a tube or bottle-shaped multilayer container (laminated structure) from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulator type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion cold parison biaxial stretch blow molding, injection cold parison biaxial stretch blow molding, injection molding online biaxial stretch blow molding, etc.) can be listed. The obtained laminate may be subjected to heat treatment, cooling treatment, calendaring treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, drawing processing, box processing, tube processing, slitting processing, etc. as necessary.

[0163] The single-layer film formed from the modified EVOH resin composition, the bag composed of the multilayer structure, and the container and cover composed of cups, trays, tubes, bottles, etc. are useful not only as packaging material containers for ordinary foods, but also as packaging material containers for various condiments such as mayonnaise and salad dressing, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, and pharmaceuticals.

[0164] Example

[0165] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to the following examples in any way.

[0166] It should be noted that the "portions" in the examples refer to the mass standard unless otherwise specified.

[0167] <Example 1>

[0168] As the modified EVOH resin having a primary hydroxyl structural unit in the side chain, particles of a modified EVOH resin containing 1,2-diol in the side chain (ethylene structural unit content 38 mol%, primary hydroxyl structural unit modification rate 1.5 mol%, saponification degree 99.6 mol%, MFR 4.0 g / 10 minutes (210°C, load 2160 g)) were used.

[0169] In addition, titanium oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the titanium compound.

[0170] The titanium oxide was dry-blended with the modified EVOH resin pellets so that the content of the titanium oxide was 0.1 ppm based on the unit mass of the EVOH resin composition in terms of metal conversion, thereby obtaining a mixture.

[0171] The mixture was supplied to a twin-screw extruder (20 mm φ) equipped with a two-hole die and extruded under the following extrusion conditions, and the discharged strands were cooled and solidified on a belt conveyor. The solidified strands were then cut to obtain pellets of a modified EVOH resin composition.

[0172] [Extrusion conditions]

[0173] Extruder set temperature (℃): C1 / C2 / C3 / C4 / C5 / C6

[0174] =150 / 200 / 210 / 210 / 210 / 210

[0175] <Example 2>

[0176] Pellets of a modified EVOH resin composition were obtained in the same manner as in Example 1 except that the amount of titanium oxide added in Example 1 was changed to 1 ppm in terms of metal relative to the unit mass of the EVOH resin composition.

[0177] <Comparative Example 1>

[0178] Pellets of a modified EVOH resin composition were obtained in the same manner as in Example 1 except that the titanium oxide in Example 1 was not used.

[0179] <Comparative Example 2>

[0180] Pellets of a modified EVOH resin composition were obtained in the same manner as in Example 1 except that the amount of titanium oxide added in Example 1 was changed to 10 ppm in terms of metal relative to the unit mass of the EVOH resin composition.

[0181] The following thermal stability evaluation was performed using the obtained pellets of the modified EVOH resin compositions of Examples 1 and 2 and Comparative Examples 1 and 2. The results are shown in Table 1 described below.

[0182] [Thermal stability evaluation]

[0183] 5 mg of the pellets of the obtained EVOH resin composition were measured using a thermogravimetric measuring apparatus (manufactured by Perkin Elmer, Pyris 1TGA) under nitrogen atmosphere, gas flow rate: 20 mL / min, temperature rise rate: 10°C / min, temperature range: 30 to 550°C, and the temperature at which the weight decreased to 95% of the weight before measurement (5% weight loss temperature) and the temperature at which the weight decreased to 90% of the weight before measurement (10% weight loss temperature) were measured. The higher the temperature, the better the thermal stability.

[0184] [Table 1]

[0185]

[0186] As can be seen from Table 1, the EVOH resin compositions of Examples 1 and 2 containing a specific trace amount of titanium compound have a higher weight loss temperature and excellent thermal stability than the EVOH resin composition of Comparative Example 1 not containing a titanium compound and the EVOH resin composition of Comparative Example 2 containing a titanium compound exceeding a specific range. In addition, the multilayer structure having a layer composed of the EVOH resin composition of Examples 1 and 2 can also obtain the effect of suppressing thermal degradation and excellent thermal stability.

[0187] The above embodiments show specific aspects of the present invention, but the above embodiments are merely illustrative and are not to be construed as limiting. It should be understood that various modifications obvious to those skilled in the art are within the scope of the present invention.

[0188] Industrial Applicability

[0189] Since the modified EVOH resin composition can suppress the degradation caused by heat during heating, it is useful as a packaging material for various foods, and is also useful as a packaging material for various condiments such as mayonnaise and salad dressing, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, and pharmaceuticals.

Claims

1. A modified ethylene-vinyl alcohol copolymer composition, comprising a modified ethylene-vinyl alcohol copolymer having a primary hydroxyl structural unit in a side chain and a titanium compound, The metal equivalent content of the titanium compound is 0.001 ppm or more and less than 5 ppm based on the unit mass of the modified ethylene-vinyl alcohol-based copolymer composition. 2 . The modified ethylene-vinyl alcohol copolymer composition according to claim 1 , wherein the content of ethylene structural units in the modified ethylene-vinyl alcohol copolymer is 20 to 60 mol %. 3 . The modified ethylene-vinyl alcohol copolymer composition according to claim 1 , wherein the modification rate of the primary hydroxyl structural unit in the side chain of the modified ethylene-vinyl alcohol copolymer is 0.1 to 30 mol %.

4. The modified ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 3, wherein the primary hydroxyl structural unit in the side chain of the modified ethylene-vinyl alcohol copolymer is represented by the following general formula (1): In the formula, R 1 ~R 3 Each independently represents a hydrogen atom or an organic group, and X represents a single bond or a bond chain. 5 . Pellets comprising the modified ethylene-vinyl alcohol copolymer composition according to claim 1 . 6 . A multilayer structure comprising at least one layer comprising the modified ethylene-vinyl alcohol copolymer composition according to claim 1 .

7. A method for producing a modified ethylene-vinyl alcohol copolymer composition, which is a method for producing the modified ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 4, The method comprises the step of melt-mixing a composition raw material containing the modified ethylene-vinyl alcohol-based copolymer and a titanium compound.

8. A method for producing a multilayer structure, which is a method for producing the multilayer structure according to claim 6, The method comprises the step of melt-molding a layer composed of the modified ethylene-vinyl alcohol copolymer composition.