Two-component thermally conductive addition-curable silicone composition and cured silicone product thereof

By adding specific components and metal complexes to the thermally conductive silicone composition, the problem of hardness increase during high temperature aging at 150°C is solved, high heat resistance and initial performance are maintained, and it is suitable for heat dissipation applications of electronic components. .

CN118804952APending Publication Date: 2024-10-18SHIN ETSU CHEMICAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380025147.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-08
Filing Date
2023-02-21
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The existing thermally conductive silicone composition has a problem of increasing hardness when aged at a high temperature of 150°C, resulting in a decrease in heat dissipation performance and making it difficult to maintain initial performance during long-term use.

Method used

A two-component thermally conductive addition-curable silicone composition is used by adding an organopolysiloxane having at least two alkenyl groups bonded to silicon atoms, a thermally conductive filler material and a platinum group metal catalyst into the composition , and a complex of metal and 8-hydroxyquinoline is added to suppress the increase in hardness.

Benefits of technology

It effectively suppresses the increase in hardness during aging at 150°C, maintains high heat resistance and initial heat dissipation performance, and is suitable for long-term use of electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0005024208440000041
    Figure BDA0005024208440000041
  • Figure BDA0005024208440000071
    Figure BDA0005024208440000071
Patent Text Reader

Abstract

A two-component thermally conductive addition-curable silicone composition which is a two-component thermally conductive addition-curable silicone composition comprising a first component and a second component, the first component containing (A) an organopolysiloxane having an alkenyl group bonded to a silicon atom, (C) a thermally conductive filler, and (E) a platinum group metal catalyst, and the second component containing (A) an organopolysiloxane having an alkenyl group bonded to a silicon atom, (C) a thermally conductive filler, and (E) a platinum group metal catalyst. The first component contains (A) an organopolysiloxane having an alkenyl group bonded to a silicon atom, the second component contains (A) an organopolysiloxane having an alkenyl group bonded to a silicon atom, (B) an organohydrogenpolysiloxane, and (C) a thermally conductive filler, the first component does not contain component (B), the second component does not contain component (E), and either or both of the first component and the second component contains (D) a complex of a metal and an 8-hydroxyquinoline.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a two-component thermally conductive addition-curable silicone composition, and more particularly to a silicone composition that forms a thermally conductive silicone cured product whose hardness increase from an initial hardness is suppressed during high-temperature aging at 150°C, and a silicone cured product thereof. Background Art

[0002] As for heat-generating electronic components, it is well known that heat is generated during use and the resulting performance degradation is caused. As a means to solve this problem, various heat dissipation technologies are used. Generally, a cooling member (heat sink, etc.) is arranged near the heat generating part so that the two are in close contact, and the cooling member efficiently removes heat to dissipate heat. At this time, if there is a gap between the heat generating member and the cooling member, the air with poor thermal conductivity is interposed between them, so the thermal conductivity is reduced and the temperature of the heat generating member is not sufficiently reduced. In order to prevent such a phenomenon, a heat dissipation material with good thermal conductivity and the ability to follow the surface of the component is used, such as heat dissipation grease and heat sink (Patent Documents 1 to 13: Japanese Patent No. 2938428, Japanese Patent No. 2938429, Japanese Patent No. 3580366, Japanese Patent No. 3952184, Japanese Patent No. 4572243, Japanese Patent No. 4656340, Japanese Patent No. 4913874, Japanese Patent No. 4917380, Japanese Patent No. 4933094, Japanese Patent No. 5283346, Japanese Patent No. 5233325, Japanese Patent No. 5553006, Japanese Patent No. 5447337).

[0003] However, the hardening type heat dissipation grease used after being sandwiched between components and solidified sometimes increases in hardness over time due to the heat generated by the electronic components during installation. The heat dissipation grease with increased hardness can no longer follow the "warping" caused by the thermal expansion and thermal contraction of the contact substrate surface, and peels off from the substrate, resulting in a decrease in heat dissipation performance. In addition, as the hardness increases, the elongation of the material decreases, the followability decreases, and the Young's modulus increases, which has an adverse effect on the solder joint life. Therefore, in order to obtain a material with high reliability, it is important to suppress the increase in hardness over time.

[0004] Therefore, in order to prevent the hardness of thermally conductive polysiloxane materials from increasing over time at high temperatures, compositions containing phthalocyanine pigments have been reported (Patent Document 14: Japanese Patent No. 6048416). Japanese Patent No. 6048416 discloses a thermally conductive polysiloxane material in which the hardness increase at 90°C and 120°C is suppressed.

[0005] In addition, as a thermally conductive silicone composition with a small increase in hardness during high-temperature aging, compositions containing various heat resistance improvers have been reported (Patent Document 15: Japanese Patent Application Publication No. 2018-123200). Japanese Patent Application Publication No. 2018-123200 discloses a thermally conductive silicone composition that suppresses the increase in hardness at 220°C for 250 hours.

[0006] On the other hand, it is also often necessary to suppress the increase in hardness during long-term aging at 150°C, mainly in automotive applications. However, conventional thermally conductive silicone compositions have insufficient heat resistance and have a problem of increasing hardness during long-term aging at a high temperature higher than 125°C and for more than 250 hours. In addition, when the amount of thermally conductive filler that causes the increase in hardness is increased to improve thermal conductivity, the hardness also increases during aging at 150°C.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent No. 2938428

[0010] Patent Document 2: Japanese Patent No. 2938429

[0011] Patent Document 3: Japanese Patent No. 3580366

[0012] Patent Document 4: Japanese Patent No. 3952184

[0013] Patent Document 5: Japanese Patent No. 4572243

[0014] Patent Document 6: Japanese Patent No. 4656340

[0015] Patent Document 7: Japanese Patent No. 4913874

[0016] Patent Document 8: Japanese Patent No. 4917380

[0017] Patent Document 9: Japanese Patent No. 4933094

[0018] Patent Document 10: Japanese Patent No. 5283346

[0019] Patent Document 11: Japanese Patent No. 5233325

[0020] Patent Document 12: Japanese Patent No. 5553006

[0021] Patent Document 13: Japanese Patent No. 5447337

[0022] Patent Document 14: Japanese Patent No. 6048416

[0023] Patent Document 15: Japanese Patent Application Publication No. 2018-123200 Summary of the invention

[0024] Problems to be solved by the invention

[0025] The present invention has been made in view of the above-mentioned actual situation, and an object of the present invention is to provide a two-component thermally conductive addition-curable composition that can form a thermally conductive silicone cured product having high heat resistance and capable of suppressing the hardness increase from the initial hardness during high-temperature aging at 150°C not only by heating curing but also by room temperature curing.

[0026] Means for solving problems

[0027] The present inventors have conducted intensive studies to achieve the above-mentioned object, and as a result, have found that by adding a complex based on a metal and 8-hydroxyquinoline to a specific thermally conductive addition-curable silicone composition, an increase in hardness during aging at 150° C. can be suppressed. The inventors have further found that a two-component thermally conductive addition-curable silicone composition consisting of a first component and a second component, wherein the first component contains (A) an organopolysiloxane having at least two alkenyl groups bonded to silicon atoms in one molecule, (C) a thermally conductive filler, and (E) a platinum group metal catalyst, and the second component contains (A) an organopolysiloxane having at least two alkenyl groups bonded to silicon atoms in one molecule, (B) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in one molecule, and (C) a thermally conductive filler, and that by adding (D) a complex based on a metal and 8-hydroxyquinoline to one or both of the first component and the second component, the composition has high heat resistance not only by heat curing but also by room temperature curing, and have completed the present invention.

[0028] Therefore, the present invention provides the following two-component thermally conductive addition-curable silicone composition.

[0029] 1. A two-component thermally conductive addition-curing silicone composition, which is a two-component thermally conductive addition-curing silicone composition consisting of a first component and a second component, wherein the first component contains:

[0030] (A) an organopolysiloxane having at least two alkenyl groups bonded to silicon atoms in one molecule,

[0031] (C) thermally conductive filler material, and

[0032] (E) a platinum group metal catalyst,

[0033] The second component contains:

[0034] (A) an organopolysiloxane having at least two alkenyl groups bonded to silicon atoms in one molecule,

[0035] (B) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in one molecule, and

[0036] (C) thermally conductive filling material,

[0037] The first component does not contain the component (B), the second component does not contain the component (E), and either or both of the first component and the second component contain a complex of a metal and 8-hydroxyquinoline (D).

[0038] The amount of the silicone composition is such that the number of silicon-bonded hydrogen atoms in the component (B) is 0.1 to 5.0 per alkenyl group in the component (A) in the entire composition obtained by combining the first component and the second component.

[0039] 2. The two-component thermally conductive addition-curable silicone composition according to 1, further comprising (F) an organosilane represented by the following general formula (1),

[0040] R 1 a R 2 b Si(OR 3 ) 4-a-b (1)

[0041] In the formula, R 1 are independently a monovalent hydrocarbon group having 4 to 20 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups having 4 to 20 carbon atoms, R 3 They are independently monovalent hydrocarbon groups having 1 to 6 carbon atoms, a is an integer of 1 to 3, b is an integer of 0 to 2, and a+b is an integer of 1 to 3.

[0042] 3. The two-component thermally conductive addition-curable silicone composition according to 1 or 2, further comprising (G) an organopolysiloxane represented by the following general formula (2),

[0043] [Chemistry 1]

[0044]

[0045] In the formula, R 4 are independently monovalent hydrocarbon groups, R 5 are independently alkyl, alkoxyalkyl, alkenyl or acyl, c is an integer of 5-100, and d is an integer of 1-3.

[0046] 4. The two-component thermally conductive addition-curable silicone composition according to any one of 1 to 3, wherein the amount of component (C) in each of the first component and the second component is 300 to 3000 parts by mass relative to 100 parts by mass of the total of components (A) and (B),

[0047] The amount of component (D) is 0.001 to 5.0% by mass of the total composition obtained by combining the first component and the second component.

[0048] The amount of the component (E) is 0.1 to 500 ppm in terms of mass of the platinum group metal relative to the total of the components (A) and (B) in the entire composition obtained by combining the first component and the second component.

[0049] 5. A two-component thermally conductive addition-curing silicone cured product, which is a cured product of the silicone composition according to any one of 1 to 4.

[0050] 6. The two-component thermally conductive addition-curing silicone cured material according to 5, which is in the form of a sheet.

[0051] Effects of the Invention

[0052] According to the present invention, a two-component thermally conductive addition-curable composition can be provided which forms a cured product whose hardness increase from the initial hardness can be suppressed when aged at 150° C. compared with a cured product formed from a conventional thermally conductive silicone composition. DETAILED DESCRIPTION

[0053] The present invention is described in detail below.

[0054] The two-component thermally conductive addition-curable silicone composition of the present invention is a two-component thermally conductive addition-curable silicone composition composed of a first component and a second component, wherein the first component contains:

[0055] (A) an organopolysiloxane having at least two alkenyl groups bonded to silicon atoms in one molecule,

[0056] (C) thermally conductive filler material, and

[0057] (E) a platinum group metal catalyst,

[0058] The second component contains:

[0059] (A) an organopolysiloxane having at least two alkenyl groups bonded to silicon atoms in one molecule,

[0060] (B) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in one molecule, and

[0061] (C) thermally conductive filling material,

[0062] The first component does not contain the above-mentioned component (B), the second component does not contain the above-mentioned component (E), and either or both of the first component and the second component contain (D) a complex of a metal and 8-hydroxyquinoline,

[0063] The amount of hydrogen atoms bonded to silicon atoms in the component (B) is 0.1 to 5.0 per alkenyl group in the component (A) in the entire composition obtained by combining the first component and the second component.

[0064] [(A) ingredient]

[0065] The component (A) of the composition of the present invention is a component that becomes the main agent (base polymer) of the composition, and one kind can be used alone or two or more kinds can be used in combination. The component (A) is an organopolysiloxane having at least two alkenyl groups bonded to silicon atoms (hereinafter sometimes referred to as "silicon atom-bonded alkenyl groups") in one molecule. As for the alkenyl groups bonded to silicon atoms, it is preferred to have 2 to 50, and more preferably 2 to 20. These silicon atom-bonded alkenyl groups may be bonded to the silicon atoms at the ends of the molecular chain, may be bonded to the silicon atoms at non-terminal ends of the molecular chain (i.e., other than the ends of the molecular chain), or may be a combination thereof.

[0066] R 6 e R 7 f SiO (4-e-f) / 2 (3)

[0067] (Where R 6 are independently alkenyl, R 7 are independently unsubstituted or substituted monovalent hydrocarbon groups having no aliphatic unsaturated bonds, e is 0.0001 to 0.2, f is 1.7 to 2.2, and e+f is a positive number satisfying 1.9 to 2.4.

[0068] In addition, e and f are appropriately selected so as to have at least two alkenyl groups bonded to a silicon atom in one molecule.

[0069] Examples of the alkenyl group include alkenyl groups having 2 to 6 carbon atoms, such as vinyl, allyl, isopropenyl, 1-butenyl, 1-pentenyl, and 1-hexenyl. Among these, alkenyl groups having 2 to 4 carbon atoms are preferred, and vinyl groups are more preferred.

[0070] As the residual organic group bonded to the silicon atom (for example, R 7), unsubstituted or substituted monovalent hydrocarbon groups having no aliphatic unsaturated bonds may be listed, and the number of carbon atoms is preferably 1 to 12, and more preferably 1 to 6. Specific examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, hexyl, cyclohexyl, octyl, and dodecyl; aryl groups such as phenyl, 1-naphthyl, 2-naphthyl, and tolyl; aralkyl groups such as benzyl and 2-phenylethyl; groups in which a part or all of the hydrogen atoms of these groups are substituted with halogen atoms such as fluorine, chlorine, and bromine, chloromethyl, and 3,3,3-trifluoropropyl. From the viewpoint of ease of synthesis, methyl, phenyl, and 3,3,3-trifluoropropyl are preferred.

[0071] In formula (3), e is a positive number of 0.0001 to 0.2, preferably a positive number of 0.0005 to 0.1. f is a positive number of 1.7 to 2.2, preferably a positive number of 1.9 to 2.0. e+f is a positive number satisfying 1.9 to 2.4, preferably a positive number satisfying 1.95 to 2.05.

[0072] The kinematic viscosity of the component (A) at 25° C. measured by an Ostwald viscometer is preferably 10 to 100,000 mm 2 / s, more preferably 100 to 50000 mm 2 / s. At this viscosity of 50 to 100000 mm 2 / s, the obtained cured product becomes more excellent in strength, fluidity and handleability. Examples of the organopolysiloxane of the component (A) satisfying the above characteristics include organopolysiloxane represented by the following general formula (4).

[0073] [Chemistry 2]

[0074]

[0075] (Where R 8 are independently unsubstituted or substituted monovalent hydrocarbon groups. 8 At least two of them are alkenyl groups, and g is an integer from 20 to 2000. )

[0076] In the formula (4), R 8 The unsubstituted or substituted monovalent hydrocarbon group represented by 6 (alkenyl) and R 7 The monovalent hydrocarbon group defined in (unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bond) is the same as the monovalent hydrocarbon group defined in (unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bond), and the number of carbon atoms, specific examples, etc. thereof are also the same. 8At least two, preferably 2 to 50, and more preferably 2 to 20, of the total number of alkenyl groups are alkenyl groups. If the number of alkenyl groups is too small, the crosslinking density of the resulting thermally conductive silicone cured product sometimes decreases excessively and no longer cures. If the number of alkenyl groups is too large, the crosslinking density of the resulting thermally conductive silicone cured product increases, and the curing properties sometimes become unstable. In addition, g is preferably an integer of 40 to 1200, and more preferably an integer of 50 to 600. If the number of g is too small, the viscosity of the resulting thermally conductive silicone composition decreases, the handling operability deteriorates, and the resulting cured product becomes brittle. On the other hand, if the number of g is too large, the viscosity of the resulting thermally conductive silicone composition increases, and the handling operability deteriorates.

[0077] Specific examples of the organopolysiloxane represented by the above formula (4) include dimethylpolysiloxane having both ends of the molecular chain capped with dimethylvinylsiloxy groups, dimethylsiloxane-methylvinylsiloxane copolymer having both ends of the molecular chain capped with trimethylsiloxy groups, dimethylsiloxane-methylvinylsiloxane copolymer having one end of the molecular chain capped with trimethylsiloxy groups and one end of the molecular chain capped with dimethylvinylsiloxane groups, dimethylsiloxane-methylvinylsiloxane copolymer having both ends of the molecular chain capped with dimethylvinylsiloxy groups, and dimethylsiloxane-diphenylsiloxane copolymer having both ends of the molecular chain capped with dimethylvinylsiloxy groups.

[0078] The above-mentioned organopolysiloxane having an alkenyl group is known per se and can be produced by a conventionally known method.

[0079] [(B) ingredient]

[0080] Examples of the component (B) include organohydrogenpolysiloxanes represented by the following average composition formula (5) and having at least two hydrogen atoms bonded to silicon atoms in one molecule.

[0081] R 9 h H i SiO (4-h-i) / 2 (5)

[0082] (Where R 9 Each of the following is independently an unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bond, h is 0.7 to 2.2, i is 0.001 to 0.5, and h+i is a positive number satisfying 0.8 to 2.5. h and i are appropriately selected so that at least two hydrogen atoms bonded to silicon atoms are present in one molecule.

[0083] In the above formula (5), R 9It is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms, preferably 1 to 6 carbon atoms, without an aliphatic unsaturated bond. Specific examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, hexyl, cyclohexyl, octyl, and dodecyl; aryl groups such as phenyl, 1-naphthyl, 2-naphthyl, and tolyl; aralkyl groups such as benzyl and 2-phenylethyl; and groups in which a part or all of the hydrogen atoms of these groups are substituted with halogen atoms such as fluorine, chlorine, and bromine, chloromethyl, and 3,3,3-trifluoropropyl. Among them, methyl, phenyl, and 3,3,3-trifluoropropyl are preferred from the viewpoint of ease of synthesis.

[0084] In the above formula (5), h is a positive number of 0.7 to 2.2, preferably a positive number of 1.0 to 2.1. i is a positive number of 0.001 to 0.5, preferably a positive number of 0.005 to 0.1. h+i is a positive number satisfying 0.8 to 2.5, preferably a positive number satisfying 1.0 to 2.3, and more preferably a positive number satisfying 1.5 to 2.2. It should be noted that h and i are appropriately selected so that there are at least two hydrogen atoms bonded to silicon atoms in one molecule.

[0085] The number of silicon atoms in one molecule of the organohydrogenpolysiloxane of component (B) (i.e., degree of polymerization) is generally 10 to 1000, but preferably 20 to 500, more preferably 20 to 100, from the perspective of good handling properties of the composition and the properties of the resulting cured product. If the degree of polymerization is too low, the viscosity of the resulting thermally conductive silicone composition decreases, the handling properties deteriorate, and the resulting cured product becomes brittle. If the degree of polymerization is too high, the viscosity of the resulting thermally conductive silicone composition increases, and the handling properties deteriorate.

[0086] The molecular structure of the organohydrogenpolysiloxane of the component (B) is not particularly limited as long as it satisfies the above-mentioned characteristics.

[0087] The viscosity of the organohydrogenpolysiloxane of the component (B) at 25° C. is preferably 1 to 10,000 mPa·s, more preferably 3 to 2,000 mPa·s, and even more preferably 10 to 1,000 mPa·s, and is preferably liquid at room temperature (25° C.). The viscosity is a value measured using a B-type rotational viscometer, and the type of spindle (e.g., BL type, BM type, BH type, BS type) and the rotation speed are appropriately selected depending on the viscosity.

[0088] Examples of the organohydrogenpolysiloxane represented by the formula (4) include methylhydrogensiloxane-dimethylsiloxane cyclic copolymers, methylhydrogenpolysiloxane having both ends of the molecular chain blocked with dimethylhydrogensiloxy groups, methylhydrogen-dimethylsiloxane copolymers having both ends of the molecular chain blocked with dimethylhydrogensiloxy groups, methylhydrogen-diphenylsiloxane copolymers having both ends of the molecular chain blocked with dimethylhydrogensiloxy groups, and methylhydrogen-diphenylsiloxane copolymers having both ends of the molecular chain blocked with dimethylhydrogensiloxy groups. Methylsiloxane-diphenylsiloxane copolymer, methylhydrogenpolysiloxane having trimethylsiloxy end-capped molecular chain terminals, dimethylsiloxane-methylhydrogensiloxane copolymer having trimethylsiloxy end-capped molecular chain terminals, methylhydrogensiloxane-diphenylsiloxane copolymer having trimethylsiloxy end-capped molecular chain terminals, methylhydrogensiloxane-diphenylsiloxane-dimethylsiloxane copolymer having trimethylsiloxy end-capped molecular chain terminals, (CH3)2HS iO 1 / 2 unit, (CH3)2S iO unit and CH3S iO 3 / 2 The copolymer is composed of (CH3)2HSiO 1 / 2 unit, (CH3)2S iO unit, (CH3)HS iO unit and CH3S iO 3 / 2 The copolymer is composed of (CH3)3SiO 1 / 2 unit, (CH3)2SiO unit, (CH3)HSiO unit and CH3SiO 3 / 2 The copolymer is composed of (CH3)2HSiO 1 / 2 unit, (C6H5)2SiO unit, (CH3)2SiO unit and CH3SiO 3 / 2 The copolymer is composed of (CH3)(C6H5)HSiO 1 / 2 unit, (CH3)2SiO unit and CH3SiO 3 / 2 The copolymer is composed of (CH3)2HSiO 1 / 2 unit, (CH3)2SiO unit and C6H5SiO 3 / 2 The copolymer is composed of (CH3)(CF3C2H4)HSiO 1 / 2 unit, (CH3)(CF3C2H4)SiO unit and CH3SiO 3 / 2 The copolymer is composed of (CH3)(CF3C2H4)HSiO 1 / 2 unit, (CH3)(CF3C2H4)SiO unit, (CH3)2SiO unit and CH3SiO 3 / 2 The copolymer is composed of (CH3)2HSiO 1 / 2 unit, (CH3)(CF3C2H4)SiO unit and CH3SiO3 / 2 The copolymer is composed of (CH3)2HSiO 1 / 2 unit, (CH3)(CF3C2H4)SiO unit, (CH3)2SiO unit and CH3SiO 3 / 2 The copolymer is composed of (CH3)2HSiO 1 / 2 unit, (CH3)(CF3C2H4)SiO unit, (CH3)2SiO unit and (CF3C2H4)SiO 3 / 2 The copolymer is composed of (CH3)2HSiO 1 / 2 unit, (CH3)3SiO unit and SiO 4 / 2 The copolymer is composed of (CH3)2HSiO 1 / 2 unit, (CH3)2SiO unit and SiO 4 / 2 The copolymer is composed of (CH3)2HSiO 1 / 2 unit, (CH3)2SiO unit, (CH3)HSiO unit and SiO 4 / 2 The copolymer is composed of (CH3)3SiO 1 / 2 unit, (CH3)2SiO unit, (CH3)HSiO unit and SiO 4 / 2 Copolymers composed of units, etc.

[0089] The component (B) is used in the second component and is not contained in the first component. The amount of the organohydrogenpolysiloxane of the component (B) is such that the number of hydrogen atoms (SiH groups) bonded to silicon atoms in the component (B) is 0.1 to 5.0, preferably 0.1 to 2.0, and more preferably 0.1 to 1.5, relative to one alkenyl group in the component (A) and one hydrogen atom (SiH group) bonded to silicon atoms in the component (B) in the entire composition obtained by combining the first component and the second component. If the amount is too small, the effect of improving the storage stability may become insufficient, and if the amount is too large, the physical properties of the obtained thermally conductive silicone cured product may become unstable.

[0090] [(C) ingredient]

[0091] Component (C) is a thermally conductive filler, which can be used alone or in combination of two or more. Examples of the thermally conductive filler include aluminum hydroxide, magnesium hydroxide, aluminum oxide, crystalline silicon dioxide, zinc oxide, magnesium oxide, titanium oxide, beryllium oxide, aluminum nitride, boron nitride, metallic silicon, silicon nitride, silicon carbide, gold, silver, copper, iron, nickel, aluminum, stainless steel, gallium, indium, graphite, carbon fiber, diamond, and the like.

[0092] The thermal conductivity of the thermally conductive filler of component (C) is preferably 1 to 1000 W / m·°C [W / (m·°C)], and the lower limit of the thermal conductivity is preferably 10 W / m·°C or more, and more preferably 15 W / m·°C or more. The higher the thermal conductivity, the better, but the upper limit of the thermal conductivity of the thermally conductive filler that can be handled technically is 1000 W / m·°C. If the thermal conductivity of the filler is less than 1 W / m·°C, the thermal conductivity of the thermally conductive silicone composition itself may become small.

[0093] The shape of the particles of component (C) may be any shape, but preferably crushed particles, slightly rounded particles, spherical particles or polyhedral particles. The average particle size of component (C) is preferably 0.1 to 100 μm, more preferably 0.1 to 80 μm. The average particle size is determined by the volume average particle size (cumulative average diameter D) measured by laser diffraction method. 50 (median diameter)). When the average particle diameter is less than 0.1 μm, the obtained composition does not become grease-like and may lack stretchability. When it is larger than 100 μm, the thermal resistance of the heat dissipating grease increases and the performance may be reduced.

[0094] The component (C) is used in both the first component and the second component. The ratio of the component (C) used in the first component and the second component is not particularly limited as long as the mixing ratio of the first component and the second component is substantially the same in mass ratio.

[0095] The amount of component (C) is preferably 300 to 3000 parts by mass, more preferably 300 to 2800 parts by mass, and even more preferably 300 to 2500 parts by mass, relative to 100 parts by mass of the total of components (A) and (B) in each of the first component and the second component. If it is less than 300 parts by mass, the thermal conductivity of the composition may decrease, and if it exceeds 3000 parts by mass, the viscosity of the composition increases, and it may become lacking in stretchability.

[0096] [(D) ingredient]

[0097] The component (D) of the present invention is a complex of a metal and 8-hydroxyquinoline, and one kind thereof can be used alone or in combination of two or more kinds thereof. Examples of the metal include lithium, magnesium, aluminum, zinc, iron, copper, gallium, and indium, preferably aluminum, zinc, and copper, and more preferably copper. Examples of the component (D) include additives selected from complexes formed by metals and 8-hydroxyquinolines represented by the following general formula (6).

[0098] [Chemistry 3]

[0099]

[0100] (Where R 10 ~R15 are independently a hydrogen atom, a halogen atom, or an unsubstituted or substituted monovalent hydrocarbon group, and n is a positive number of 1 to 3.

[0101] These also include hydrates.

[0102] R 10 ~R 15 They are independently a hydrogen atom, a halogen atom, or an unsubstituted or substituted monovalent organic group. Examples of the halogen atom include fluorine, chlorine, bromine, and iodine. Examples of the organic group include a monovalent hydrocarbon group, an alkoxy group, an acyl group, an amide group, and an amino group.

[0103] The monovalent hydrocarbon group preferably has 1 to 12 carbon atoms, and more preferably has 1 to 6 carbon atoms. Specific examples of the monovalent hydrocarbon group include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, hexyl, cyclohexyl, octyl, and dodecyl; aryl groups such as phenyl, 1-naphthyl, 2-naphthyl, and tolyl; aralkyl groups such as benzyl and 2-phenylethyl; groups in which a part or all of the hydrogen atoms of these groups are substituted with halogen atoms such as fluorine, chlorine, and bromine; chloromethyl, 3,3,3-trifluoropropyl, and the like.

[0104] Examples of the alkoxy group include alkoxy groups having 1 to 10 carbon atoms, such as methoxy and ethoxy groups; examples of the acyl group include formyl, acetyl, benzoyl and the like; examples of the amide group include acetamide groups; and examples of the nitro group, nitroso group, sulfone group, primary amino group or secondary amino group may also be mentioned.

[0105] In the above formula (6), the metal atom represented by M is preferably lithium, magnesium, aluminum, zinc, iron, copper, gallium, indium or the like, more preferably aluminum, zinc, copper, and still more preferably copper.

[0106] Examples of the complex composed of a metal and 8-quinolinol represented by the above formula (6) include bis(8-quinolinol)copper(II), tris(8-quinolinol)aluminum(III), bis(8-quinolinol)zinc(II), (8-quinolinol)lithium(I), bis(2-methyl-8-quinolinol)copper(II), bis(2-methoxy-8-quinolinol)copper(II), bis(2-formyl-8-quinolinol)copper(II), bis(5-fluoro-8-quinolinol)copper(II), bis(5-chloro-8-quinolinol)copper(II), bis(5-bromo-8-quinolinol)copper(II), bis(5,7-dibromo-8-quinolinol)copper(II), and bis(5-nitroso-8-quinolinol)copper(II).

[0107] The component (D) is blended into either or both of the first component and the second component.

[0108] The amount of (D) is preferably 0.001 to 5.0% by mass, more preferably 0.01 to 1.0% by mass, and still more preferably 0.01 to 0.5% by mass relative to the entire composition. In order to further exert the effect of suppressing the increase in hardness during high temperature aging, the amount of (D) component is preferably 0.001% by mass or more, and even if it is more than 5.0% by mass, the effect corresponding to the amount used is not exhibited.

[0109] [(E) ingredient]

[0110] The (E) component of the composition of the present invention is a platinum group metal catalyst, which is a catalyst for promoting the addition reaction of the alkenyl group in the (A) component and the hydrogen atom bonded to the silicon atom in the (B) component. (E) component can be used alone or in combination of two or more. As (E) component, for example, chloroplatinic acid, alcohol-modified chloroplatinic acid, chloroplatinic acid and olefins, aldehydes, vinyl siloxanes or acetylenic compounds, tetrakis (triphenylphosphine) palladium, chlorotris (triphenylphosphine) rhodium, etc. can be listed. Among them, preferably a platinum catalyst, more preferably a complex (coordination compound) of chloroplatinic acid and vinyl siloxane.

[0111] The component (E) is mixed only in the first component and is not mixed in the second component.

[0112] The amount of the component (E) may be a catalytic amount, and is preferably 0.1 to 500 ppm, more preferably 2 to 100 ppm, based on the mass of the platinum group metal relative to the total of the components (A) and (B) of the entire composition obtained by combining the first component and the second component. From the perspective of obtaining appropriate curability, the amount of the component (E) is preferably within this range.

[0113] [(F)INGREDIENT]

[0114] The composition of the present invention may contain (F) an organosilane represented by the following general formula (1), if necessary.

[0115] R 1 a R 2 b Si(OR 3 ) 4-a-b (1)

[0116] (Where R 1 are independently a monovalent hydrocarbon group having 4 to 20 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups having 4 to 20 carbon atoms, R 3 are independently monovalent hydrocarbon groups having 1 to 6 carbon atoms, a is an integer of 1 to 3, b is an integer of 0 to 2, wherein a+b is an integer of 1 to 3.

[0117] By combining the component (F), the effect of reducing the viscosity of the silicone composition can be obtained. The (F) organosilane can be used alone or in combination of two or more. Examples of the (F) component include hexyltrimethoxysilane, decyltrimethoxysilane, hexadecyltrimethoxysilane, decylmethyldimethoxysilane, decyldimethylmethoxysilane, decyltriethoxysilane, 7-octenyltrimethoxysilane, and phenyltrimethoxysilane, and decyltrimethoxysilane is particularly preferred.

[0118] In the present invention, when the component (F) is used, it is preferred to prepare a heat-treated mixture together with the above-mentioned component (C) or components (A) to (C) at a temperature of 70°C or above, or the component (C) may be treated in advance with the component (F). By treating the component (C) with the component (F), the effect of lowering the viscosity of the obtained silicone composition is obtained. In this case, as a surface treatment method for the component (C) using the component (F), a spray method using a fluid nozzle, a stirring method with shear force, a ball mill, a mixer, or a dry method, or a water-based or organic solvent-based wet method may be adopted. The stirring is performed to such an extent that the thermally conductive filler is not destroyed. The temperature in the system in the dry method or the drying temperature after the treatment is appropriately determined according to the type of the surface treatment agent in the region where the surface treatment agent does not volatilize or decompose, and is 80 to 180°C.

[0119] When the (F) component is added, it can be added to either the first component or the second component or both. The amount of the (F) component added is preferably 0.1 to 5.0 parts by mass, more preferably 0.3 to 5.0 parts by mass, relative to 100 parts by mass of the (C) component of the entire composition obtained by combining the first component and the second component. If it is less than 0.1 parts by mass, the effect of lowering the viscosity is small, and even if it is more than 5.0 parts by mass, the effect corresponding to the amount used is not shown.

[0120] [(G) ingredient]

[0121] In the composition of the present invention, an organopolysiloxane represented by the following general formula (2) containing at least one hydrolyzable silyl group in one molecule may be used as necessary. By adding the component (G), the viscosity of the obtained silicone composition can be reduced.

[0122] [Chemistry 4]

[0123]

[0124] (Where R 4 are independently monovalent hydrocarbon groups, R 5 are independently alkyl, alkoxyalkyl, alkenyl or acyl, c is an integer of 5 to 100, and d is an integer of 1 to 3.

[0125] In the above formula (2), R 4 R is independently unsubstituted or substituted, preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms, more preferably 1 to 6 carbon atoms, and further preferably 1 to 3 carbon atoms. Specific examples thereof include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, hexyl, cyclohexyl, octyl, and dodecyl; aryl groups such as phenyl, 1-naphthyl, 2-naphthyl, and tolyl; aralkyl groups such as benzyl and 2-phenylethyl; chloromethyl and 3,3,3-trifluoropropyl groups in which a part or all of the hydrogen atoms of these groups are substituted with halogen atoms such as fluorine, chlorine, and bromine. 4 , preferably methyl, phenyl, 3,3,3-trifluoropropyl.

[0126] In the above formula (2), R 5 are independently alkyl, alkoxyalkyl, alkenyl or acyl. Examples of the alkyl group include 4 The same linear alkyl, branched alkyl, and cyclic alkyl groups as those exemplified in . Examples of alkoxyalkyl groups include methoxyethyl and methoxypropyl groups, and groups having 2 to 10 carbon atoms are preferred. Examples of alkenyl groups include the same R as those described above. 4 The alkenyl groups are the same as those exemplified in , and preferably have 1 to 8 carbon atoms. Examples of the acyl group include acetyl and octanoyl, and preferably have 2 to 10 carbon atoms. 5 An alkyl group is preferred, and a methyl group or an ethyl group is more preferred.

[0127] Moreover, c is an integer of 5 to 100, preferably an integer of 8 to 50, and d is an integer of 1 to 3, preferably 3. As the (G) component, (G1) used in Examples and the organopolysiloxane shown below can be exemplified.

[0128] [Chemistry 5]

[0129]

[0130] (In the formula, Me is a methyl group. The same applies below.)

[0131] The viscosity of the organopolysiloxane of the component (G) at 25°C is usually 0.01 to 30 Pa·s, preferably 0.01 to 10 Pa·s. If the viscosity is lower than 0.01 Pa·s, oil bleeding from the component (G) of the silicone composition may occur easily. If the viscosity is higher than 30 Pa·s, the fluidity of the obtained silicone composition becomes significantly lacking, and the coating operability may deteriorate. It should be noted that the viscosity is a value measured using a B-type rotational viscometer. According to the viscosity, the type of spindle (e.g., BL type, BM type, BH type, BS type) and the rotation speed are appropriately selected.

[0132] In the present invention, when the component (G) is used, it is preferred to prepare a heat-treated mixture together with the component (C) or the components (A) to (D) at a temperature of 70°C or higher. A more preferred temperature is 80 to 180°C.

[0133] When the (G) component is added, it can be added to either the first component or the second component or both. The amount of the (G) component added is preferably 0.5 to 90.0 parts by mass, more preferably 1.0 to 90.0 parts by mass, and further preferably 1.5 to 70.0 parts by mass, relative to 100 parts by mass of the (C) component of the entire composition obtained by combining the first component and the second component. If the amount of the (G) component added is less than 0.5 parts by mass, the effect of reducing the viscosity is small. If it is more than 90.0 parts by mass, oil bleeding from the (G) component of the silicone composition may occur easily.

[0134] The composition of the present invention may contain various additives known per se as other compounding ingredients in addition to the above-mentioned components (A) to (G) within a range not impairing the purpose of the present invention.

[0135] For example, a reaction control agent for adjusting the curing speed and storage stability can be added, specifically, alkynyl alcohols such as triallyl isocyanate alkyl maleate, ethynyl decyl methyl carbinol, ethynyl cyclohexanol, and silanes, siloxane-modified products, hydroperoxides, tetramethylethylenediamine, benzotriazole, etc., ferrous oxide, ferric oxide, etc. as colorants, alone or in combination, fumed silica as a thixotropy imparting agent, etc. The amount of each of these is preferably 0.01 to 100,000 ppm by mass of the entire composition obtained by combining the first component and the second component.

[0136] [Manufacturing method]

[0137] The composition of the present invention is a two-component thermally conductive addition-curable silicone composition, wherein the first component contains the above-mentioned (A), (C), (E) components and the above-mentioned (F), (G) components and other components as needed, but does not contain the above-mentioned (B) component; the second component contains the above-mentioned (A), (B), (C) components and the above-mentioned (F), (G) components and other components as needed, but does not contain the above-mentioned (E) component, and the above-mentioned (D) component is contained in either or both of the first component and the second component.

[0138] The composition of the present invention may be produced by mixing the components of the first component and the second component. For the first component, for example, a production method having the following steps can be mentioned.

[0139] A step of mixing the components (A), (C) and (component (D)) and, if necessary, the components (F) and (G), and heating them at a temperature of 70° C. or higher to obtain a heated mixture;

[0140] A step of cooling the heated mixture obtained above to room temperature (25° C.) or lower and then adding the component (E).

[0141] For the second component:

[0142] A step of mixing the components (A), (B), (C) and (D) and, if necessary, the components (F) and (G), and heating them at a temperature of 70° C. or higher to obtain a heated mixture;

[0143] A step of cooling the heated mixture obtained above to room temperature (25° C.) or lower and then adding a reaction control agent, a coloring agent, and a thixotropic agent.

[0144] For both the first component and the second component, the heating temperature is preferably 70° C. or higher, more preferably 70 to 180° C. The heating time is not particularly limited, but is preferably 1 hour or longer, more preferably 1 to 3 hours. It should be noted that when the additive is added, it can be added in any process, preferably after the heated mixture is cooled. As for the mixing device when preparing the first component and the second component, a known mixer such as a static mixer, a planetary mixer, and a paddle mixer can be used.

[0145] As for the thermal conductivity of the first component and the second component of the present invention, in the hot plate method according to ISO 22007-2, they are preferably 0.1 W / m·K or more, and more preferably 0.5 W / m·K or more. If the thermal conductivity is too low, the heat dissipation performance of the heat-generating electronic component may become insufficient. It should be noted that there is no particular limitation on the upper limit of the thermal conductivity, and it can be set to less than 20.0 W / m·K or less than 15.0 W / m·K. It should be noted that in the present invention, when the thermal conductivity is to be within the above range, it can be achieved in particular by making the amount of component (C) within the above-specified range.

[0146] The viscosity of the first component and the second component of the present invention at 25°C is preferably 10 to 1000 Pa·s, more preferably 30 to 800 Pa·s, based on a spiral viscometer: Malcom viscometer (model PC-10AA, rotation speed 10 rpm). If the viscosity is too low, the shape retention of the present composition may be insufficient, and if it is too high, the operability may be difficult. It should be noted that in the present invention, when the viscosity is to be within the above range, it can be achieved by making the blending amount of the (C) component within the above specified range.

[0147] In the composition of the present invention, the difference in viscosity between the first component and the second component is preferably small. They can be uniformly mixed using a static mixer such as a static mixer. The viscosity at 25° C. can be measured using a spiral viscometer. As a spiral viscometer, for example, a Malcom viscometer (model PC-10AA) can be used. At a rotation speed of 10 rpm, the initial (during preparation) viscosity difference between the first component and the second component is preferably ±0 to 80%, particularly ±0 to 50%, based on the viscosity of the first component.

[0148] In the composition of the present invention, the mixing ratio of the first component and the second component is preferably set to be substantially the same mass ratio. Specifically, the first component and the second component are preferably 1:0.5 to 1:2, more preferably 1:0.75 to 1:1.25, further preferably 1:0.9 to 1:1.1, and particularly preferably 1:0.95 to 1:1.05.

[0149] The thermal conductivity of the mixed composition of the first component and the second component before curing is preferably 0.1 W / m·K or more, more preferably 0.5 W / m·K or more in the hot plate method according to ISO 22007-2. If the thermal conductivity is too low, the heat dissipation performance of the heat-generating electronic component may become insufficient. It should be noted that there is no particular limitation on the upper limit of the thermal conductivity, and it can be set to less than 20.0 W / m·K or less than 15.0 W / m·K. It should be noted that in the present invention, when the thermal conductivity is to be within the above range, it can be achieved in particular by making the amount of component (C) within the above-specified range.

[0150] [Thermal conductive addition-curing silicone curing material]

[0151] The curing conditions of the composition of the present invention are not particularly limited, and can be the same as the curing conditions of the known addition reaction curing type silicone composition. For example, it can be fully cured even at room temperature, but can be heated as needed. In the case of curing at room temperature, the curing conditions at room temperature can be set to 0 to 40°C for 1 to 96 hours. It should be noted that the curing conditions when heated can be set to 70 to 200°C for 1 to 180 minutes.

[0152] The shape of the cured product is not particularly limited, but is preferably in the form of a sheet. The thickness of the sheet is preferably 0.1 to 10.0 mm. In addition, the cured product of the composition of the present invention preferably has a hardness of 10 to 90, more preferably 20 to 80, measured at 25°C using a Shore OO durometer as specified in ASTM D 2240-05. In addition, the hardness after aging at 150°C for 2000 hours is preferably 10 to 90, more preferably 20 to 80.

[0153] Example

[0154] The present invention is specifically described below by showing examples and comparative examples, but the present invention is not limited to the following examples. It should be noted that in the present invention, the order of siloxane bonding of the formula is not particularly limited.

[0155] [Example 1]

[0156] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 50 parts by mass of dimethylpolysiloxane having a molecular chain having both ends blocked with dimethylvinylsiloxy groups and a viscosity of 30,000 mm 2 / s, 40 parts by mass of dimethylpolysiloxane having a molecular chain end-capped with dimethylvinylsiloxy groups at both ends, 240 parts by mass of molten spherical alumina A having an average particle size of 43 μm as component (C), 160 parts by mass of crushed alumina B having an average particle size of 1.2 μm, and 5 parts by mass of n-decyltrimethoxysilane as component (F) were mixed, heated at 70°C for 1 hour, and then heated at 150°C for 1 hour.

[0157] Next, after the heat-treated mixture is fully cooled to room temperature (25°C), 0.25 parts by weight of a vinyl siloxane complex of chloroplatinic acid (Pt content 1% by weight) as component (E) is uniformly mixed at room temperature (25°C) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (first component).

[0158] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 50 parts by mass of dimethylpolysiloxane having a molecular chain having both ends blocked with dimethylvinylsiloxy groups and a viscosity of 30,000 mm 2 / s, 30 parts by mass of dimethylpolysiloxane having molecular chain ends blocked with dimethylvinylsiloxy groups, 5.2 parts by mass of methylhydrogen-dimethylpolysiloxane having dimethylhydrogensiloxy groups blocked with dimethylhydrogensiloxy groups as the component (B) (the total Si-Vi groups in the dimethylpolysiloxane having molecular chain ends blocked with dimethylvinylsiloxy groups in the component (A) in the entire composition when the first component and the second component are mixed at a mass ratio of 1:1 = 0.41), 240 parts by mass of molten spherical alumina A having an average particle size of 43 μm as the component (C), and crushed alumina B having an average particle size of 1.2 μm. 160 parts by mass of bis(8-hydroxyquinoline)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) represented by the general formula (D1) as the component (D), and 5 parts by mass of n-decyltrimethoxysilane as the component (F) were mixed, heated at 70°C for 1 hour, and then heated at 150°C for 1 hour.

[0159] Next, after the heat-treated mixture was sufficiently cooled to room temperature (25° C.), 0.03 parts by mass of ethynyldecylmethylcarbinol was uniformly mixed at room temperature (25° C.) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (second component).

[0160] [Chemistry 6]

[0161]

[0162] [Chemistry 7]

[0163]

[0164] [Comparative Example 1]

[0165] A thermally conductive addition-curable silicone composition (first component / second component) was obtained in the same manner except that (D) bis(8-quinolinol)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) was not added to the second component described in Example 1.

[0166] [Example 2]

[0167] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 50 parts by mass of dimethylpolysiloxane having a molecular chain having both ends blocked with dimethylvinylsiloxy groups and a viscosity of 30,000 mm 240 parts by mass of dimethylpolysiloxane having a molecular chain having both ends terminated with dimethylvinylsiloxy groups, 480 parts by mass of molten spherical alumina A having an average particle size of 43 μm as component (C), and 320 parts by mass of crushed alumina B having an average particle size of 1.2 μm were mixed and heated at 150° C. for 1 hour.

[0168] Next, after the heat-treated mixture is fully cooled to room temperature (25°C), 0.25 parts by weight of a vinyl siloxane complex of chloroplatinic acid (Pt content 1% by weight) as component (E) is uniformly mixed at room temperature (25°C) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (first component).

[0169] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 50 parts by mass of dimethylpolysiloxane having a molecular chain having both ends blocked with dimethylvinylsiloxy groups and a viscosity of 30,000 mm 2 / s, 30 parts by mass of dimethylpolysiloxane having molecular chain ends blocked with dimethylvinylsiloxy groups, 6.2 parts by mass of methylhydrogen-dimethylpolysiloxane represented by the general formula (B1) as the component (B) (the total Si-Vi groups in the dimethylpolysiloxane having molecular chain ends blocked with dimethylvinylsiloxy groups in the component (A) in the entire composition when the first component and the second component are mixed at a mass ratio of 1:1 = 0.49), 480 parts by mass of molten spherical alumina A having an average particle size of 43 μm as the component (C), 320 parts by mass of crushed alumina B having an average particle size of 1.2 μm, and 0.5 parts by mass of bis(8-quinolinolate)copper(II) represented by the general formula (D1) (manufactured by Tokyo Chemical Industry Co., Ltd.) as the component (D) were mixed and heated at 150° C. for 1 hour.

[0170] Next, after the heat-treated mixture was sufficiently cooled to room temperature (25° C.), 0.03 parts by mass of ethynyldecylmethylcarbinol was uniformly mixed at room temperature (25° C.) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (second component).

[0171] [Comparative Example 2]

[0172] A thermally conductive addition-curable silicone composition (first component / second component) was obtained in the same manner except that (D) bis(8-quinolinol)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) was not added to the second component described in Example 2.

[0173] [Example 3]

[0174] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 50 parts by mass of dimethylpolysiloxane having a molecular chain having both ends blocked with dimethylvinylsiloxy groups and a viscosity of 30,000 mm 2 / s, 40 parts by mass of dimethylpolysiloxane having a molecular chain end-capped with dimethylvinylsiloxy groups at both ends, 480 parts by mass of molten spherical alumina A having an average particle size of 43 μm as component (C), 320 parts by mass of crushed alumina B having an average particle size of 1.2 μm, and 5 parts by mass of n-decyltrimethoxysilane as component (F) were mixed, heated at 70°C for 1 hour, and then heated at 150°C for 1 hour.

[0175] Next, after the heat-treated mixture is fully cooled to room temperature (25°C), 0.25 parts by weight of a vinyl siloxane complex of chloroplatinic acid (Pt content 1% by weight) as component (E) is uniformly mixed at room temperature (25°C) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (first component).

[0176] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 50 parts by mass of dimethylpolysiloxane having a molecular chain having both ends blocked with dimethylvinylsiloxy groups and a viscosity of 30,000 mm 2 / s, 30 parts by mass of dimethylpolysiloxane having molecular chain ends terminated by dimethylvinylsiloxy groups, 6.2 parts by mass of methylhydrogen-dimethylpolysiloxane terminated by dimethylhydrogensiloxy groups represented by the general formula (B1) as the component (B) (the total Si-Vi groups in the dimethylpolysiloxane having molecular chain ends terminated by dimethylvinylsiloxy groups in the component (A) in the entire composition when the first component and the second component are mixed at a mass ratio of 1:1 = 0.49), 480 parts by mass of molten spherical alumina A having an average particle size of 43 μm as the component (C), and crushed alumina B having an average particle size of 1.2 μm. 320 parts by mass of bis(8-hydroxyquinoline)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) represented by the general formula (D1) as the component (D), and 5 parts by mass of n-decyltrimethoxysilane as the component (F) were mixed, heated at 70°C for 1 hour, and then heated at 150°C for 1 hour.

[0177] Next, after the heat-treated mixture was sufficiently cooled to room temperature (25° C.), 0.03 parts by mass of ethynyldecylmethylcarbinol was uniformly mixed at room temperature (25° C.) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (second component).

[0178] [Example 4]

[0179] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 50 parts by mass of dimethylpolysiloxane having a molecular chain having both ends blocked with dimethylvinylsiloxy groups and a viscosity of 30,000 mm 2 / s, 40 parts by mass of dimethylpolysiloxane having a molecular chain having both ends terminated by dimethylvinylsiloxy groups, 480 parts by mass of molten spherical alumina A having an average particle size of 43 μm as component (C), 320 parts by mass of crushed alumina B having an average particle size of 1.2 μm, 5 parts by mass of n-decyltrimethoxysilane as component (F), and 0.5 parts by mass of bis(8-hydroxyquinoline)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) represented by the general formula (D1) as component (D) were mixed, heated at 70°C for 1 hour, and then heated at 150°C for 1 hour.

[0180] Next, after the heat-treated mixture is fully cooled to room temperature (25°C), 0.25 parts by weight of a vinyl siloxane complex of chloroplatinic acid (Pt content 1% by weight) as component (E) is uniformly mixed at room temperature (25°C) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (first component).

[0181] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 50 parts by mass of dimethylpolysiloxane having a molecular chain having both ends blocked with dimethylvinylsiloxy groups and a viscosity of 30,000 mm 2 / s, 30 parts by mass of dimethylpolysiloxane having molecular chain ends blocked with dimethylvinylsiloxy groups, 6.2 parts by mass of methylhydrogen-dimethylpolysiloxane represented by the general formula (B1) as the component (B) (the total Si-Vi groups in the dimethylpolysiloxane having molecular chain ends blocked with dimethylvinylsiloxy groups in the component (A) in the entire composition when the first component and the second component are mixed at a mass ratio of 1:1 = 0.49), 480 parts by mass of molten spherical alumina A having an average particle size of 43 μm as the component (C), 320 parts by mass of crushed alumina B having an average particle size of 1.2 μm, and 5 parts by mass of n-decyltrimethoxysilane as the component (F) were mixed, heated at 70°C for 1 hour, and then heated at 150°C for 1 hour.

[0182] Next, after the heat-treated mixture was sufficiently cooled to room temperature (25° C.), 0.03 parts by mass of ethynyldecylmethylcarbinol was uniformly mixed at room temperature (25° C.) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (second component).

[0183] [Example 5]

[0184] A thermally conductive addition-curable silicone composition (first component / second component) was obtained in the same manner as in Example 3 except that the amount of (D) bis(8-quinolinol)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) in the second component was changed to 5 parts by mass.

[0185] [Example 6]

[0186] A thermally conductive addition-curable silicone composition (first component / second component) was obtained in the same manner except that (D) bis(8-quinolinol)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) in the second component described in Example 3 was replaced with 0.5 parts by mass of tris(8-quinolinol)aluminum(III) (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0187] [Example 7]

[0188] A thermally conductive addition-curable silicone composition (first component / second component) was obtained in the same manner except that 0.5 parts by mass of bis(8-quinolinolato)zinc(II) hydrate (manufactured by Tokyo Chemical Industry Co., Ltd.) was used as the (D) bis(8-quinolinolato)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) in the second component described in Example 3.

[0189] [Comparative Example 3]

[0190] A thermally conductive addition-curable silicone composition (first component / second component) was obtained in the same manner except that (D) bis(8-quinolinol)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) was not added in the second component described in Example 3.

[0191] [Comparative Example 4]

[0192] A thermally conductive addition-curable silicone composition (first component / second component) was obtained in the same manner except that (D) bis(8-hydroxyquinoline)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) in the second component described in Example 3 was replaced by 0.41 parts by mass of 8-hydroxyquinoline (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0193] [Example 8]

[0194] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 50 parts by mass of dimethylpolysiloxane having a molecular chain having both ends blocked with dimethylvinylsiloxy groups and a viscosity of 30,000 mm 2 / s, 40 parts by mass of dimethylpolysiloxane having a molecular chain end-capped with dimethylvinylsiloxy groups, 510 parts by mass of molten spherical alumina A having an average particle size of 43 μm as component (C), 340 parts by mass of crushed alumina B having an average particle size of 1.2 μm, and 15 parts by mass of an organic polysiloxane represented by the general formula (G1) and having a viscosity of 30 mPa·s at 25°C as component (G) were mixed, and the mixture was heated at 150°C for 1 hour.

[0195] Next, after the heat-treated mixture is fully cooled to room temperature (25°C), 0.25 parts by weight of a vinyl siloxane complex of chloroplatinic acid (Pt content 1% by weight) as component (E) is uniformly mixed at room temperature (25°C) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (first component).

[0196] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 50 parts by mass of dimethylpolysiloxane having a molecular chain having both ends blocked with dimethylvinylsiloxy groups and a viscosity of 30,000 mm 2 / s, 30 parts by mass of dimethylpolysiloxane having molecular chain ends blocked with dimethylvinylsiloxy groups, 6.2 parts by mass of methylhydrogen-dimethylpolysiloxane having dimethylhydrogensiloxy groups blocked with dimethylhydrogensiloxy groups as the component (B) (the total Si-Vi groups in the dimethylpolysiloxane having molecular chain ends blocked with dimethylvinylsiloxy groups in the component (A) in the entire composition when the first component and the second component are mixed at a mass ratio of 1:1 = 0.49), 510 parts by mass of molten spherical alumina A having an average particle size of 43 μm as the component (C), and crushed alumina B having an average particle size of 1.2 μm. 340 parts by mass of bis(8-hydroxyquinoline)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) represented by the general formula (D1) as the component (D), and 15 parts by mass of an organopolysiloxane represented by the general formula (G1) and having a viscosity of 30 mPa·s at 25° C. as the component (G) were mixed, and the mixture was heated at 150° C. for 1 hour.

[0197] Next, after the heat-treated mixture was sufficiently cooled to room temperature (25° C.), 0.03 parts by mass of ethynyldecylmethylcarbinol was uniformly mixed at room temperature (25° C.) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (second component).

[0198] [Chemistry 8]

[0199]

[0200] [Comparative Example 5]

[0201] A thermally conductive addition-curable silicone composition (first component / second component) was obtained in the same manner except that (D) bis(8-quinolinol)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) was not added in the second component described in Example 8.

[0202] [Example 9]

[0203] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 / s, 66 parts by mass of dimethylpolysiloxane having a molecular chain end-capped with dimethylvinylsiloxy groups at both ends, 480 parts by mass of molten spherical alumina A having an average particle size of 43 μm as component (C), 320 parts by mass of crushed alumina B having an average particle size of 1.2 μm, and 5 parts by mass of n-decyltrimethoxysilane as component (F) were mixed, heated at 70°C for 1 hour, and then heated at 150°C for 1 hour.

[0204] Next, after the heat-treated mixture is fully cooled to room temperature (25°C), 0.25 parts by weight of a vinyl siloxane complex of chloroplatinic acid (Pt content 1% by weight) as component (E) is uniformly mixed at room temperature (25°C) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (first component).

[0205] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 / s, 57 parts by mass of dimethylpolysiloxane having molecular chain ends blocked with dimethylvinylsiloxy groups, 5.6 parts by mass of methylhydrogen-dimethylpolysiloxane having dimethylhydrogensiloxy groups blocked with dimethylhydrogensiloxy groups as the component (B) (the total SiVi groups in the dimethylpolysiloxane having molecular chain ends blocked with dimethylvinylsiloxy groups in the component (A) in the entire composition when the first component and the second component are mixed at a ratio of 1:1 = 0.43), 480 parts by mass of molten spherical alumina A having an average particle size of 43 μm as the component (C), and crushed alumina B having an average particle size of 1.2 μm. 320 parts by mass of bis(8-hydroxyquinoline)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) represented by the general formula (D1) as the component (D), and 5 parts by mass of n-decyltrimethoxysilane as the component (F) were mixed, heated at 70°C for 1 hour, and then heated at 150°C for 1 hour.

[0206] Next, after the heat-treated mixture was sufficiently cooled to room temperature (25° C.), 0.03 parts by mass of ethynyldecylmethylcarbinol was uniformly mixed at room temperature (25° C.) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (second component).

[0207] [Comparative Example 6]

[0208] A thermally conductive addition-curable silicone composition (first component / second component) was obtained in the same manner except that (D) bis(8-quinolinol)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) was not added in the second component described in Example 9.

[0209] [Comparative Example 7]

[0210] A thermally conductive addition-curable silicone composition (first component / second component) was obtained in the same manner as in Example 9 except that 0.7 parts by mass of copper (II) phthalocyanine (Tokyo Chemical Industry Co., Ltd.) was used instead of bis(8-quinolinolato)copper(II) (Tokyo Chemical Industry Co., Ltd.).

[0211] [Comparative Example 8]

[0212] A thermally conductive addition-curable silicone composition (first component / second component) was obtained in the same manner as in Example 9 except that bis(8-quinolinol)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) in the second component was replaced with 1 part by mass of ferric oxide.

[0213] [Example 10]

[0214] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 / s, 66 parts by mass of dimethylpolysiloxane having a molecular chain having both ends terminated by dimethylvinylsiloxy groups, 660 parts by mass of crushed aluminum nitride C having an average particle size of 64 μm as component (C), 180 parts by mass of crushed aluminum oxide B having an average particle size of 1.2 μm, and 5 parts by mass of n-decyltrimethoxysilane as component (F) were mixed, heated at 70°C for 1 hour, and then heated at 150°C for 1 hour.

[0215] Next, after the heat-treated mixture is fully cooled to room temperature (25°C), 0.25 parts by weight of a vinyl siloxane complex of chloroplatinic acid (Pt content 1% by weight) as component (E) is uniformly mixed at room temperature (25°C) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (first component).

[0216] A 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. was added as the component (A) with a viscosity of 600 mm 2 / s, 57 parts by mass of dimethylpolysiloxane having molecular chain ends blocked with dimethylvinylsiloxy groups, 5.6 parts by mass of methylhydrogen-dimethylpolysiloxane having dimethylhydrogensiloxy groups blocked with dimethylhydrogensiloxy groups as the component (B) (the total Si-Vi groups in the dimethylpolysiloxane having molecular chain ends blocked with dimethylvinylsiloxy groups in the component (A) in the entire composition when the first component and the second component are mixed at a mass ratio of 1:1 = 0.43), 660 parts by mass of crushed aluminum nitride C having an average particle size of 64 μm as the component (C), and crushed aluminum oxide B having an average particle size of 1.2 μm. 180 parts by mass of bis(8-hydroxyquinoline)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) represented by the general formula (D1) as the component (D) and 5 parts by mass of n-decyltrimethoxysilane as the component (F) were mixed, heated at 70°C for 1 hour and then heated at 150°C for 1 hour.

[0217] Next, after the heat-treated mixture was sufficiently cooled to room temperature (25° C.), 0.03 parts by mass of ethynyldecylmethylcarbinol was uniformly mixed at room temperature (25° C.) for 20 minutes to obtain a thermally conductive addition-curable silicone composition (second component).

[0218] [Comparative Example 9]

[0219] A thermally conductive addition-curable silicone composition (first component / second component) was obtained in the same manner except that (D) bis(8-quinolinol)copper(II) (manufactured by Tokyo Chemical Industry Co., Ltd.) in the second component described in Example 10 was not added.

[0220] The viscosity of the component (A) described in the above examples and comparative examples is the kinematic viscosity at 25° C. measured using an Ostwald viscometer, and the average particle size of the component (C) is the volume average particle size (cumulative average diameter D) measured by laser diffraction. 50 (median diameter)). The viscosity of the thermally conductive addition-curing silicone compositions 1 (first component / second component) to 19 (first component / second component) was measured at 25°C using a spiral viscometer: Malcom viscometer (model PC-10AA, rotation speed 10 rpm). For thermal conductivity, the thermal conductivity of the silicone composition before curing at 25°C was measured using a hot plate method thermal property measuring device TPS 2500S manufactured by Kyoto Electronics Co., Ltd. (according to the hot plate method of ISO22007-2).

[0221] As a composition obtained by combining the first component and the second component, only the components (C), (D), (F), and (G) are described in the table.

[0222] C1: The thermal conductivity of the thermally conductive addition-curable silicone composition of each example and comparative example is 1.0 W / m·°C

[0223] C2: The thermal conductivity of the thermally conductive addition-curable silicone composition of each example and comparative example is 2.5 W / m·°C

[0224] C3: The thermal conductivity of the thermally conductive addition-curable silicone composition of each example and comparative example is 3.5 W / m·°C

[0225] C4: The thermal conductivity of the thermally conductive addition-curable silicone composition of each example and comparative example is 5.0 W / m·°C

[0226] D1: Bis(8-hydroxyquinoline)copper(II)

[0227] D2: Tris(8-hydroxyquinoline)aluminum(III)

[0228] D3: Bis(8-hydroxyquinoline)zinc(II) hydrate

[0229] D4 Comparative product: 8-Hydroxyquinoline

[0230] D5 Comparative product: Copper phthalocyanine (II)

[0231] D6 Comparative product: Ferrous oxide

[0232] F1: n-decyltrimethoxysilane

[0233] G1: an organopolysiloxane represented by the general formula (G1) and having a viscosity of 30 mPa·s at 25°C

[0234] For the thermally conductive addition-curable silicone composition, the first component and the second component of each composition were uniformly mixed at a mass ratio of 1:1 at room temperature (25°C) using a static mixer (MXA6.3-21) manufactured by NORITAKE COMPANY LIMITED, and then fully vacuum-degassed and poured into a molding die with a cured thickness of 6 mm. The cured product was cured at 25°C for 24 hours to obtain a sheet-like cured product, and its hardness (hardness) was measured using a Shore OO durometer specified in ASTM D 2240-05. Then, the sheet-like cured products from the thermally conductive addition-curable silicone compositions 1 to 19 were aged at 150°C for 2000 hours, and the hardness was measured every 500 hours using a Shore OO durometer specified in ASTM D 2240-05. The results of the above-mentioned viscosity, thermal conductivity, initial hardness, and hardness after aging are shown in Tables 1 to 5.

[0235] [Table 1]

[0236]

[0237] [Table 2]

[0238]

[0239] [Table 3]

[0240]

[0241] [Table 4]

[0242]

[0243] [Table 5]

[0244]

[0245] From the above results, the compositions of Examples 1 to 10 of the present invention showed a small increase in hardness after being stored at 150°C for 2000 hours, while the compositions of Comparative Examples 1 to 3 and 5 to 9 showed a significant increase in hardness after being stored at 150°C for 2000 hours. From Examples 2 and 3, it can be seen that even if the filler is not treated with an organosilane, the effect of suppressing the increase in hardness is obtained by adding the component (D). In addition, from Examples 3 and 4, it can be seen that the effect of suppressing the increase in hardness is obtained as long as the component (D) is added to any one of the first component and the second component. From Examples 3, 6 and 7, it can be seen that the central metal of the complex that can suppress the increase in hardness is not limited to copper. From Example 8, it can be seen that even if the filler is treated with an organopolysiloxane, the effect of suppressing the increase in hardness is obtained by adding the component (D). From the results of the Examples and Comparative Examples, it can be seen that the increase in hardness is suppressed by using the component (D) of the present invention. Therefore, according to the present invention, a thermally conductive silicone composition and a cured product thereof that can suppress the increase in hardness from the initial hardness when aged at 150°C are obtained.

[0246] Industrial Applicability

[0247] The thermally conductive silicone cured product obtained by curing the thermally conductive silicone composition according to the present invention, in which the hardness increase from the initial hardness during high-temperature aging is suppressed, can maintain the initial hardness even if it is subjected to heat generated by electronic components during installation for a long period of time. Therefore, it is expected to improve reliability in the use of heat dissipation and protection of electronic components such as power devices, transistors, thyristors, CPUs (central processing units), etc.

Claims

1. A two-component thermally conductive addition-curing silicone composition, which is a two-component thermally conductive addition-curing silicone composition consisting of a first component and a second component, wherein the first component contains: (A) an organopolysiloxane having at least two alkenyl groups bonded to silicon atoms in one molecule, (C) thermally conductive filler material, and (E) platinum group metal catalysts, The second component contains: (A) an organopolysiloxane having at least two alkenyl groups bonded to silicon atoms in one molecule, (B) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in one molecule, and (C) Thermally conductive filling materials, The first component does not contain the component (B), the second component does not contain the component (E), and either or both of the first component and the second component contain a complex of a metal and 8-hydroxyquinoline (D). The amount of the silicone composition is such that the number of hydrogen atoms bonded to silicon atoms in the component (B) is 0.1 to 5.0 per alkenyl group in the component (A) in the entire composition obtained by combining the first component and the second component.

2. The two-component thermally conductive addition-curable silicone composition according to claim 1, further comprising (F) an organosilane represented by the following general formula (1), R 1 a R 2 b Si(OR 3 ) 4-a-b (1) In the formula, R 1 are independently a monovalent hydrocarbon group having 4 to 20 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups having 4 to 20 carbon atoms, R 3 are independently monovalent hydrocarbon groups having 1 to 6 carbon atoms, a is an integer of 1 to 3, b is an integer of 0 to 2, wherein, a+b is an integer from 1 to 3.

3. The two-component thermally conductive addition-curable silicone composition according to claim 1, further comprising (G) an organopolysiloxane represented by the following general formula (2): [Chemistry 1] In the formula, R 4 are independently monovalent hydrocarbon groups, R 5 are independently alkyl, alkoxyalkyl, alkenyl or acyl, c is an integer of 5-100, and d is an integer of 1-3.

4. The two-component thermally conductive addition-curable silicone composition according to claim 1, wherein: The amount of component (C) in each of the first component and the second component is 300 to 3000 parts by mass per 100 parts by mass of the total of components (A) and (B). The amount of the component (D) is 0.001 to 5.0% by mass of the entire composition obtained by combining the first component and the second component. The amount of the component (E) is 0.1 to 500 ppm in terms of mass of the platinum group metal relative to the total of the components (A) and (B) in the entire composition obtained by combining the first component and the second component.

5. A two-component thermally conductive addition-curing silicone cured product, which is a cured product of the silicone composition according to any one of claims 1 to 4. 6 . The two-component thermally conductive addition-curing silicone cured material according to claim 5 , which is in the form of a sheet.

Citation Information

Patent Citations

  • Heat-resistant heat-conductive silicone composition

    JP2018123200A