Curable composition and application thereof

By adding operating oil and silica sand to organic polymers with hydrolyzable silyl groups, combined with silane compounds, the problems of bad odor during use and insufficient adhesion after alkali treatment of epoxy resin are solved, and excellent curability is prepared Compositions suitable for alkali-resistant applications and support sustainability goals.

CN118804953APending Publication Date: 2024-10-18KANEKA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380022685.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-22
Filing Date
2023-02-07
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing curable compositions have bad odor problems when using epoxy resin, and have insufficient adhesion after alkali treatment, making it difficult to meet alkali resistance requirements.

Method used

By adding specific amounts of process oil, silica sand and silane compounds to an organic polymer with a hydrolyzable silyl group, a curable composition without using epoxy resin is prepared to improve operability and adhesion after alkali treatment.

Benefits of technology

An epoxy resin-free curable composition is achieved, which has good operability and high adhesion after alkali treatment, is suitable for alkali-resistant applications, and supports the realization of sustainable development goals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005000907040000311
    Figure BDA0005000907040000311
  • Figure BDA0005000907040000321
    Figure BDA0005000907040000321
Patent Text Reader

Abstract

The purpose of the present invention is to provide a curable composition which does not use an epoxy resin, has good workability, and has excellent adhesiveness after alkali treatment. The present invention provides a composition containing (A) 100 parts by weight of an organic polymer having a hydrolyzable silyl group, (B) 3-35 parts by weight of at least one selected from the group consisting of paraffin-based process oils, cycloparaffin-based process oils and aromatic process oils, (C) 20-200 parts by weight of silica sand, and (D) a silane compound having an epoxy group and / or a silane compound 2-having an amino group. And 10 parts by weight of a curable composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a curable composition, and a cured product thereof, an adhesive, and a laminate. Background Art

[0002] Conventionally, curable compositions containing an organic polymer having a hydrolyzable silyl group have been used in tile adhesives and the like, and are required to have alkali resistance. Conventionally, alkali resistance has been imparted to such curable compositions by blending an epoxy resin in the above curable compositions.

[0003] For example, Patent Document 1 discloses a two-component curable resin composition, which contains a specific amount of epoxy resin as liquid A and a specific amount of tertiary amine as liquid B, and either or both of the liquid A and liquid B contain an organic polymer containing a crosslinkable silicon group, a filler, a diluent, a silane coupling agent, and a catalyst.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2019-183090 Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, in the above-mentioned technology, there is still room for improvement mainly from the viewpoint of the bad smell accompanying the use of the amine curing agent for epoxy resin. In addition, when used as an adhesive or the like, workability is also required.

[0009] Therefore, an object of the present invention is to provide a curable composition which does not use an epoxy resin, has good workability, and has excellent adhesion after an alkali treatment.

[0010] Solution to the problem

[0011] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found for the first time that, by respectively adding specific amounts of a specific process oil, silica sand, and a specific silane compound to a curable composition containing an organic polymer having a hydrolyzable silyl group, bad odor can be suppressed, workability can be improved, and adhesion after alkali treatment can be excellent, thereby completing the present invention.

[0012] Therefore, one embodiment of the present invention is a curable composition (hereinafter referred to as “the present curable composition”) comprising:

[0013] (A) 100 parts by weight of an organic polymer having a hydrolyzable silyl group;

[0014] (B) 3 to 35 parts by weight of at least one selected from paraffinic process oil, cycloparaffinic process oil and aromatic process oil;

[0015] (C) 20 to 200 parts by weight of silica sand; and

[0016] (D) 2 to 10 parts by weight of a silane compound having an epoxy group and / or a silane compound having an amino group.

[0017] Effects of the Invention

[0018] According to one embodiment of the present invention, a curable composition can be provided which does not use an epoxy resin, has good workability, and has excellent adhesiveness even after an alkali treatment. DETAILED DESCRIPTION

[0019] Hereinafter, one embodiment of the present invention will be described in detail. It should be noted that, in this specification, unless otherwise specified, "A to B" indicating a numerical range means "A or more and B or less". In addition, all the contents of the documents described in this specification are cited in this specification as references.

[0020] [1. Summary of the Invention]

[0021] Curable compositions using organic polymers having hydrolyzable silyl groups (e.g., adhesives for exterior tiles) currently meet the alkali-resistant warm water adhesion test by being used in combination with epoxy resins. However, tertiary amines used as curing agents for epoxy resins, ketimines in the case of single-component types, etc., have an amine odor, and therefore, the occasions in which they can be used are limited, resulting in a problem of difficulty in indoor use.

[0022] Therefore, the present inventors have conducted intensive research on a curable composition containing an organic polymer having a hydrolyzable silyl group, which does not use an epoxy resin, reduces bad odor, and imparts alkali resistance. As a result, they have found for the first time that by adding a specific process oil and a specific silane compound to the curable composition, a curable composition having excellent adhesion even after alkali treatment can be obtained. In addition, the present inventors have also found for the first time that by further adding silica sand to the curable composition, workability is improved.

[0023] There has been no known technology that can solve the problem of bad odor, ensure good workability, and impart alkali resistance to curable compositions containing organic polymers having hydrolyzable silyl groups without using epoxy resins, but the present invention can exert extremely excellent effects. In particular, the addition of a specific process oil surprisingly improves the adhesion after alkali treatment.

[0024] As described above, according to one embodiment of the present invention, a curable composition containing an organic polymer having a hydrolyzable silyl group can be obtained, which solves the problem of bad odor, has good workability, and imparts alkali resistance. Therefore, it can contribute to the realization of the Sustainable Development Goals (SDGs), such as Goal 11 "Building sustainable cities and human settlements."

[0025] It should be noted that, in this specification, "having alkali resistance" means that when the alkali warm water immersion treatment is carried out by the method described in the Examples, the bonding strength is 0.40 N / mm 2 The cohesive failure rate is 50% or more. The structure of the curable composition will be described in detail below.

[0026] [2. Curable composition]

[0027] The curable composition comprises: (A) 100 parts by weight of an organic polymer having a hydrolyzable silyl group, (B) 3 to 35 parts by weight of at least one selected from paraffinic process oil, cycloparaffinic process oil and aromatic process oil, (C) 20 to 200 parts by weight of silica sand, and (D) 2 to 10 parts by weight of a silane compound having an epoxy group and / or a silane compound having an amino group.

[0028] Hereinafter, the “organic polymer having a hydrolyzable silyl group” may be referred to as the “organic polymer having a hydrolyzable silyl group (A)” or the “component (A)”, the “paraffinic process oil, cycloparaffinic process oil, and aromatic process oil” may be referred to as the “paraffinic process oil, cycloparaffinic process oil, and aromatic process oil (B)” or the “component (B)”, the “silica sand” may be referred to as the “silica sand (C)” or the “component (C)”, the “silane compound having an epoxy group and / or a silane compound having an amino group” may be referred to as the “silane compound having an epoxy group and / or a silane compound having an amino group (D)” or the “component (D)”, the “polyoxyalkylene polymer (A1) containing a hydrolyzable silyl group” may be referred to as the “component (A1)”, and the “(meth)acrylate copolymer (A2) containing a hydrolyzable silyl group” may be referred to as the “component (A2)”.

[0029] (2-1. Organic polymer having a hydrolyzable silyl group (A))

[0030] The curable composition comprises an organic polymer (A) having a hydrolyzable silyl group. In one embodiment of the present invention, the organic polymer (A) having a hydrolyzable silyl group is preferably a polyoxyalkylene polymer (A1) containing a hydrolyzable silyl group (hereinafter sometimes referred to as "component (A1)") and / or a (meth)acrylate copolymer (A2) containing a hydrolyzable silyl group (hereinafter sometimes referred to as "component (A2)").

[0031] In the present specification, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are values ​​converted to standard polystyrene measured by gel permeation chromatography (GPC).

[0032] As the molecular weight of the component (A), the terminal group concentration can be directly measured by titration analysis of the polymer precursor before the introduction of the hydrolyzable silyl group based on the principle of the hydroxyl value determination method of JIS K 1557 and the iodine value determination method specified in JIS K 0070, or it can be expressed as a terminal group-converted molecular weight determined by considering the structure of the polymer (depending on the branching degree of the polymerization initiator used). The terminal group-converted molecular weight of the polymer (A) can be converted into the terminal group-converted molecular weight by converting the number average molecular weight (Mn) obtained by general GPC measurement of the polymer precursor and the number average molecular weight (Mn) obtained by preparing a calibration curve of the terminal group-converted molecular weight and GPC of the polymer containing the hydrolyzable silyl group.

[0033] <Polyoxyalkylene polymer having a hydrolyzable silyl group (A1)>

[0034] The polyoxyalkylene polymer (A1) having a hydrolyzable silyl group is a compound in which the polymer part (also referred to as "main chain") is a polyoxyalkylene. The polyoxyalkylene polymer (A1) having a hydrolyzable silyl group forms a siloxane bond between molecules under specific conditions known to those skilled in the art to form a crosslinked product.

[0035] In one embodiment of the present invention, the lower limit of the number average molecular weight (Mn) of the component (A1) is preferably 500 or more, more preferably 1500 or more, further preferably 5000 or more, and most preferably 10000 or more. The upper limit of the number average molecular weight of the component (A1) is preferably 100000 or less, more preferably 50000 or less, and further preferably 40000 or less. From the viewpoint of ease of handling and adhesion, the number average molecular weight is preferably within the above range.

[0036] In one embodiment of the present invention, the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the component (A1) (Mw / Mn; molecular weight distribution) is preferably 1.6 or less, more preferably 1.5 or less, further preferably 1.4 or less, particularly preferably 1.3 or less, and even more particularly preferably 1.2 or less. From the viewpoint of ease of handling and adhesion, the molecular weight distribution is preferably within the above range.

[0037] [Hydrolyzable silyl group]

[0038] The structure of the hydrolyzable silyl group contained in the component (A1) is not particularly limited, and any hydrolyzable silyl group commonly used in the technical field may be used.

[0039] In one embodiment, the hydrolyzable silyl group of the component (A1) is represented by the following general formula (1). Two or more hydrolyzable silyl groups represented by the general formula (1) may be contained in one polymer molecule.

[0040] -Si(R 1 ) 3-a (X) a (1)

[0041] In the formula, R 1 represents a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms (in the case of a substituted hydrocarbon group, it may be substituted by a heteroatom-containing group). 1 When R 1 The structures of R 1 Examples of the group include an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, and an aralkyl group having 7 to 20 carbon atoms.

[0042] X represents a hydroxyl group or a hydrolyzable group. Examples of hydrolyzable groups include hydroxyl, halogen, alkoxy, acyloxy, ketoximate, amino, amide, acid amide, aminooxy, mercapto, alkenyloxy, etc. Among them, from the perspective of stable hydrolysis and easy handling, alkoxy groups such as methoxy and ethoxy are more preferred, methoxy and ethoxy are further preferred, and methoxy is particularly preferred.

[0043] a is 1, 2 or 3. As a, 2 or 3 is preferable, which can form a network structure by condensation and give a cured product.

[0044] Generally speaking, alkoxy groups with fewer carbon atoms have higher reactivity. That is, the reactivity decreases in the order of methoxy, ethoxy, and propoxy. By utilizing this property, the specific structure of the hydrolyzable silyl group can be appropriately determined according to the production method and application of the component (A1).

[0045] Specific examples of the hydrolyzable silyl group include a trimethoxysilyl group, a triethoxysilyl group, a triisopropoxysilyl group, a dimethoxymethylsilyl group, a diethoxymethylsilyl group, a diisopropoxymethylsilyl group, a (chloromethyl)dimethoxysilyl group, and a (methoxymethyl)dimethoxysilyl group.

[0046] From the perspective of the physical properties of the obtained cured product, the availability of the raw material compound, and the ease of handling, the hydrolyzable silyl group is preferably a dialkoxysilyl group or a trialkoxysilyl group. In addition, from the perspective of the excellent shape retention of the curable composition and during curing, a dialkoxysilyl group is preferred, and from the perspective of a fast crosslinking reaction rate, a trialkoxysilyl group is preferred.

[0047] The lower limit of the number of hydrolyzable silyl groups contained in one polymer molecule is preferably 0.5 or more, more preferably 1.0 or more, and further preferably 1.5 or more. The upper limit of the number of hydrolyzable silyl groups contained in one polymer molecule is preferably 5.0 or less, and more preferably 4.0 or less. If the number of hydrolyzable silyl groups is within the above range, the cured product obtained by the condensation reaction of the silyl group can obtain sufficient flexibility.

[0048] The distribution of the hydrolyzable silyl group may be random or block-like. The distribution position of the hydrolyzable silyl group may be at any position of the polymer molecule. Regarding the distribution position of the hydrolyzable silyl group, the preferred distribution position includes the end or near the end of the polymer molecule. The distribution position of the hydrolyzable silyl group is more preferably concentrated at the end or near the end of the polymer molecule. In one embodiment of the present invention, "near the end of the polymer molecule" refers to the region from each end of the polymer molecule to a specific position in the polymer molecule, and the weight of the region accounts for less than 20% by weight, less than 15% by weight, or less than 10% by weight of the total weight of the polymer molecule. In one embodiment of the present invention, "concentrated at the end or near the end of the polymer molecule" means that among the hydrolyzable silyl groups contained in the polymer molecule, the number located at the end or near the end accounts for more than 70%, more than 80%, or more than 90%.

[0049] As a method for introducing a hydrolyzable silyl group into a polyoxyalkylene polymer, a known method can be adopted.

[0050] [Polyoxyalkylene]

[0051] The polyoxyalkylene structure in the component (A1) may be linear or branched. The polyoxyalkylene structure is preferably a structure derived from polyoxypropylene diol or polyoxypropylene triol.

[0052] The polyoxyalkylene polymer molecule may be composed of only one type of repeating unit or may contain two or more types of repeating units. One type of polyoxyalkylene polymer may be blended or two or more types of polyoxyalkylene polymers may be blended.

[0053] Examples of the main chain structure of the polyoxyalkylene polymer include a structure having a repeating unit represented by the following general formula (2): 2 It is a divalent alkenyl group.

[0054] -R 2 -O-(2)

[0055] The structure represented by the general formula (2) preferably accounts for 50% by weight or more, more preferably 70% by weight or more, and even more preferably 90% by weight or more of the total weight of the polyoxyalkylene polymer in the component (A1).

[0056] R contained in the general formula (2) 2 The specific structure of R is not particularly limited. 2 It is preferably an alkenyl group having 1 to 14 carbon atoms, and more preferably a linear or branched alkenyl group having 2 to 4 carbon atoms.

[0057] Specific examples of the repeating unit represented by the general formula (2) include -CH2O-, -CH2CH2O-, -CH2CH(CH3)O-, -CH2CH(C2H5)O-, -CH2C(CH3)2O-, and -CH2CH2CH2CH2O-. Among them, -CH2CH(CH3)O- is preferred. The polyoxyalkylene polymer containing -CH2CH(CH3)O- in the repeating unit can easily adjust the glass transition temperature (Tg) to below 0°C.

[0058] The polyoxyalkylene polymer may contain a urethane bond or a urea bond in the main chain structure.

[0059] As the polyoxyalkylene polymer, commercial products may also be used. Examples of commercial products include Kaneka MS polymer (registered trademark) S810, S257, S327, S203H, S303H (all manufactured by Kaneka Co., Ltd.); SILYL (registered trademark) SAX220, SAT350, SAT400, SAX510, SAX520, SAX580, SAX590, SAX750 (all manufactured by Kaneka Co., Ltd.); EXCESTAR (registered trademark) ES-S2410, ES-S2420, ES-S3630 (all manufactured by AGC Co., Ltd.); GENIOSIL (registered trademark) STP-E10, STP-E15, STP-E-30, STP-E-35 (all manufactured by Wacker).

[0060] (Method for producing polyoxyalkylene polymer)

[0061] As a method for producing the polyoxyalkylene polymer (A1) having a hydrolyzable silyl group, the following methods (I) to (III) can be used.

[0062] (I) A method of polymerizing an epoxy compound using a composite metal cyanide complex catalyst in the presence of an initiator having a hydroxyl group, obtaining a hydroxyl-terminated polyoxyalkylene polymer based on this method, converting the hydroxyl group of the obtained hydroxyl-terminated polyoxyalkylene polymer into a carbon-carbon unsaturated group, and then adding a silane compound through a hydrosilylation reaction.

[0063] (II) A method in which an epoxy compound is polymerized using a composite metal cyanide complex catalyst in the presence of an initiator having a hydroxyl group to obtain a hydroxyl-terminated polyoxyalkylene polymer based on this method, and then the obtained hydroxyl-terminated polyoxyalkylene polymer is reacted with a compound containing both a group reactive with a hydroxyl group and a hydrolyzable silyl group.

[0064] (III) A method of reacting a hydroxyl-terminated polyoxyalkylene polymer with an excess of a polyisocyanate compound to obtain a polymer having an isocyanate group at the terminal, and then reacting the polymer with a compound containing both a group reactive with an isocyanate group and a hydrolyzable silyl group.

[0065] Examples of the initiator having a hydroxyl group used in methods (I) and (II) include substances having one or more hydroxyl groups, such as ethylene glycol, propylene glycol, glycerol, pentaerythritol, low molecular weight polypropylene glycol, polyoxypropylene triol, allyl alcohol, methanol, ethanol, propanol, butanol, pentanol, hexanol, polypropylene monoallyl ether, and polypropylene monoalkyl ether.

[0066] Examples of the epoxy compound used in the methods (I) and (II) include alkylene oxides such as ethylene oxide and propylene oxide, and glycidyl ethers such as methyl glycidyl ether and allyl glycidyl ether. Among them, propylene oxide is preferred.

[0067] Examples of the carbon-carbon unsaturated group used in the method (I) include vinyl, allyl, methallyl, propargyl, etc. Among them, allyl is preferred.

[0068] As a method for converting the hydroxyl group in (I) into a carbon-carbon unsaturated group, a method of allowing an alkali metal salt to act on a polymer having a hydroxyl terminal and then reacting it with a halogenated hydrocarbon compound having a carbon-carbon unsaturated bond is preferred.

[0069] Examples of the halogenated hydrocarbon compound used in the method (I) include vinyl chloride, allyl chloride, methylallyl chloride, propargyl chloride, vinyl bromide, allyl bromide, methylallyl bromide, propargyl bromide, vinyl iodide, allyl iodide, methylallyl iodide, propargyl iodide and the like.

[0070] As the hydrosilane compound used in the method (I), trimethoxysilane, triethoxysilane, tri(2-propyleneoxy)silane, triacetoxysilane, dimethoxymethylsilane, (chloromethyl)dimethoxysilane, (methoxymethyl)dimethoxysilane, (N,N-diethylaminomethyl)dimethoxysilane, etc. can be used.

[0071] (I) The hydrosilylation reaction used in the method can be accelerated by various catalysts. As a catalyst for hydroalkylation, a known catalyst can be used. For example, a substance containing platinum on a carrier such as alumina, silica, carbon black, chloroplatinic acid; a chloroplatinic acid complex composed of chloroplatinic acid and an alcohol, aldehyde, ketone, etc.; a platinum-olefin complex [such as Pt(CH2=CH2)2(PPh3), Pt(CH2=CH2)2Cl2]; a platinum-vinylsiloxane complex [Pt{(vinyl)Me2SiOSiMe2(vinyl)}, Pt{Me(vinyl)SiO}4]; a platinum-phosphine complex [Ph(PPh3)4, Pt(PBu3)4]; a platinum-phosphite complex [Pt{P(OPh)3}4], etc. can also be used.

[0072] As compounds containing both a group reactive with a hydroxyl group and a hydrolyzable silyl group that can be used in method (II), for example, isocyanate silanes such as 3-isocyanate propyl trimethoxy silane, 3-isocyanate propyl dimethoxy methyl silane, 3-isocyanate propyl triethoxy silane, isocyanate methyl trimethoxy silane, isocyanate methyl triethoxy silane, and isocyanate methyl dimethoxy methyl silane; mercapto silanes such as 3-mercaptopropyl trimethoxy silane, 3-mercaptopropyl dimethoxy methyl silane, and 3-mercaptopropyl triethoxy silane; epoxy silanes such as 3-glycidoxy propyl trimethoxy silane, 3-glycidoxy propyl dimethoxy methyl silane, and 3-glycidoxy propyl triethoxy silane, etc. can be used.

[0073] Examples of the polyisocyanate compound that can be used in the method (III) include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylene diisocyanate; and aliphatic polyisocyanates such as isophorone diisocyanate and hexamethylene diisocyanate.

[0074] Examples of the compound containing both a group reactive with an isocyanate group and a hydrolyzable silyl group that can be used in the method (III) include γ-aminopropyltrimethoxysilane, γ-aminopropyldimethoxymethylsilane, γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyldimethoxymethylsilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, γ-(N-phenyl)aminopropyltrimethoxysilane, and γ-(N-phenyl)aminopropyltrimethoxysilane. Silanes containing amino groups such as γ-(N-phenyl)aminopropyldimethoxymethylsilane, N-ethylaminoisobutyltrimethoxysilane, N-ethylaminoisobutyldimethoxymethylsilane, N-cyclohexylaminomethyltrimethoxysilane, and N-cyclohexylaminomethyldimethoxymethylsilane; silanes containing hydroxy groups such as γ-hydroxypropyltrimethoxysilane and γ-hydroxypropyldimethoxymethylsilane; silanes containing mercapto groups such as γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyldimethoxymethylsilane.

[0075] Furthermore, as the polyoxyalkylene polymer (A1) containing a hydrolyzable silyl group, a polyoxyalkylene polymer having a plurality of hydrolyzable silyl groups at one terminal may be used. Examples of the method for synthesizing a polyoxyalkylene polymer having a plurality of hydrolyzable silyl groups at one terminal include: (i) a method of obtaining a hydroxyl-terminated polyoxyalkylene polymer by polymerizing an epoxy compound in the presence of an initiator having a hydroxyl group using a composite metal cyanide complex catalyst; (ii) a method of reacting the hydroxyl group of the obtained hydroxyl-terminated polyoxyalkylene polymer with allyl glycidyl ether after allowing an alkali metal salt to act on the hydroxyl group of the obtained hydroxyl-terminated polyoxyalkylene polymer, and then reacting the polymer with an alkali metal salt on the generated hydroxyl group, and then reacting the polymer with a halogenated hydrocarbon compound having a carbon-carbon unsaturated bond to obtain a polyoxyalkylene polymer having a plurality of hydrolyzable silyl groups at one terminal; (iii) a method of adding a silane compound to the obtained polyoxyalkylene polymer having a plurality of hydrolyzable silyl groups at one terminal by a hydroalkylation reaction, or (iv) reacting the polymer with an epoxy compound having a hydrolyzable silyl group during or after the step (i).

[0076] <(Meth)acrylate copolymer having a hydrolyzable silyl group (A2)>

[0077] The (meth)acrylate copolymer (A2) having a hydrolyzable silyl group is a compound in which the polymer part of the polymer containing a hydrolyzable silyl group is a (meth)acrylate copolymer. The (meth)acrylate copolymer (A2) having a hydrolyzable silyl group forms a siloxane bond between molecules under specific conditions known to those skilled in the art to form a crosslinked body.

[0078] In one embodiment of the present invention, the lower limit of the number average molecular weight (Mn) of the component (A2) is preferably 500 or more, more preferably 1500 or more, further preferably 5000 or more, and most preferably 10000 or more. The upper limit of the number average molecular weight of the component (A2) is preferably 100000 or less, more preferably 50000 or less, and further preferably 45000 or less. From the viewpoint of ease of operation such as workability and adhesiveness, the number average molecular weight is preferably within the above range.

[0079] In one embodiment of the present invention, the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the component (A2) (Mw / Mn; molecular weight distribution) is preferably 1.6 or less, more preferably 1.5 or less, further preferably 1.4 or less, particularly preferably 1.3 or less, and even more particularly preferably 1.2 or less. From the viewpoint of ease of handling and adhesion, the molecular weight distribution is preferably within the above range.

[0080] [Hydrolyzable silyl group]

[0081] The hydrolyzable silyl group in the hydrolyzable silyl group-containing (meth)acrylic acid ester copolymer (A2) refers to the contents described in the section [Hydrolyzable silyl group] of the above-mentioned <Hydrolyzable silyl group-containing polyoxyalkylene polymer (A1)>.

[0082] [(Meth)acrylate]

[0083] (Meth)acrylate contains a structural unit derived from a (meth)acrylic acid-based monomer. In the present specification, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid.

[0084] The (meth)acrylate structure in the component (A2) may be linear or branched.

[0085] The (meth)acrylate ester molecule may be composed of only one type of repeating unit or may contain two or more types of repeating units. One type of (meth)acrylate ester may be blended or two or more types of (meth)acrylate ester may be blended.

[0086] Examples of the (meth)acrylate structure include the structure represented by the following general formula (3). 3 is a hydrogen atom or a methyl group, R 4 is a group having 1 or more carbon atoms. 4 The number of carbon atoms in R can be, for example, 1 to 22. 4 It can be an alkyl group, a cycloalkyl group or an aryl group. 4 It may be substituted by halogen, hydroxy, alkoxy, amino or the like.

[0087] -CH(R 3)-CH(COOR 4 )-(3)

[0088] The structure represented by the general formula (3) can be obtained by polymerization of (meth)acrylic acid monomers. Specific examples of (meth)acrylic acid monomers include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxyethyl (meth)acrylate, butyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, isopropoxyethyl (meth)acrylate, phenyl (meth)acrylate, toluene (meth)acrylate, benzyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, glycidyl (meth)acrylate, 1-ethylcyclopentyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, eicosyl (meth)acrylate, behenyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, oleyl (meth)acrylate, linoleyl (meth)acrylate, isobornyl (meth)acrylate, 2-aminoethyl (meth)acrylate, γ-(methacryloyloxypropyl) trimethoxy Silane, ethylene oxide adduct of (meth)acrylic acid, trifluoromethyl methyl (meth)acrylate, 2-trifluoromethyl methyl (meth)acrylate, 2-perfluoroethyl ethyl (meth)acrylate, 2-perfluoroethyl-2-perfluorobutyl ethyl (meth)acrylate, 2-perfluoroethyl (meth)acrylate, perfluoromethyl (meth)acrylate, diperfluoromethyl methyl (meth)acrylate, 2-perfluoromethyl-2-perfluoroethyl methyl (meth)acrylate, 2-perfluorohexyl ethyl (meth)acrylate, 2-perfluorodecyl ethyl (meth)acrylate, 2-perfluorohexadecyl ethyl (meth)acrylate.

[0089] Among the above (meth)acrylic monomers, at least one selected from ethyl acrylate, n-propyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, and stearyl acrylate is preferred. The main chain structure composed of these monomers can easily adjust the glass transition temperature (Tg) to below 0°C.

[0090] As the (meth)acrylate, commercial products may be used. Examples of commercial products include XMAP (registered trademark) SA100S, SA110S, SA120S, SA310S, and SA410S (all manufactured by Kaneka Co., Ltd.); ARUFON (registered trademark) US-6100, US-6110, US-6120, US-6130, US-6140, US-6150, US-6170, US-6180, and US-6190 (all manufactured by Toagosei Co., Ltd.); ACTFLOW NE-1000 (registered trademark) (manufactured by Soken Chemical Co., Ltd.); and Joncryl (registered trademark) (manufactured by BASF).

[0091] In one embodiment of the present invention, it is preferred that the (meth)acrylate contains an XY double segment structure or an XYX three segment structure in the molecule. Here, the X segment refers to a segment with a relatively high content of hydrolyzable silyl groups. The Y segment refers to a segment with a relatively low content of hydrolyzable silyl groups. The overall structure of the (meth)acrylate molecule is not particularly limited as long as it contains an XY double segment structure or an XYX three segment structure. For example, it can also be an XYXY four segment structure. Here, the "XYX three segment structure" refers to what is generally referred to as an "ABA three segment" by those skilled in the art.

[0092] The number of repeating units derived from a hydrolyzable silyl group-containing monomer contained in segment X is more than 1.0 on average, preferably 1.5 or more, more preferably 1.7 or more. In addition, the number of repeating units derived from a hydrolyzable silyl group-containing monomer contained in segment X is preferably more than 3% by weight, more preferably 4.5% by weight or more, and further preferably 5% by weight or more, based on the weight of all repeating units contained in segment X.

[0093] In one embodiment of the present invention, the (meth)acrylate is a XYX three-segment polymer, and it is preferred that each of the segments (X segments) constituting the terminal portion of the (meth)acrylate has more than one hydrolyzable silane.

[0094] The repeating unit derived from the hydrolyzable silyl group-containing monomer contained in the Y segment is 0 to 3% by weight, preferably 0 to 2% by weight, more preferably 0 to 1% by weight, based on the weight of all repeating units contained in the Y segment.

[0095] In the (meth)acrylate containing an XY double-segment structure or an XYX triple-segment structure in the molecule, repeating units derived from a hydrolyzable silyl group-containing monomer are concentrated in a region near the terminal (near one or both ends).

[0096] (Method for producing (meth)acrylate)

[0097] (Meth)acrylates can be produced by known polymerization methods (radical polymerization, cationic polymerization, anionic polymerization, etc.).

[0098] As a preferred method for producing the hydrolyzable silyl group-containing (meth)acrylate copolymer (A2), the following methods (IV) to (VI) can be used.

[0099] (IV) A method of copolymerizing a compound containing a polymerizable unsaturated group and a hydrolyzable silyl group with a monomer containing a (meth)acrylic acid structure.

[0100] (V) A method of copolymerizing a monomer having a (meth)acrylic acid structure in the presence of a hydrolyzable silyl group and a mercapto group-containing compound as a chain transfer agent.

[0101] A combination of (IV) and (V) may be used to copolymerize a compound containing a polymerizable unsaturated group and a hydrolyzable silyl group with a monomer in the presence of a thiol having a hydrolyzable silyl group as a chain transfer agent.

[0102] (VI) A method of introducing a hydrolyzable silyl group at the terminal of a molecular chain after polymerizing a monomer having a (meth)acrylic acid structure by a living radical polymerization method.

[0103] The living polymerization method (VI) is preferred because it can introduce a functional group into the terminal of the polymer molecule and can synthesize a (meth)acrylate having a small molecular weight distribution.

[0104] Examples of the compound containing a polymerizable unsaturated group and a hydrolyzable silyl group used in (IV) include 3-(dimethoxymethylsilyl)propyl (meth)acrylate, (dimethoxymethylsilyl)methyl (meth)acrylate, (diethoxymethylsilyl)methyl (meth)acrylate, and 3-((methoxymethyl)dimethoxysilyl)propyl (meth)acrylate.

[0105] Examples of the compound having a hydrolyzable silyl group and a mercapto group used in (V) include 3-mercaptopropyldimethoxymethylsilane and (mercaptomethyl)dimethoxymethylsilane.

[0106] Examples of the living polymerization method (VI) include living radical polymerization, living cationic polymerization, and living anionic polymerization. Among them, living radical polymerization is suitable for the production of (meth)acrylates. Examples of the living radical polymerization method include the following.

[0107] Atom transfer radical polymerization (refer to Atom Transfer Radical Polymerization; ATRP (J. Am. Chem. Soc. 1995, 117, 5614; Macromolecules. 1995, 28, 1721))

[0108] Single electron transfer polymerization (refer to Sigle Electron Transfer Polymerization; SET-LRP (J.Am.Chem.Soc.2006,128,14156; JPS Chem2007,45,1607)

[0109] Reversible Chain Transfer Catalyzed Polymerization (RTCP ("Living Radical Polymerization Controlled by Organic Catalysts" Polymer Thesis Collection 68, 223-231 (2011); see Japanese Patent Application Laid-Open No. 2014-111798))

[0110] Reversible addition-fragmentation chain transfer polymerization (RAFT polymerization)

[0111] Nitro radical method (NMP method)

[0112] ·Polymerization method using organotellurium compounds (TERP method)

[0113] ·Polymerization method using organic antimony compounds (SBRP method)

[0114] ·Bismuth organic polymerization method (BIRP)

[0115] Iodine transfer polymerization

[0116] As a method for introducing a hydrolyzable silyl group in (meth)acrylate, the method described in Japanese Patent Publication No. 2007-302749 and the method described in Japanese Patent Publication No. 2018-162394 can be cited. The method described in Japanese Patent Publication No. 2007-302749 introduces a hydrolyzable silyl group by changing the terminal functional group of (meth)acrylate. Specifically, the hydrolyzable silyl group is introduced by changing the molecular end of (meth)acrylate in the order of hydroxyl, alkenyl, and hydrolyzable silyl. The method described in Japanese Patent Publication No. 2018-162394 is to introduce a hydrolyzable silyl group by copolymerization with a (meth)acrylate monomer containing a hydrolyzable silyl group. Specifically, the amount of (meth)acrylate monomer containing a hydrolyzable silyl group is controlled according to the stage of active polymerization, thereby introducing a hydrolyzable silyl group near the end of the (meth)acrylate molecule. The hydrolyzable silyl group-containing (meth)acrylate obtained by these methods has a hydrolyzable silyl group locally at a molecular terminal or near a terminal.

[0117] The upper limit of the glass transition temperature (Tg) of the (meth)acrylate in the component (A2) is preferably 100°C or lower, more preferably 50°C or lower, further preferably 0°C or lower, and most preferably -10°C or lower. The lower limit of the glass transition temperature (Tg) of the (meth)acrylate is not particularly limited, but is preferably -80°C or higher, more preferably -70°C or higher. The glass transition temperature of the (meth)acrylate can be substantially regarded as the glass transition temperature of the component (A2) itself.

[0118] In one embodiment of the present invention, component (A) may be used by mixing component (A1) of low viscosity and component (A2) of high viscosity. When component (A1) and component (A2) are used in combination, there is an advantage of further improving adhesion and improving operability compared to the case where each component is used alone.

[0119] The viscosity of the component (A1) at 23° C. is not particularly limited, but is preferably 1 to 100 Pa·s, more preferably 5 to 80 Pa·s, and even more preferably 10 to 70 Pa·s. This configuration provides an advantage of a low viscosity curable composition.

[0120] The viscosity of the component (A2) at 23°C is not particularly limited, but is preferably 6.0 Pa·s to 1000 Pa·s, more preferably 50 Pa·s to 750 Pa·s, and even more preferably 100 Pa·s to 500 Pa·s. This configuration has the advantage of improving the adhesiveness of the obtained curable composition and the tensile elongation of the cured product.

[0121] The weight ratio of component (A1) to component (A2) is preferably 5:95 to 50:50. Within this range, a cured product exhibiting flexibility and high shear bond strength can be obtained. Furthermore, from the perspective of achieving both high rigidity and flexibility, (A1): (A2) is preferably 100:0 to 50:50, and more preferably 100:0 to 70:30.

[0122] (2-2. (B) Component)

[0123] The curable composition contains at least one selected from the group consisting of paraffinic process oil, cycloparaffinic process oil and aromatic process oil (B). By including the component (B) in the curable composition, alkali resistance can be imparted.

[0124] Examples of paraffinic process oils include Diana Process Oil PW-32, PW-90, PW-380, PS-32, PS-90, PS-430, PA-32, and PA-90 (all manufactured by Idemitsu Kosan Co., Ltd.), VC CLEAN AN100, AN110, AN200, AN220, AN230, AN240, AN1013, AN1416, AI40, AI50, AI60, AI70, AI80, AI95, ISOPAR E, ISOPAR G, ISOPAR HBHT, ISOPAR L, and ISOPAR M (all manufactured by Andoh Parachemie Co., Ltd.), and SUNPAR 107, 110, 115, 150, 2100, and 2280 (all manufactured by Sun Oil Co., Ltd.). Liquid paraffin (manufactured by Fuji Wako Pure Chemical Industries, Ltd.) may also be used.

[0125] Examples of the cycloparaffin process oil include Diana Process Oil NP-24, NR-68, NS-90S, NS-100, and NM-280 (all manufactured by Idemitsu Kosan Co., Ltd.), EXXSOL D40, EXXSOL D80, EXXSOL D110, EXXSOL D130, EXXSOL DSP80 / 100, EXXSOL DSP100 / 140, and EXXSOL D145 / 160 (all manufactured by ANDOHPARACHEMIE Co., Ltd.), and SUNTHENE 410, 415, 450, 4130, 4240, and 250J (all manufactured by Japan Sun Oil Co., Ltd.).

[0126] Examples of the aromatic process oil include Diana Process Oil AC-12, AC-460, and AH-16 (all manufactured by Idemitsu Kosan Co., Ltd.), and JSO AROMA 790 (manufactured by Japan Sun Oil Co., Ltd.).

[0127] In one embodiment of the present invention, from the viewpoint of adhesive strength after alkali treatment, component (B) is preferably a cycloparaffinic process oil or an aromatic process oil, and among them, from the viewpoint of heat resistance, a cycloparaffinic process oil is preferred.

[0128] The content of the component (B) in the curable composition is 3 to 35 parts by weight, preferably 3.5 to 33 parts by weight, and more preferably 4 to 30 parts by weight relative to 100 parts by weight of the component (A). When the content of the component (B) is 3 to 35 parts by weight, the adhesiveness after alkali treatment is excellent.

[0129] (2-3. (C) Component)

[0130] The present curable composition contains silica sand (C). When the present curable composition contains the component (C), workability such as ease of coating is improved.

[0131] The average particle size of the component (C) is, for example, 10 to 800 μm, preferably 20 to 600 μm, more preferably 30 to 500 μm, and further preferably 40 to 400 μm. When the average particle size of the component (C) is 10 to 800 μm, the handling property is more excellent.

[0132] The content of the component (C) in the curable composition is 20 to 200 parts by weight, preferably 30 to 180 parts by weight, and more preferably 40 to 160 parts by weight based on 100 parts by weight of the component (A). When the content of the component (C) is 20 to 200 parts by weight, workability is improved.

[0133] (2-4. (D) Component)

[0134] The present curable composition contains a silane compound having an epoxy group and / or a silane compound having an amino group (D). When the present curable composition contains the component (D), the adhesiveness is improved.

[0135] The silane compound having an epoxy group (also referred to as "epoxysilane") is not particularly limited, and examples thereof include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltriethoxysilane, etc. Among them, γ-glycidoxypropyltrimethoxysilane is preferred from the viewpoint of adhesion.

[0136] The silane compound having an amino group (also referred to as "aminosilane") is not particularly limited, and examples thereof include γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropylmethyldiethoxysilane, γ-ureidopropyltrimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-benzyl-γ-aminopropyltrimethoxysilane, and N-vinylbenzyl-γ-aminopropyltriethoxysilane. Among them, from the viewpoint of adhesiveness, γ-aminopropyltrimethoxysilane and γ-(2-aminoethyl)aminopropyltrimethoxysilane are preferred, and γ-(2-aminoethyl)aminopropyltrimethoxysilane is particularly preferred.

[0137] In one embodiment of the present invention, from the viewpoint of water resistance, the component (D) is preferably a silane compound having an epoxy group.

[0138] The content of the component (D) in the curable composition is 2 to 10 parts by weight, preferably 2.2 to 9 parts by weight, and more preferably 2.4 to 8 parts by weight, based on 100 parts by weight of the component (A). When the content of the component (D) is 2 to 10 parts by weight, workability is improved.

[0139] (2-5. Other additives)

[0140] As other additives in addition to the above-mentioned components, the present curable composition may contain silanol condensation catalysts, tackifiers, plasticizers, solvents, diluents, fillers, anti-sagging agents, antioxidants, light stabilizers, ultraviolet absorbers, property adjusters, tackifying resins, epoxy group-containing compounds, photocurable substances, oxygen-curable substances, etc.

[0141] <Silanol condensation catalyst>

[0142] In the present curable composition, a silanol condensation catalyst may be used for the purpose of promoting the hydrolysis / condensation reaction of the hydrolyzable silyl group of the organic polymer (A) having a hydrolyzable silyl group and extending or crosslinking the polymer chain.

[0143] Examples of the silanol condensation catalyst include organic tin compounds, carboxylic acid metal salts, amine compounds, carboxylic acids, and metal alkoxides.

[0144] Specific examples of the organotin compound include dibutyltin dilaurate, dibutyltin dioctoate, dibutyltin di(butyl maleate), dibutyltin diacetate, dibutyltin oxide, dibutylbis(acetylacetonate)tin, dioctylbis(acetylacetonate)tin, dioctyltin dilaurate, dioctyltin distearate, dioctyltin diacetate, dioctyltin oxide, a reaction product of dibutyltin oxide and a silicate compound, a reaction product of dioctyltin oxide and a silicate compound, and a reaction product of dibutyltin oxide and a phthalate ester.

[0145] Specific examples of the carboxylic acid metal salt include tin carboxylate, bismuth carboxylate, titanium carboxylate, zirconium carboxylate, iron carboxylate, potassium carboxylate, calcium carboxylate, etc. As the carboxylic acid group, the following carboxylic acids can be combined with various metals.

[0146] Specific examples of amine compounds include: amines such as octylamine, 2-ethylhexylamine, laurylamine, and stearylamine; nitrogen-containing heterocyclic compounds such as pyridine, 1,8-diazabicyclo[5,4,0]undec-7-ene (DBU), and 1,5-diazabicyclo[4,3,0]non-5-ene (DBN); guanidines such as guanidine, phenylguanidine, and diphenylguanidine; biguanides such as butylbiguanidine, 1-o-tolylbiguanidine, and 1-phenylbiguanidine; silane coupling agents containing an amino group; ketimine compounds, etc.

[0147] Specific examples of the carboxylic acid include acetic acid, propionic acid, butyric acid, 2-ethylhexanoic acid, lauric acid, stearic acid, oleic acid, linoleic acid, neodecanoic acid, and versatic acid.

[0148] Specific examples of the alkoxide metal include titanium compounds such as tetrabutyl titanate, titanium tetra(acetylacetonate), and diisopropoxydi(ethyl acetylacetonate)titanium; aluminum compounds such as tri(acetylacetonate)aluminum and diisopropoxyethyl acetylacetonate; and zirconium compounds such as zirconium tetra(acetylacetonate).

[0149] As other silanol condensation catalysts, compounds containing fluoride anions, photoacid generators, and photobase generators may also be used.

[0150] The silanol condensation catalyst may be used in combination of two or more different catalysts.

[0151] The amount of the silanol condensation catalyst used is preferably 0.001 to 20 parts by weight, more preferably 0.01 to 15 parts by weight, particularly preferably 0.01 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group.

[0152] <Thickener>

[0153] A tackifier may be added to the present curable composition.

[0154] As the thickener, a silane coupling agent or a reaction product of a silane coupling agent may be added.

[0155] Specific examples of the silane coupling agent include amino group-containing silanes such as γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldimethoxysilane, N-β-aminoethyl-γ-aminopropyltrimethoxysilane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, and (2-aminoethyl)aminomethyltrimethoxysilane; γ-isocyanatepropyltrimethoxysilane, γ-isocyanatepropyltriethylsilane, and the like. Silanes containing isocyanate groups, such as oxysilane, γ-isocyanate propyl methyl dimethoxysilane, α-isocyanate methyl trimethoxysilane, α-isocyanate methyl dimethoxymethyl silane; silanes containing mercapto groups, such as γ-mercaptopropyl trimethoxysilane, γ-mercaptopropyl triethoxysilane, γ-mercaptopropyl methyl dimethoxysilane; silanes containing epoxy groups, such as γ-glycidoxypropyl trimethoxysilane, β-(3,4-epoxycyclohexyl) ethyl trimethoxysilane.

[0156] In addition, various silane coupling agent condensates such as aminosilane condensates and condensates of aminosilane and other alkoxysilanes; reaction products of various silane coupling agents such as reaction products of aminosilane and epoxysilane and reaction products of aminosilane and (meth)acrylic group-containing silanes can also be used.

[0157] The above-mentioned thickeners may be used alone or in combination of two or more.

[0158] The amount of the silane coupling agent used is preferably 0.1 to 20 parts by weight, particularly preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group.

[0159] <Plasticizer>

[0160] A plasticizer may be added to the curable composition. Specific examples of the plasticizer include phthalate compounds such as dibutyl phthalate, diisononyl phthalate (DINP), diheptyl phthalate, di(2-ethylhexyl) phthalate, diisodecyl phthalate (DIDP), and butyl benzyl phthalate; terephthalate compounds such as bis(2-ethylhexyl)-1,4-benzenedicarboxylate; and non-phthalate compounds such as diisononyl 1,2-cyclohexanedicarboxylate. Ester compounds; aliphatic polycarboxylic acid ester compounds such as dioctyl adipate, dioctyl sebacate, dibutyl sebacate, diisodecyl succinate, and acetyl tributyl citrate; unsaturated fatty acid ester compounds such as butyl oleate and methyl acetylic ricinoleate; alkyl sulfonate phenyl esters; phosphate compounds; trimellitate compounds; chlorinated paraffins; hydrocarbon oils such as alkyl biphenyls and partially hydrogenated terphenyls; process oils; epoxy plasticizers such as epoxidized soybean oil and epoxy stearate benzyl; and the like.

[0161] In addition, polymer plasticizers can also be used. Specific examples of polymer plasticizers include vinyl polymers; polyester plasticizers; polyether polyols such as polyethylene glycol and polypropylene glycol having a number average molecular weight of 500 or more, and polyether derivatives such as derivatives obtained by converting the hydroxyl groups of these polyether polyols into ester groups, ether groups, etc.; polystyrenes; polybutadiene, polybutylene, polyisobutylene, butadiene-acrylonitrile, polychloroprene, etc.

[0162] The amount of the plasticizer used is preferably 5 to 150 parts by weight, more preferably 10 to 120 parts by weight, and particularly preferably 20 to 100 parts by weight, relative to 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group. When the amount is less than 5 parts by weight, the effect as a plasticizer cannot be exhibited, and when the amount exceeds 150 parts by weight, the mechanical strength of the cured product is insufficient. The plasticizer may be used alone or in combination of two or more.

[0163] <Solvents and diluents>

[0164] A solvent or a diluent may be added to the curable composition. The solvent and the diluent are not particularly limited, and aliphatic hydrocarbons, aromatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, alcohols, esters, ketones, ethers, etc. may be used. When a solvent or a diluent is used, the boiling point of the solvent is preferably 150° C. or more, more preferably 200° C. or more, and particularly preferably 250° C. or more, from the perspective of air pollution when the composition is used indoors. The above-mentioned solvents or diluents may be used alone or in combination of two or more.

[0165] <Filling agent>

[0166] Various fillers can be incorporated into the curable composition. Examples of fillers include heavy calcium carbonate, colloidal calcium carbonate, magnesium carbonate, diatomaceous earth, clay, calcined clay, talc, titanium oxide, fumed silica, precipitated silica, crystalline silica, fused silica, anhydrous silicic acid, hydrous silicic acid, carbon black, iron oxide, aluminum powder, zinc oxide, active zinc flower, PVC powder, PMMA powder, glass fiber and filament, etc. The above-mentioned fillers can be used alone or in combination of two or more.

[0167] The amount of the filler used is preferably 1 to 300 parts by weight, particularly preferably 10 to 250 parts by weight, based on 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group.

[0168] For the purpose of reducing the weight of the composition (lowering the specific gravity), organic hollow spheres and inorganic hollow spheres can be added. The hollow spheres are spherical fillers and are hollow inside. The materials of the hollow spheres include inorganic materials such as glass, white sand, and silica, and organic materials such as phenolic resin, urea resin, polystyrene, and Saran.

[0169] The amount of the hollow spheres used is preferably 0.1 to 100 parts by weight, particularly preferably 1 to 20 parts by weight, based on 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group.

[0170] <Anti-sagging agent>

[0171] In order to prevent sagging and improve workability, an anti-sagging agent may be added to the curable composition as needed. In addition, the anti-sagging agent is not particularly limited, and examples thereof include polyamide waxes; hydrogenated castor oil derivatives; metal soaps such as calcium stearate, aluminum stearate, and barium stearate; and silicon dioxide. These anti-sagging agents may be used alone or in combination of two or more.

[0172] The amount of the anti-sagging agent used is preferably 0.1 to 20 parts by weight based on 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group.

[0173] <Antioxidants>

[0174] An antioxidant (anti-aging agent) can be used in this curable composition. When an antioxidant is used, the weather resistance of the cured product can be improved. As antioxidants, hindered phenols, monophenols, bisphenols, and polyphenols can be exemplified. Specific examples of antioxidants are also recorded in Japanese Patent Publication No. 4-283259 and Japanese Patent Publication No. 9-194731.

[0175] The amount of the antioxidant used is preferably 0.1 to 10 parts by weight, particularly preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group.

[0176] <Light stabilizer>

[0177] A light stabilizer can be used in the curable composition. When a light stabilizer is used, photo-oxidative degradation of the cured product can be prevented. Examples of light stabilizers include benzotriazoles, hindered amines, and benzoate compounds, and hindered amines are particularly preferred.

[0178] The amount of the light stabilizer used is preferably 0.1 to 10 parts by weight, particularly preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group.

[0179] <Ultraviolet light absorber>

[0180] Ultraviolet light absorbers can be used in this curable composition. When ultraviolet light absorbers are used, the surface weather resistance of the cured product can be improved. As ultraviolet light absorbers, benzophenones, benzotriazoles, salicylates, substituted acrylonitriles, hydroxyphenyl triazines and metal chelate compounds can be exemplified, benzotriazoles and hydroxyphenyl triazines are particularly preferred, and commercially available Tinuvin P, Tinuvin 213, Tinuvin 234, Tinuvin 326, Tinuvin 327, Tinuvin 328, Tinuvin 329, Tinuvin 571, Tinuvin 400, Tinuvin 405, Tinuvin 460, Tinuvin 477, Tinuvin 479 (more than BASF company system) can be cited.

[0181] The amount of the ultraviolet absorber used is preferably 0.1 to 10 parts by weight, particularly preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group.

[0182] <Physical property adjuster>

[0183] In this curable composition, a physical property adjuster for adjusting the tensile properties of the generated cured product can be added as needed. As a physical property adjuster, there is no particular limitation, and examples thereof include: alkyl alkoxysilanes such as phenoxytrimethylsilane, methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, and n-propyltrimethoxysilane; aryl alkoxysilanes such as diphenyldimethoxysilane and phenyltrimethoxysilane; alkyl isopropenoxysilanes such as dimethyldiisopropenoxysilane, methyltriisopropenoxysilane, and γ-glycidoxypropylmethyldiisopropenoxysilane; trialkylsilyl borate such as tri(trimethylsilyl) borate and tri(triethylsilyl) borate; silicone varnish; polysiloxanes, etc. By using the above-mentioned physical property adjuster, the hardness of the composition of the present invention can be increased when it is cured, otherwise the hardness is reduced and tensile fracture may occur. The above-mentioned physical property adjuster can be used alone or in combination of two or more.

[0184] In particular, compounds that can generate compounds with a univalent silanol group in the molecule by hydrolysis have the effect of reducing the modulus of the cured product without causing the surface of the cured product to become sticky. Particularly preferably, compounds that generate trimethylsilanol. As compounds that can generate compounds with a univalent silanol group in the molecule by hydrolysis, silicon compounds that generate monohydroxy silane by hydrolysis can be cited, which are derivatives of alcohols such as hexanol, octanol, phenol, trimethylolpropane, glycerol, pentaerythritol, and sorbitol. Specific examples can include phenoxytrimethylsilane, tris((trimethylsilyloxy)methyl)propane, etc.

[0185] The amount of the property adjuster used is preferably 0.1 to 10 parts by weight, particularly preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group.

[0186] <Tackifying resin>

[0187] In order to improve the adhesiveness and adhesion to the substrate or according to other needs, a tackifier resin may be added to the curable composition. The tackifier resin is not particularly limited, and a commonly used tackifier resin can be used.

[0188] As specific examples, terpene resin, aromatic modified terpene resin, hydrogenated terpene resin, terpene-phenolic resin, phenolic resin, modified phenolic resin, xylene-phenolic resin, cyclopentadiene-phenolic resin, coumarone indene resin, rosin resin, rosin ester resin, hydrogenated rosin ester resin, xylene resin, low molecular weight polystyrene resin, styrene copolymer resin, styrene block copolymer and hydride thereof, petroleum resin (for example, C5 hydrocarbon resin, C9 hydrocarbon resin, C5C9 hydrocarbon copolymer resin, etc.), hydrogenated petroleum resin, DCPD resin, etc. can be enumerated. These can be used alone, and two or more combinations can also be used.

[0189] The amount of the tackifier resin used is preferably 2 to 100 parts by weight, more preferably 5 to 50 parts by weight, and even more preferably 5 to 30 parts by weight relative to 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group. When the amount is less than 2 parts by weight, it is difficult to obtain an adhesive or close adhesion effect to the substrate, and when the amount exceeds 100 parts by weight, the viscosity of the composition becomes too high, and it may be difficult to handle.

[0190] <Compounds containing epoxy groups>

[0191] Compounds containing epoxy groups can be used in this curable composition. When a compound having an epoxy group is used, the recovery of the cured product can be improved. Examples of compounds having an epoxy group include epoxidized unsaturated oils and fats, epoxidized unsaturated fatty acid esters, alicyclic epoxy compounds, compounds represented by epichlorohydrin derivatives, and mixtures thereof. Specifically, examples include: epoxidized soybean oil, epoxidized linseed oil, bis(2-ethylhexyl)-4,5-epoxycyclohexane-1,2-dicarbonate (E-PS), octyl epoxystearate, butyl epoxystearate, and the like. The epoxy compound can be used in a range of 0.5 to 50 parts by weight relative to 100 parts by weight of the polymer (A) having a hydrolyzable silyl group.

[0192] <Photocurable substances>

[0193] Photocurable substances can be used in the curable composition. When photocurable substances are used, a film of the photocurable substance can be formed on the surface of the cured product to improve the stickiness and weather resistance of the cured product. There are many known compounds of this type, such as organic monomers, oligomers, resins, or compositions containing them. As representative substances, monomers, oligomers, or unsaturated acrylic compounds that are mixtures of one or more acrylic or methacrylic unsaturated groups, polyvinyl cinnamate, or azidized resins can be used.

[0194] The photocurable material can be used in an amount of 0.1 to 20 parts by weight, preferably 0.5 to 10 parts by weight, relative to 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group. When the amount is less than 0.1 parts by weight, the effect of improving weather resistance cannot be exerted, and when the amount is more than 20 parts by weight, the cured product becomes too hard and tends to crack.

[0195] <Oxygen-curable substances>

[0196] Oxygen-curing substances can be used in the present curing composition. As for oxygen-curing substances, unsaturated compounds that can react with oxygen in the air can be listed. The unsaturated compounds react with oxygen in the air to form a cured film near the surface of the cured product, which plays a role in preventing the surface from becoming sticky and preventing dirt and dust from adhering to the surface of the cured product. Specific examples of oxygen-curing substances include drying oils represented by tung oil, linseed oil, etc., various alkyd resins modified from the compounds; acrylic polymers, epoxy resins, and silicone resins modified with drying oils; liquid polymers such as 1,2-polybutadiene, 1,4-polybutadiene, and polymers of C5 to C8 dienes obtained by polymerization or copolymerization of diene compounds such as butadiene, chloroprene, isoprene, and 1,3-pentadiene. These can be used alone or in combination of two or more.

[0197] The amount of the oxygen-curable substance used can be in the range of 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, relative to 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group. When the amount is less than 0.1 parts by weight, the staining property cannot be sufficiently improved, and when it exceeds 20 parts by weight, there is a tendency to impair the tensile properties of the cured product. It is preferred to use an oxygen-curable substance and a photocurable substance in combination as described in Japanese Patent Application Laid-Open No. 3-160053.

[0198] (2-6. Preparation of curable composition)

[0199] The curable composition can be prepared as a single-component type in which all the ingredients are mixed and sealed beforehand, and cured by moisture in the air after construction, or can be prepared as a two-component type in which another curing catalyst, filler, plasticizer, water and other ingredients as a curing agent are mixed beforehand, and the mixed materials are mixed with the organic polymer composition before use. From the viewpoint of operability, a single-component type is preferred.

[0200] In the case where this curable composition is a single-component type, due to the pre-coordination of all the coordinating components, therefore, the coordinating components preferably containing moisture are used after dehydration in advance, or dehydrated by decompression etc. in the coordinating mixing. In addition, except the dehydration drying method, the storage stability can also be further improved by adding alkoxysilane compounds such as methyltrimethoxysilane, phenyltrimethoxysilane, n-propyltrimethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, γ-glycidoxypropyltrimethoxysilane, methylcarbamatemethyltrimethoxysilane. In addition, by adding calcium oxide, the adhesion after storage stability and the alkali warm water test is further improved. As a dehydrating agent, from the viewpoints of safety, stability etc., it is also preferred to use the partially condensed silane compounds such as Dynasylan6490 of Evonik company etc.

[0201] The amount of the dehydrating agent, particularly a silicon compound reactive with water such as vinyltrimethoxysilane and methyl carbamatemethyltrimethoxysilane, is 0.1 to 20 parts by weight, preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A) having a hydrolyzable silyl group.

[0202] 〔3. Cured product〕

[0203] In one embodiment of the present invention, there is provided a cured product obtained by curing the present curable composition (hereinafter referred to as “the present cured product”).

[0204] The present cured product is obtained by curing the present curable composition. Therefore, the present cured product has excellent adhesiveness.

[0205] In one embodiment of the present invention, the present cured product is formed by curing the following curable composition at room temperature or under heating up to 70°C.

[0206] A curable composition comprising an agent A containing the components (A), (B) and (C) and an agent B containing the component (D)

[0207] 〔4. Application〕

[0208] The curable composition can be used in a variety of applications, such as waterproof materials, elastic sealing materials for buildings, sealing materials for sidings, sealing materials for multi-layered glass, sealing materials for vehicles and other sealing materials for buildings and industries, electrical / electronic component materials such as solar cell back sealants, electrical insulating materials such as insulating coating materials for wires / cables, adhesives, bonding agents (e.g., elastic bonding agents, contact bonding agents, tile bonding agents, reactive hot melt bonding agents), paints, powder coatings, coating materials, foams, sealing materials such as can lids, heat sinks, electrical and electronic castings, films, gas gaskets, ship deck caulking materials, casting materials, various molding materials, artificial marble, and rust-proof / waterproof sealing materials for the end faces (cut portions) of wired glass and laminated glass, vibration-proof / vibration-damping / sound-insulating / seismic-resistant materials for automobiles, ships, home appliances, etc., liquid sealing materials used for automobile components, motor components, various machine components, etc.

[0209] In one embodiment of the present invention, an adhesive comprising the present curable composition is provided, preferably an adhesive for tiles is provided.

[0210] In one embodiment of the present invention, a laminated body is provided in which tiles are laminated on at least one side of a substrate via an adhesive comprising the present curable composition. In this embodiment, the substrate may include, for example, mortar, concrete, ceramics, sanitary ceramics, wooden substrates, waterproof sheets, etc. The laminated body may include, for example, walls, floors, etc., preferably floors.

[0211] The present invention is not limited to the above-described embodiments, and various modifications can be made within the scope of the claims. Embodiments obtained by appropriately combining technical means disclosed in different embodiments are also included in the technical scope of the present invention.

[0212] That is, one embodiment of the present invention is as follows.

[0213] <1> A curable composition comprising:

[0214] (A) 100 parts by weight of an organic polymer having a hydrolyzable silyl group;

[0215] (B) 3 to 35 parts by weight of at least one selected from paraffinic process oil, cycloparaffinic process oil and aromatic process oil;

[0216] (C) 20 to 200 parts by weight of silica sand; and

[0217] (D) 2 to 10 parts by weight of a silane compound having an epoxy group and / or a silane compound having an amino group.

[0218] <2> The curable composition according to <1>, wherein

[0219] The organic polymer (A) is a hydrolyzable silyl group-containing polyoxyalkylene polymer (A1) and / or a hydrolyzable silyl group-containing (meth)acrylate copolymer (A2).

[0220] <3> The curable composition according to <2>, wherein

[0221] The main chain of the hydrolyzable silyl group-containing polyoxyalkylene polymer (A1) is polypropylene glycol.

[0222] <4> The curable composition according to any one of <1> to <3>, further comprising 150 to 400 parts by weight of calcium carbonate.

[0223] <5> A cured product obtained by curing the curable composition according to any one of <1> to <4>.

[0224] <6> An adhesive comprising the curable composition according to any one of <1> to <4>.

[0225] <7> A laminated body comprising tiles laminated on at least one surface of a substrate via the adhesive according to <1> or <2>.

[0226] Example

[0227] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0228] 〔Material〕

[0229] The materials used in Examples and Comparative Examples are as follows.

[0230] ((A) ingredient)

[0231] Organic polymers (A-1), (A-2), (A-3), (A-4), and (A-5) produced according to the following synthesis examples were used.

[0232] ((B) ingredient)

[0233] Process oil (B-1): Diana Process Oil PS-32 (paraffinic process oil, manufactured by Idemitsu Kosan Co., Ltd.)

[0234] Process oil (B-2): VC CLEAN AI95 (paraffinic process oil, manufactured by ANDOH PARACHEMIE)

[0235] Process oil (B-3): liquid paraffin (reagent, manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.)

[0236] Process oil (B-4): Exxol D80 (cycloparaffinic process oil, manufactured by ANDOH PARACHEMIE)

[0237] Process oil (B-5): Diana Process Oil NP-24 (cycloparaffinic process oil, manufactured by Idemitsu Kosan Co., Ltd.)

[0238] Process oil (B-6): Diana Process Oil AC-12 (aromatic process oil, manufactured by Idemitsu Kosan Co., Ltd.)

[0239] ((C) ingredient)

[0240] Silica sand: Silica sand No. 8 (manufactured by Maruo Calcium Co., Ltd.)

[0241] ((D) ingredient)

[0242] Silane compound having an epoxy group: Silquest A-187 (3-glycidoxypropyltrimethoxysilane, manufactured by Momentive Performance Materials)

[0243] Silane compound having an amino group: Silquest A-1120 (N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, “aminosilane”, manufactured by Momentive Performance Materials)

[0244] (Other ingredients)

[0245] Plasticizer: DIDP (diisodecyl phthalate, manufactured by J-PLUS)

[0246] Heavy calcium carbonate-1: TC-1016 (manufactured by Maruo Calcium Co., Ltd.)

[0247] Heavy calcium carbonate-2: Omyacarb 2T-HB (manufactured by Omya)

[0248] Colloidal calcium carbonate-1: Viscolite EL20 (manufactured by Shiraishi Industries, Ltd.)

[0249] Colloidal calcium carbonate-2: TNA (produced by TAEKYUNG BK Co., Ltd., South Korea)

[0250] Antioxidant: Irganox 1010 (manufactured by BASF Japan)

[0251] Dehydrating agent-1: Silquest A-171 (vinyltrimethoxysilane, manufactured by Momentive Performance Materials)

[0252] Dehydrating agent - 2: Calcium oxide (CML35, manufactured by Omi Chemical Industry Co., Ltd.)

[0253] Curing catalyst: NEOSTANN U - 130 (dibutyltin - based curing catalyst, manufactured by Nitto Kasei Co., Ltd.)

[0254] Epoxy resin: EPIKOTE 828 (bisphenol A - type epoxy resin, manufactured by Hexion)

[0255] Curing agent for epoxy resin: Ancamine K54 (manufactured by Evonik Japan Co., Ltd.).

[0256] [Measurement and evaluation methods]

[0257] The measurements and evaluations in the examples and comparative examples were carried out by the following methods.

[0258] (Viscosity)

[0259] Using the composition prepared in the example, the viscosities at 1 rpm, 2 rpm, and 10 rpm were measured using a BS - type viscometer (manufactured by TOKIMEC, rotor No. 7) as the initial viscosity (Pa·s).

[0260] (Workability)

[0261] For the curable composition prepared in the example, the trowel flexibility (sabaki - sei) and stringing when contacting with a toothed trowel were evaluated. Specifically, an appropriate amount of the curable composition was placed on a horizontally placed plate, leveled smoothly to a thickness of 7 - 10 mm using a spatula, etc., and then a standard toothed trowel was set at an angle of 60 degrees and pulled forward in one go. When the above - mentioned toothed trowel was lifted upward, the case where the curable composition extended more than 5 mm on the toothed trowel was regarded as having stringing, and the case where it was less than 5 mm was regarded as having no stringing. It should be noted that as the toothed trowel, a standard toothed trowel (product name: LKT - 5) suitable for elastic adhesives with a tooth mark height of 5 mm was used. The workability was evaluated as follows.

[0262] · "○": Good resistance of the toothed trowel (trowel flexibility), no stringing

[0263] · "×": The resistance of the toothed trowel (trowel flexibility) is extremely light or heavy, or there is stringing.

[0264] (Tensile physical properties)

[0265] The curable composition prepared in the example was made into a sheet test body with a thickness of about 3 mm, and after being cured by aging at 23°C × 3 days and 50°C × 4 days, it was punched into a dumbbell shape No. 3. A tensile test (23°C, 50% RH) was carried out at a tensile speed of 200 mm / min using an Autograph manufactured by Shimadzu Corporation, and the 50% tensile modulus, breaking strength, and elongation at break (%) were measured.

[0266] (Tile Adhesion)

[0267] The test was carried out in accordance with JIS A5557-2020 (organic adhesive for bonding exterior tiles) using ceramic tiles produced by LIXIL Co., Ltd.

[0268] Standard aging: The test specimens were aged at 23°C and 50% RH for 28 days.

[0269] Alkaline warm water immersion treatment: After standard aging, the samples were immersed in a saturated aqueous solution of calcium hydroxide at 60°C for 7 days.

[0270] (bad smell)

[0271] The curable compositions prepared in the Examples were evaluated for unpleasant odors based on the following three-level criteria.

[0272] 1 With respect to the curable composition, almost no unpleasant odor was observed even when the nose was brought close to a distance of 10 cm.

[0273] 2 With respect to the curable composition, an unpleasant odor was detected when the nose was brought close to a distance of 10 cm.

[0274] 3 For the curable composition, an unpleasant odor can be detected when the nose is brought closer than 10 cm.

[0275] (Number average molecular weight)

[0276] The following apparatus was used for the measurement of the number average molecular weight. The measured value is a polystyrene-equivalent molecular weight.

[0277] ·Liquid delivery system: HLC-8120GPC (manufactured by Tosoh Corporation)

[0278] ·Column: TSK-GEL H type (manufactured by Tosoh Corporation)

[0279] Solvent: THF.

[0280] (Method for determining the number of terminal silyl groups)

[0281] according to 1 The number of terminal silyl groups was calculated from the results of H-NMR measurement. 1The following apparatus was used for the H-NMR measurement.

[0282] ·Measurement instrument: JNM-LA400 (manufactured by JEOL Ltd.)

[0283] Solvent: CDCl3.

[0284] [Synthesis Example 1: Organic polymer (A-1) (corresponding to component (A1))]

[0285] A polyoxyalkylene polymer (A-1) having a methyldimethoxysilyl group introduced at a molecular terminal was synthesized according to the following procedure.

[0286] 1. Propylene oxide was polymerized to obtain polypropylene oxide with a number average molecular weight of about 1600. Polyoxypropylene triol (molecular weight: about 4500) was used as an initiator. Zinc hexacyanocobaltate glyme complex was used as a catalyst. The three terminals of the obtained polypropylene oxide molecule were hydroxyl groups.

[0287] 2. Add 1.2 equivalents of NaOMe to the hydroxyl groups at the ends of the polypropylene oxide molecules in the form of a methanol solution, and distill off the methanol.

[0288] 3. Add 1.5 molar equivalents of allyl chloride to convert the hydroxyl groups at the ends of the polypropylene oxide molecules into allyl groups, thereby obtaining unpurified allyl-terminated polypropylene oxide.

[0289] 4. 300 parts by weight of n-hexane and 300 parts by weight of water were mixed with 100 parts by weight of the unpurified allyl-terminated polypropylene oxide and stirred, and then the water was removed by centrifugal separation.

[0290] 5. 300 parts by weight of water was again mixed with the obtained solution and stirred, and then the water was removed by centrifugal separation.

[0291] 6. Remove the hexane by devolatilization under reduced pressure. Thus, purified allyl-terminated polypropylene oxide is obtained.

[0292] 7. 1.80 parts by weight of methyldimethoxysilane was added to 100 parts by weight of the purified allyl-terminated polypropylene oxide, and the mixture was reacted at 90°C for 2 hours. An isopropanol solution of a vinylsiloxane platinum complex (platinum content: 3 wt%) was used as the catalyst. The concentration of the catalyst in the system was 150 ppm. Thus, an organic polymer (A-1) was obtained.

[0293] The organic polymer (A-1) is polypropylene oxide having a methyldimethoxysilyl group introduced at the terminal, and has a number average molecular weight of about 16,000. 1H-NMR measurement revealed that the organic polymer (A-1) had an average of 0.7 dimethoxymethylsilyl groups at one terminal and an average of 2.1 dimethoxymethylsilyl groups in one molecule.

[0294] [Synthesis Example 2: Organic polymer (A-2) (corresponding to component (A1))]

[0295] A polyoxyalkylene polymer (A-2) having a methyldimethoxysilyl group introduced at a molecular terminal was synthesized according to the following procedure.

[0296] 1. Propylene oxide was polymerized to obtain polypropylene oxide with a number average molecular weight of about 15,000. Polyoxypropylene glycol (molecular weight: about 4,500) was used as an initiator. Zinc hexacyanocobaltate glyme complex was used as a catalyst. Both ends of the obtained polypropylene oxide molecule were hydroxyl groups.

[0297] 2. Purified allyl-terminated polypropylene oxide was obtained by the same procedures as steps 2 to 6 of the above-mentioned synthesis example of organic polymer (A-1).

[0298] 3. 1.70 parts by weight of methyldimethoxysilane was added to 100 parts by weight of the purified allyl-terminated polypropylene oxide, and the mixture was reacted at 90°C for 2 hours. An isopropanol solution of a vinylsiloxane platinum complex (platinum content: 3 wt%) was used as the catalyst. The concentration of the catalyst in the system was 150 ppm. Thus, an organic polymer (A-2) was obtained.

[0299] The organic polymer (A-2) is polypropylene oxide having a methyldimethoxysilyl group introduced at the terminal, and has a number average molecular weight of about 15,000. 1 H-NMR measurement revealed that the organic polymer (A-2) had an average of 0.8 dimethoxymethylsilyl groups at one terminal and an average of 1.5 dimethoxymethylsilyl groups in one molecule.

[0300] [Synthesis Example 3: Organic polymer (A-3) (corresponding to component (A1))]

[0301] A polyoxyalkylene polymer (A-3) having a methyldimethoxysilyl group introduced at a molecular terminal was synthesized according to the following procedure.

[0302] 1. Propylene oxide was polymerized to obtain polypropylene oxide with a number average molecular weight of about 26,000. Polyoxypropylene triol (molecular weight: about 4,500) was used as an initiator. Zinc hexacyanocobaltate glyme complex was used as a catalyst. The three terminals of the obtained polypropylene oxide molecule were hydroxyl groups.

[0303] 2. Purified allyl-terminated polypropylene oxide was obtained by the same procedures as steps 2 to 6 of the above-mentioned synthesis example of organic polymer (A-1).

[0304] 3. 1.30 parts by weight of methyldimethoxysilane was added to 100 parts by weight of the purified allyl-terminated polypropylene oxide, and the mixture was reacted at 90°C for 2 hours. The catalyst used was an isopropanol solution of a vinylsiloxane platinum complex (platinum content: 3 wt%). The catalyst concentration in the system was 150 ppm. Thus, an organic polymer (A-3) was obtained.

[0305] The organic polymer (A-3) is polypropylene oxide having a methyldimethoxysilyl group introduced at the terminal, and has a number average molecular weight of about 26,000. 1 H-NMR measurement revealed that the organic polymer (A-3) had an average of 0.7 dimethoxymethylsilyl groups at one terminal and an average of 2.2 dimethoxymethylsilyl groups in one molecule.

[0306] [Synthesis Example 4: Organic polymer (A-4) (corresponding to component (A1))]

[0307] A polyoxyalkylene polymer (A-4) having a methyldimethoxysilyl group introduced at a molecular terminal was synthesized according to the following procedure.

[0308] 1. Propylene oxide was polymerized to obtain polypropylene oxide with a number average molecular weight of about 29,000. Polyoxypropylene glycol (molecular weight: about 4,500) was used as an initiator. Zinc hexacyanocobaltate glyme complex was used as a catalyst. Both ends of the obtained polypropylene oxide molecule were hydroxyl groups.

[0309] 2. NaOMe was added in a methanol solution in an amount of 1.0 molar equivalent to the hydroxyl group at the terminal of the polypropylene oxide molecule, and the methanol was distilled off.

[0310] 3. 1.0 molar equivalent of allyl glycidyl ether was added to the hydroxyl group of the hydroxyl-terminated polypropylene oxide, and the mixture was reacted at 130°C for 2 hours. Then, 0.28 molar equivalent of NaOMe was added in the form of a methanol solution, the methanol was distilled off, and 1.8 molar equivalent of allyl chloride was further added to convert the hydroxyl group at the terminal of the polypropylene oxide molecule into an allyl group. Thus, unpurified allyl-terminated polypropylene oxide was obtained.

[0311] 4. 300 parts by weight of n-hexane and 300 parts by weight of water were mixed with 100 parts by weight of the unpurified allyl-terminated polypropylene oxide and stirred, and then the water was removed by centrifugal separation.

[0312] 5. 300 parts by weight of water was again mixed with the obtained solution and stirred, and then the water was removed by centrifugal separation.

[0313] 6. Remove the hexane by devolatilization under reduced pressure. Thus, purified allyl-terminated polypropylene oxide is obtained.

[0314] 7. 1.90 parts by weight of methyldimethoxysilane was added to 100 parts by weight of the purified allyl-terminated polypropylene oxide, and the mixture was reacted at 90°C for 2 hours. An isopropanol solution of a vinylsiloxane platinum complex (platinum content: 3 wt%) was used as the catalyst. The concentration of the catalyst in the system was 150 ppm. Thus, an organic polymer (A-4) was obtained.

[0315] The organic polymer (A-4) is polypropylene oxide having a methyldimethoxysilyl group introduced at the terminal, and has a number average molecular weight of about 29,000. 1 H-NMR measurement revealed that the organic polymer (A-4) had an average of 1.7 dimethoxymethylsilyl groups at one terminal and an average of 3.4 dimethoxymethylsilyl groups in one molecule.

[0316] [Synthesis Example 5: Organic polymer (A-5) (corresponding to component (A1))]

[0317] A polyoxyalkylene polymer (A-5) having a trimethoxysilyl group introduced at a molecular terminal was synthesized according to the following procedure.

[0318] 1. Propylene oxide was polymerized to obtain polypropylene oxide with a number average molecular weight of about 29,000. Polyoxypropylene glycol (molecular weight: about 4,500) was used as an initiator. Zinc hexacyanocobaltate glyme complex was used as a catalyst. Both ends of the obtained polypropylene oxide molecule were hydroxyl groups.

[0319] 2. 10 ppm of bismuth (III) tris(2-ethylhexanoate) and 1.9 parts by weight of 3-isocyanatepropyltrimethoxysilane were added to 100 parts by weight of the hydroxyl-terminated polypropylene oxide, and reacted at 90° C. for 2 hours to obtain an organic polymer (A-5).

[0320] The organic polymer (A-5) is polypropylene oxide having trimethoxysilyl groups introduced at the terminals, and has a number average molecular weight of 29,500. 1 As a result of H-NMR measurement, it was found that the organic polymer (A-5) had an average of 1.0 trimethoxysilyl group at one terminal and an average of 2.0 trimethoxysilyl groups in one molecule.

[0321] [Example 1]

[0322] The organic polymer (A-1), process oil (B-1), silica sand, plasticizer, heavy calcium carbonate-1, colloidal calcium carbonate-1, antioxidant, and dehydrating agent-2 were weighed and mixed according to the ratios listed in Table 1, and dispersed by passing through a three-roll mixer three times. The mixture was placed in a thermostatic chamber at 23° C. and 50% conditions overnight, and then the viscosity of the composition was measured.

[0323] Next, a silane compound having an epoxy group, a dehydrating agent-1, and a curing catalyst were added and kneaded in the proportions described in Table 1 to obtain a curable composition. A rotation / revolution mixer (made by THINKY, Degassing Rentaro ARE-250) was used for kneading. Using the prepared curable composition, various physical properties were evaluated by the method described in the above-mentioned [Measurement and Evaluation Method]. The results are shown in Table 1. It should be noted that the amount of each component in Table 1 is expressed in parts by weight.

[0324] [Examples 2 to 13, Comparative Examples 1 to 9]

[0325] A curable composition was prepared by the same procedure as in Example 1 except that the amount of each component was changed as shown in Tables 1 and 2. Using the prepared curable composition, various physical properties were evaluated by the methods described in the above [Measurement and Evaluation Methods]. The results are shown in Tables 1 and 2.

[0326]

[0327]

[0328] 〔result〕

[0329] As shown in Tables 1 and 2, the curable compositions of Examples 1 to 13 had good workability, suppressed bad odor, and had excellent adhesion even after alkali treatment.

[0330] Industrial Applicability

[0331] According to one embodiment of the present invention, a curable composition having good workability, suppressed bad odor, and excellent adhesiveness can be provided, and thus the composition can be suitably used for a sealant or the like.

Claims

1. A curable composition comprising: (A) 100 parts by weight of an organic polymer having a hydrolyzable silyl group; (B) 3 to 35 parts by weight of at least one selected from paraffinic process oil, cycloparaffinic process oil and aromatic process oil; (C) 20 to 200 parts by weight of silica sand; and (D) 2 to 10 parts by weight of a silane compound having an epoxy group and / or a silane compound having an amino group.

2. The curable composition according to claim 1, in, The organic polymer (A) is a hydrolyzable silyl group-containing polyoxyalkylene polymer (A1) and / or a hydrolyzable silyl group-containing (meth)acrylate copolymer (A2).

3. The curable composition according to claim 2, in, The main chain of the hydrolyzable silyl group-containing polyoxyalkylene polymer (A1) is polypropylene glycol.

4. The curable composition according to claim 1 or 2, further comprising 150 to 400 parts by weight of calcium carbonate.

5. A cured product obtained by curing the curable composition according to claim 1 or 2. 6 . An adhesive comprising the curable composition according to claim 1 or 2 .

7. A laminated body comprising tiles laminated on at least one surface of a substrate via the adhesive according to claim 1 or 2.