Electromagnetic wave shielding film
By adding porous inorganic particles to the adhesive layer of the electromagnetic wave shielding film, the problem of interlayer peeling caused by reflow heating is solved, the adhesive layer and the shielding layer are stably bonded, and the durability of the electromagnetic wave shielding film is improved. .
Patent Information
- Application Number
- CN202380024924.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-18
AI Technical Summary
In existing electromagnetic wave shielding films, during the heating process such as reflow soldering, the tightness between the adhesive layer and the shielding layer is easily damaged, leading to the problem of interlayer peeling.
By adding porous inorganic particles to the adhesive layer, its hygroscopicity is reduced and volatile components are prevented from accumulating, thereby improving the adhesion strength between the adhesive layer and the shielding layer. The pore volume, specific surface area and average pore diameter of the porous inorganic particles are within the range of 0.44mL/g to 1.80mL/g, 280m2/g to 700m2/g and 2.5nm to 26nm, respectively, which are moderately sized to avoid accumulation and absorption of volatile components.
Even under heating conditions such as reflow soldering, the interlayer adhesion between the adhesive layer and the shielding layer is not easily destroyed, which improves the stability and durability of the electromagnetic wave shielding film.
Smart Images

Figure CN118805451A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electromagnetic wave shielding film. Background Art
[0002] Conventionally, for example, an electromagnetic wave shielding film is attached to a printed circuit board such as a flexible printed circuit board (FPC) to shield electromagnetic waves from the outside.
[0003] The electromagnetic wave shielding film usually has a structure in which an adhesive layer, a shielding layer formed by a metal film, etc., and an insulating layer are sequentially stacked. The electromagnetic wave shielding film is heated and pressed in a state where it overlaps on a printed circuit board, so that the electromagnetic wave shielding film is bonded to the printed circuit board by the adhesive layer to produce a shielded printed circuit board. After the bonding, components are mounted on the shielded printed circuit board by solder reflow. In addition, the printed circuit board becomes a structure in which the printed pattern on the base film is covered by the insulating film.
[0004] As such an electromagnetic wave shielding film, Patent Document 1 discloses a shielding film characterized by comprising a metal layer and an anisotropic conductive adhesive layer having a thickness of 0.5 μm to 12 μm in a laminated state.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2013 / 077108 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] When such an electromagnetic shielding film is disposed on a printed circuit board and then components are mounted by reflow soldering or the like, there is a problem that the interlayer adhesion between the adhesive layer and the metal layer of the electromagnetic shielding film is destroyed, resulting in interlayer delamination.
[0010] It is considered that the above-mentioned interlayer delamination occurs due to the following mechanism.
[0011] Figure 3A and Figure 3B This is an explanatory diagram schematically showing the mechanism of interlayer delamination between an adhesive layer and a metal layer when a shield printed wiring board is manufactured using a conventional electromagnetic wave shielding film.
[0012] like Figure 3A As shown, when manufacturing a shielded printed circuit board, an electromagnetic wave shielding film 510 on which an adhesive layer 520 and a shielding layer 530 formed of a metal layer are sequentially laminated is heated by heat pressing and solder reflow.
[0013] Due to this heating, volatile components (mainly water) 560 are generated from the adhesive layer 520 and the like of the electromagnetic shielding film 510 , and are accumulated between the adhesive layer 520 and the shielding layer 530 .
[0014] In this state, if rapid heating such as reflow soldering is performed to mount components, Figure 3B As shown, the volatile component 560 accumulated between the adhesive layer 520 and the shielding layer 530 expands, thereby destroying the interlayer adhesion between the adhesive layer 520 and the shielding layer 530, and causing interlayer delamination.
[0015] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide an electromagnetic wave shielding film in which the interlayer adhesion between an adhesive layer and a shielding layer is not easily damaged even when heated by reflow soldering or the like.
[0016] Solutions for solving problems
[0017] The present inventors have found that the reason why volatile components accumulate between the adhesive layer and the shielding layer is that the adhesive layer absorbs moisture in the air when the electromagnetic shielding film is stored. The present invention was conceived to solve this problem by reducing the hygroscopicity of the adhesive layer.
[0018] That is, the electromagnetic wave shielding film of the present invention is characterized in that it contains an adhesive layer and a shielding layer laminated on the adhesive layer, the adhesive layer contains a resin and porous inorganic particles, and the pore volume of the porous inorganic particles exceeds 0.44 mL / g and is 1.80 mL / g or less.
[0019] In the electromagnetic shielding film of the present invention, the porous inorganic particles function as a filler, and thus the strength of the conductive adhesive is increased.
[0020] In addition, as described later, in the electromagnetic wave shielding film of the present invention, porous inorganic particles are not easy to absorb volatile components. Therefore, in the part with porous inorganic particles, volatile components are not absorbed. That is, by including porous inorganic particles, the hygroscopicity of the adhesive layer as a whole is reduced. Therefore, in the electromagnetic wave shielding film of the present invention, even if heated by reflow soldering, the interlayer adhesion of the adhesive layer and the shielding layer is not easy to be destroyed.
[0021] The reason why the porous inorganic particles in the electromagnetic shielding film of the present invention are less likely to absorb volatile components will be described.
[0022] In the electromagnetic shielding film of the present invention, the pore volume of the porous inorganic particles exceeds 0.44 mL / g and is 1.80 mL / g or less.
[0023] When the pore volume of the porous inorganic particles is within the above range, the pores of the porous inorganic particles have an appropriate size, and volatile components such as water are less likely to accumulate in the porous inorganic particles.
[0024] If the pore volume is 0.44 mL / g or less, the pores formed in the porous inorganic particles become smaller, and it becomes easier to exert capillary force. If the pores exert capillary force, volatile components become easier to accumulate in the pores, and the porous inorganic particles become easier to absorb volatile components. Therefore, the hygroscopicity of the adhesive layer as a whole becomes easier to improve.
[0025] If the pore volume exceeds 1.80 mL / g, the pores formed in the porous inorganic particles become larger, and the porous inorganic particles become brittle, making it difficult to improve the strength of the conductive adhesive.
[0026] Another embodiment of the electromagnetic wave shielding film of the present invention is characterized in that it comprises an adhesive layer and a shielding layer laminated on the adhesive layer, the adhesive layer comprises a resin and porous inorganic particles, and the specific surface area of the porous inorganic particles is 280 m 2 / g and below 700m 2 / g.
[0027] In the electromagnetic shielding film of another embodiment of the present invention, the porous inorganic particles function as a filler, and thus the strength of the conductive adhesive is increased.
[0028] In addition, as described later, in the electromagnetic wave shielding film of another mode of the present invention, porous inorganic particles are not easy to absorb volatile components. Therefore, in the part with porous inorganic particles, volatile components are not absorbed. That is, by including porous inorganic particles, the hygroscopicity of the adhesive layer as a whole is reduced. Therefore, in the electromagnetic wave shielding film of another mode of the present invention, even if heated by reflow soldering, the interlayer adhesion of the adhesive layer and the shielding layer is not easy to be destroyed.
[0029] The reason why the porous inorganic particles are less likely to absorb volatile components in the electromagnetic shielding film according to another embodiment of the present invention will be described.
[0030] In the electromagnetic wave shielding film according to another embodiment of the present invention, the specific surface area of the porous inorganic particles is 280 m 2 / g and below 700m 2 / g.
[0031] When the specific surface area of the porous inorganic particles is within the above range, the pores of the porous inorganic particles have an appropriate size, and volatile components such as water are less likely to accumulate in the porous inorganic particles.
[0032] If the above specific surface area is less than 280m 2 / g, the pores formed in the porous inorganic particles become larger, and the porous inorganic particles become brittle. Therefore, it becomes difficult to improve the strength of the adhesive layer.
[0033] If the above specific surface area is 700m 2 / g or more, the pores formed in the porous inorganic particles become smaller, and it becomes easier to exert capillary force. If the pores exert capillary force, volatile components become easier to accumulate in the pores, and the porous inorganic particles become easier to absorb volatile components. Therefore, the hygroscopicity of the entire adhesive layer becomes easier to improve.
[0034] Another embodiment of the electromagnetic wave shielding film of the present invention is characterized in that it includes an adhesive layer and a shielding layer stacked on the adhesive layer, the adhesive layer includes a resin and porous inorganic particles, and the average pore size of the pores of the porous inorganic particles is greater than 2.5 nm and is less than 26 nm.
[0035] In the electromagnetic shielding film according to still another embodiment of the present invention, the porous inorganic particles function as a filler, thereby increasing the strength of the conductive adhesive.
[0036] In addition, as described later, in the electromagnetic wave shielding film of another further mode of the present invention, porous inorganic particles are not easy to absorb volatile components. Therefore, in the part with porous inorganic particles, volatile components are not absorbed. That is, by including porous inorganic particles, the hygroscopicity of the adhesive layer as a whole is reduced. Therefore, in the electromagnetic wave shielding film of another further mode of the present invention, even if heated by reflow soldering, the interlayer adhesion of the adhesive layer and the shielding layer is not easy to be destroyed.
[0037] The reason why the porous inorganic particles are less likely to absorb volatile components in the electromagnetic shielding film according to still another embodiment of the present invention will be described.
[0038] In the electromagnetic shielding film according to still another aspect of the present invention, the average pore diameter of the pores of the porous inorganic particles exceeds 2.5 nm and is 26 nm or less.
[0039] When the average pore size of the pores of the porous inorganic particles is within the above range, the pores of the porous inorganic particles have an appropriate size, and volatile components such as water are less likely to accumulate in the porous inorganic particles.
[0040] If the average pore size of the above-mentioned pores is less than 2.5 nm, the pores formed in the porous inorganic particles become smaller and become easier to exert capillary force. If the pores exert capillary force, volatile components become easier to accumulate in the pores, and the porous inorganic particles become easier to absorb volatile components. Therefore, the hygroscopicity of the entire adhesive layer becomes easier to improve.
[0041] If the average pore diameter of the pores exceeds 26 nm, the pores formed in the porous inorganic particles become larger, and the porous inorganic particles become brittle, thereby making it difficult to improve the strength of the conductive adhesive.
[0042] In the electromagnetic shielding film of the present invention, the DBA value of the porous inorganic particles is preferably 50 meq / kg or more and less than 200 meq / kg.
[0043] It is difficult to produce porous inorganic particles having a DBA value below 50 meq / kg.
[0044] When the DBA value is less than 200 meq / kg, the hydrophobicity becomes high and water becomes less likely to accumulate in the pores.
[0045] It should be noted that the "DBA value" in this specification refers to the amount of di-n-butylamine adsorbed when the porous inorganic particles are treated with a toluene solution of di-n-butylamine (the amount of di-n-butylamine adsorbed relative to 1 kg of particles), and this adsorption amount can be measured by a known titration test or the like.
[0046] In the electromagnetic wave shielding film of the present invention, the particle size (D 50 ) is preferably 1.0 to 20.0 μm.
[0047] The particle size of porous inorganic particles (D 50 ) is less than 1.0 μm, it becomes difficult to form pores of an appropriate size in the porous inorganic particles.
[0048] The particle size of porous inorganic particles (D 50 ) If it exceeds 20.0 μm, the adhesive layer becomes thick, making it difficult to miniaturize the electromagnetic wave shielding film. In addition, the porous inorganic particles tend to protrude from the adhesive layer, and the connection resistance value when the adhesive layer contacts the ground circuit described later tends to increase.
[0049] It should be noted that the particle size (D 50 ) can be measured using a laser diffraction particle size distribution measuring apparatus (SALD-2200 manufactured by Shimadzu Corporation).
[0050] In addition, the particle size (D 50 ) is measured in the same way.
[0051] In the electromagnetic wave shielding film of the present invention, it is preferred that the adhesive layer contains a conductive filler, and the particle size (D 50 ) is 4.0~30.0μm.
[0052] The adhesive layer contains the conductive filler, so that the adhesive layer functions as a conductive adhesive layer.50 ) When it is within the above range, the conductivity of the adhesive layer becomes good.
[0053] In the electromagnetic shielding film of the present invention, the adhesive layer preferably has a thickness of 5 to 50 μm.
[0054] When the thickness of the adhesive layer is less than 5 μm, the adhesiveness is reduced due to the thinness.
[0055] If the thickness of the adhesive layer exceeds 50 μm, the adhesive layer becomes thick, making it difficult to reduce the size of the electromagnetic shielding film.
[0056] In the electromagnetic shielding film of the present invention, the adhesive layer preferably contains 1 to 100 parts by weight of the porous inorganic particles based on 100 parts by weight of the resin.
[0057] When the content of the porous inorganic particles is within the above range, the hygroscopicity of the adhesive layer can be suitably reduced.
[0058] In the electromagnetic wave shielding film of the present invention, it is preferable that an insulating layer is further laminated on the shielding layer.
[0059] By forming the insulating layer, the shielding layer and the adhesive layer can be protected. In addition, by having the insulating layer, the shielding layer can be prevented from coming into contact with other conductive members.
[0060] Effects of the Invention
[0061] According to the present invention, it is possible to provide an electromagnetic wave shielding film in which the interlayer adhesion between the adhesive layer and the shielding layer is not easily damaged even when heated by reflow or the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 This is a cross-sectional view schematically showing an example of the electromagnetic shielding film of the present invention.
[0063] Figure 2 This is a cross-sectional view schematically showing an example of a shield printed circuit board using the electromagnetic shield film of the present invention.
[0064] Figure 3A This is an explanatory diagram schematically showing the mechanism of interlayer delamination between an adhesive layer and a metal layer when a shield printed wiring board is manufactured using a conventional electromagnetic wave shielding film.
[0065] Figure 3B This is an explanatory diagram schematically showing the mechanism of interlayer delamination between an adhesive layer and a metal layer when a shield printed wiring board is manufactured using a conventional electromagnetic wave shielding film. DETAILED DESCRIPTION
[0066] Hereinafter, the electromagnetic wave shielding film of the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and can be applied with appropriate changes within the scope of the gist of the present invention.
[0067] Figure 1 This is a cross-sectional view schematically showing an example of the electromagnetic shielding film of the present invention.
[0068] Figure 1 The electromagnetic wave shielding film 10 shown is formed by laminating an adhesive layer 20 , a shielding layer 30 laminated on the adhesive layer 20 , and a further insulating layer 40 located on the shielding layer 30 .
[0069] Furthermore, the adhesive layer 20 contains a resin and porous inorganic particles.
[0070] In the electromagnetic shielding film 10, the porous inorganic particles function as a filler, and thus the strength of the conductive adhesive is increased.
[0071] In the electromagnetic shielding film 10 , the porous inorganic particles have at least the following characteristics.
[0072] That is, the porous inorganic particles have at least one of the following characteristics: a pore volume of the porous inorganic particles exceeding 0.44 mL / g and being 1.80 mL / g or less, a specific surface area of the porous inorganic particles being 280 m 2 / g and below 700m 2 / g, and the average pore diameter of the pores of the porous inorganic particles is more than 2.5 nm and less than 26 nm.
[0073] Because porous inorganic particles have this characteristic, porous inorganic particles are not easy to absorb volatile components. Therefore, in the part with porous inorganic particles, volatile components are not absorbed. That is, by including porous inorganic particles, the hygroscopicity of the adhesive layer 20 as a whole is reduced. Therefore, in the electromagnetic wave shielding film 10, even if heated by reflow soldering, the interlayer adhesion of the adhesive layer 20 and the shielding layer 30 is not easy to be destroyed.
[0074] The reason why the porous inorganic particles are less likely to absorb volatile components when they have the above-mentioned characteristics will be described below.
[0075] When the pore volume of the porous inorganic particles is more than 0.44 mL / g and not more than 1.80 mL / g, the pores of the porous inorganic particles have an appropriate size and volatile components such as water are less likely to accumulate in the porous inorganic particles.
[0076] If the pore volume is 0.44 mL / g or less, the pores formed in the porous inorganic particles become smaller, and it becomes easier to exert capillary force. If the pores exert capillary force, volatile components become easier to accumulate in the pores, and the porous inorganic particles become easier to absorb volatile components. Therefore, the hygroscopicity of the adhesive layer as a whole becomes easier to improve.
[0077] If the pore volume exceeds 1.80 mL / g, the pores formed in the porous inorganic particles become larger, and the porous inorganic particles become brittle, making it difficult to improve the strength of the conductive adhesive.
[0078] The pore volume of the porous inorganic particles is preferably 0.80 mL / g to 1.80 mL / g, more preferably 1.00 mL / g to 1.80 mL / g, and more preferably 1.60 mL / g to 1.80 mL / g.
[0079] The pore volume of the porous inorganic particles can be measured by a nitrogen adsorption method using an elemental analyzer: Vari EL III (manufactured by Elementar Corporation). The same applies to the methods for measuring the specific surface area and average pore diameter described below.
[0080] The specific surface area of porous inorganic particles is 280m 2 / g and below 700m 2 / g, the pores of the porous inorganic particles have an appropriate size, and volatile components such as water are less likely to accumulate in the porous inorganic particles.
[0081] If the above specific surface area is less than 280m 2 / g, the pores formed in the porous inorganic particles become larger, and the porous inorganic particles become brittle. Therefore, it becomes difficult to improve the strength of the adhesive layer.
[0082] If the above specific surface area is 700m 2 / g or more, the pores formed in the porous inorganic particles become smaller, and it becomes easier to exert capillary force. If the pores exert capillary force, volatile components become easier to accumulate in the pores, and the porous inorganic particles become easier to absorb volatile components. Therefore, the hygroscopicity of the entire adhesive layer becomes easier to improve.
[0083] It should be noted that the specific surface area of the porous inorganic particles is preferably 280 m 2 / g and above and 500m 2 / g or less, more preferably 280m 2 / g and above 480m 2 / g or less, more preferably 280m 2 / g and above and 300m 2 / g or less.
[0084] When the average pore diameter of the porous inorganic particles is more than 2.5 nm and not more than 26 nm, the pores of the porous inorganic particles have an appropriate size and volatile components such as water are less likely to accumulate in the porous inorganic particles.
[0085] If the average pore size of the above-mentioned pores is less than 2.5 nm, the pores formed in the porous inorganic particles become smaller and become easier to exert capillary force. If the pores exert capillary force, volatile components become easier to accumulate in the pores, and the porous inorganic particles become easier to absorb volatile components. Therefore, the hygroscopicity of the entire adhesive layer becomes easier to improve.
[0086] If the average pore diameter of the pores exceeds 26 nm, the pores formed in the porous inorganic particles become larger, and the porous inorganic particles become brittle, thereby making it difficult to improve the strength of the conductive adhesive.
[0087] The average pore diameter of the porous inorganic particles is preferably 7 nm or more and 26 nm or less, more preferably 11 nm or more and 26 nm or less, and further preferably 21 nm or more and 26 nm or less.
[0088] In the electromagnetic shielding film 10 , the DBA value of the porous inorganic particles is preferably 50 meq / kg or more and less than 200 meq / kg, more preferably 50 to 175 meq / kg.
[0089] It is difficult to produce porous inorganic particles having a DBA value below 50 meq / kg.
[0090] When the DBA value is less than 200 meq / kg, the hydrophobicity becomes high and water becomes less likely to accumulate in the pores.
[0091] In the electromagnetic wave shielding film 10, the particle size (D 50 ) is preferably 1.0 to 20.0 μm, more preferably more than 2.5 μm and less than 15.0 μm, and even more preferably more than 2.5 μm and less than 10.0 μm.
[0092] The particle size of porous inorganic particles (D 50 ) is less than 1.0 μm, it becomes difficult to form pores of an appropriate size in the porous inorganic particles.
[0093] The particle size of porous inorganic particles (D 50 ) If it exceeds 20.0 μm, the adhesive layer becomes thick, making it difficult to miniaturize the electromagnetic wave shielding film. In addition, the porous inorganic particles tend to protrude from the adhesive layer, and the connection resistance value when the adhesive layer contacts the ground circuit described later tends to increase.
[0094] In the electromagnetic wave shielding film, the type of the porous inorganic particles is not particularly limited, and silica, alumina, and the like can be used.
[0095] Among these, silicon dioxide is preferred, and hydrophobized silicon dioxide is more preferred.
[0096] In the electromagnetic shielding film 10 , the adhesive layer 20 preferably contains 1 to 100 parts by weight of porous inorganic particles, more preferably 1 to 50 parts by weight, and even more preferably 1 to 30 parts by weight, based on 100 parts by weight of the resin.
[0097] When the content of the porous inorganic particles is within the above range, the hygroscopicity of the adhesive layer 20 can be suitably reduced.
[0098] In the electromagnetic wave shielding film 10, the material of the resin is not particularly limited, and thermoplastic resin compositions such as styrene resin compositions, vinyl acetate resin compositions, polyester resin compositions, polyethylene resin compositions, polypropylene resin compositions, imide resin compositions, amide resin compositions, acrylic resin compositions, and thermosetting resin compositions such as phenolic resin compositions, epoxy resin compositions, urethane resin compositions, melamine resin compositions, and alkyd resin compositions can be used.
[0099] The material of the resin may be one of these alone or a combination of two or more thereof.
[0100] In the electromagnetic shielding film 10 , the adhesive layer 20 may contain a conductive filler.
[0101] The adhesive layer 20 functions as a conductive adhesive layer by including a conductive filler. In this case, the adhesive layer 20 functions as a conductive adhesive layer.
[0102] The conductive filler is not particularly limited, and may be metal fine particles, carbon nanotubes, carbon nanofibers, metal fibers, or the like.
[0103] When the conductive filler is metal particles, the metal particles are not particularly limited and may be silver powder, copper powder, nickel powder, solder powder, aluminum powder, silver-coated copper powder obtained by silver-plating copper powder, particles of polymer particles, glass beads, etc. coated with metal, etc.
[0104] Among these, copper powder or silver-coated copper powder, which is available at low cost, is preferred from the viewpoint of economic efficiency.
[0105] The shape of the conductive filler is not particularly limited, and may be appropriately selected from spherical, flat, flaky, dendritic, rod-like, fibrous, and the like.
[0106] The particle size of the conductive filler (D 50 ) is preferably 4.0 to 30.0 μm, more preferably 4.0 to 20.0 μm.
[0107] The particle size of the conductive filler (D 50 ) When it is within the above range, the conductivity of the adhesive layer 20 becomes good.
[0108] In the electromagnetic shielding film 10 , when the adhesive layer 20 contains a conductive filler, the content of the conductive filler is preferably 5 to 900 parts by weight, more preferably 10 to 800 parts by weight, based on 100 parts by weight of the resin.
[0109] In addition, when it is desired to impart isotropic conductivity to the adhesive layer 20 , it is preferable to mix the conductive filler in an amount of 500 to 900 parts by weight based on 100 parts by weight of the resin.
[0110] When anisotropic conductivity is to be imparted to the adhesive layer 20 , it is preferred that the conductive filler be blended so as to contain 5 parts by weight or more and less than 500 parts by weight based on 100 parts by weight of the resin.
[0111] In the electromagnetic shielding film 10 , the thickness of the adhesive layer 20 is preferably 5 to 50 μm, more preferably 5 to 30 μm.
[0112] When the thickness of the adhesive layer is less than 5 μm, the adhesiveness is reduced due to the thinness.
[0113] If the thickness of the adhesive layer exceeds 50 μm, the adhesive layer becomes thick, making it difficult to reduce the size of the electromagnetic shielding film.
[0114] In the electromagnetic shielding film 10 , the adhesive layer 20 may contain, in addition to the resin and the porous inorganic particles, a curing accelerator, a thickener, an antioxidant, a pigment, a dye, a plasticizer, an ultraviolet absorber, a defoaming agent, a leveling agent, a filler, a flame retardant, a viscosity modifier, etc. as needed.
[0115] In the electromagnetic wave shielding film 10 , the shielding layer 30 is preferably formed of a metal layer.
[0116] In addition, the metal layer preferably contains at least one metal selected from the group consisting of copper, silver, gold, aluminum, nickel, tin, palladium, chromium, titanium and zinc. In addition, the metal layer may be formed of at least two alloys selected from these groups.
[0117] The shielding layer 30 formed of these metals can suitably shield electromagnetic waves.
[0118] In the electromagnetic wave shielding film 10 , when the shielding layer 30 is a metal layer, the metal layer may be a rolled metal foil, a metal-plated layer, or a metal vapor-deposited layer.
[0119] In the electromagnetic shielding film 10 , when the shielding layer 30 is formed of a metal layer, the thickness thereof is preferably 0.1 to 10 μm, more preferably 0.5 to 6 μm.
[0120] If the thickness of the shielding layer is less than 0.1 μm, the shielding layer is too thin, so the strength of the shielding layer is reduced. Therefore, the bending resistance is reduced. In addition, it becomes difficult to fully reflect and absorb electromagnetic waves, so the electromagnetic wave shielding properties are easily reduced.
[0121] If the thickness of the shielding layer exceeds 10 μm, the entire electromagnetic shielding film becomes thick and becomes difficult to handle.
[0122] In the electromagnetic wave shielding film 10 , the insulating layer 40 is not particularly limited as long as it has sufficient insulating properties and can protect the shielding layer 30 and the adhesive layer 20 , and is preferably composed of, for example, a thermoplastic resin composition, a thermosetting resin composition, an active energy ray-curable composition, or the like.
[0123] The thermoplastic resin composition is not particularly limited, and examples thereof include styrene resin compositions, vinyl acetate resin compositions, polyester resin compositions, polyethylene resin compositions, polypropylene resin compositions, imide resin compositions, and acrylic resin compositions.
[0124] The thermosetting resin composition is not particularly limited, and examples thereof include phenolic resin compositions, epoxy resin compositions, urethane resin compositions, melamine resin compositions, and alkyd resin compositions.
[0125] The active energy ray-curable composition is not particularly limited, and examples thereof include polymerizable compounds having at least two (meth)acryloyloxy groups in a molecule.
[0126] The insulating layer 40 may be composed of a single material or may be composed of two or more materials.
[0127] The insulating layer 40 may contain a curing accelerator, a tackifier, an antioxidant, a pigment, a dye, a plasticizer, an ultraviolet absorber, a defoaming agent, a leveling agent, a filler, a flame retardant, a viscosity modifier, an anti-blocking agent, and the like as needed.
[0128] The thickness of the insulating layer 40 is not particularly limited and can be appropriately set as needed, but is preferably 1 to 15 μm, and more preferably 3 to 10 μm.
[0129] If the thickness of the insulating layer 40 is less than 1 μm, it is too thin and thus becomes difficult to sufficiently protect the shielding layer 30 and the adhesive layer 20 .
[0130] If the thickness of the insulating layer 40 exceeds 15 μm, the insulating layer 40 is too thick, so the electromagnetic shielding film 10 becomes difficult to bend, and the toughness of the insulating layer 40 decreases. Therefore, it becomes difficult to use it for a member that requires bending resistance.
[0131] It should be noted that, in the electromagnetic wave shielding film of the present invention, an insulating layer may be formed as needed, or an insulating layer may not be formed.
[0132] Next, a shielded printed wiring board using the electromagnetic shielding film of the present invention will be described.
[0133] Figure 2 This is a cross-sectional view schematically showing an example of a shield printed circuit board using the electromagnetic shield film of the present invention.
[0134] Figure 2 The shield printed circuit board 1 shown is formed of a printed circuit board 50 and an electromagnetic wave shielding film 10 .
[0135] The printed wiring board 50 includes a base film 51 , a printed circuit 52 disposed on the base film 51 , and a cover layer 53 disposed so as to cover the printed circuit 52 .
[0136] In the printed circuit board 50 , the printed circuit 52 includes a ground circuit 52 a , and an opening 53 a for exposing the ground circuit 52 a is formed in the cover layer 53 .
[0137] In the shielded printed circuit board 1 , the electromagnetic wave shielding film 10 is disposed on the printed circuit board 50 so that the cover layer 53 is in contact with the adhesive layer 20 .
[0138] In the shield printed circuit board 1, the adhesive layer 20 fills the opening 53a of the cover layer 53 and contacts the ground circuit 52a. With such a configuration, the shielding property of the electromagnetic shield film 10 can be improved.
[0139] Example
[0140] Hereinafter, although the Example which demonstrates this invention more concretely is shown, this invention is not limited to these Examples.
[0141] (Example 1)
[0142] As the insulating layer, an insulating layer made of epoxy resin having a thickness of 5 μm was prepared.
[0143] Next, electroplating was performed on the insulating layer to form a copper layer with a thickness of 2.0 μm. It should be noted that the copper layer functions as a shielding layer.
[0144] Next, 100 parts by weight of a polyester thermosetting resin as a resin and silver-coated copper powder (particle size D50 40 parts by weight of quartz (0.5 μm) and 10 parts by weight of porous silica particles as porous inorganic particles were mixed to prepare the conductive adhesive of Example 1. The parameters such as the pore volume of the porous silica used are shown in Table 1.
[0145] Next, the adhesive layer was applied on the metal layer so as to have a thickness of 7 μm, thereby producing the electromagnetic shielding film of Example 1.
[0146] [Table 1]
[0147]
[0148] (Example 2) to (Example 9) and (Comparative Example 1) to (Comparative Example 4)
[0149] Electromagnetic shielding films of Examples 2 to 9 and Comparative Examples 1 to 3 were produced in the same manner as in Example 1 except that the porous inorganic particles shown in Table 1 were used.
[0150] Moreover, an electromagnetic shielding film of Comparative Example 4 was produced in the same manner as in Example 1 except that the porous inorganic particles were not used.
[0151] (Evaluation of the presence or absence of interlayer peeling)
[0152] The electromagnetic wave shielding films of each embodiment and each comparative example are arranged on a printed circuit board by heat pressing. Then, after the printed circuit board is placed in a constant temperature and humidity chamber at 30°C and 60% RH for 1 day, it is exposed to the temperature conditions during reflow soldering to evaluate the presence or absence of interlayer peeling. It should be noted that as the temperature condition during tinning, a maximum temperature of 288°C is set. In addition, the presence or absence of interlayer peeling is evaluated as follows: the printed circuit board with the shielding film attached is floated in the solder tank 3 times, and the presence or absence of expansion is evaluated by visual observation. Here, the case where no expansion occurs at all in the shielding film is recorded as "◎", the case where only a part of the shielding film expands is recorded as "0", and the case where expansion is obviously generated on the entire surface of the shielding film is recorded as "×". The results are shown in Table 1.
[0153] (Evaluation of temporary fixity)
[0154] The electromagnetic shielding films of the respective Examples and Comparative Examples were used to evaluate the adhesiveness in accordance with the following procedures.
[0155] Under the conditions of 0.5 Pa, 120 ° C, and 5 sec, each electromagnetic wave shielding film was squeezed onto the polyimide film substrate side of the copper-clad laminate (polyimide film substrate / adhesive layer / copper foil) and temporarily fixed. Afterwards, the electromagnetic wave shielding film was shaken by hand to evaluate the temporary fixity of the copper-clad laminate substrate by whether the electromagnetic wave shielding film fell off. The evaluation test was performed 10 times. The results are shown in Table 1.
[0156] In addition, the evaluation criteria are as follows.
[0157] 0: All samples did not fall off
[0158] △: Some samples did not fall off
[0159] ×: All samples can be seen falling
[0160] As shown in Table 1, in the electromagnetic shielding films of the respective Examples, interlayer delamination did not occur.
[0161] Description of Reference Numerals
[0162] 1 Shielded PCB
[0163] 10.510 electromagnetic wave shielding film
[0164] 20,520 Adhesive layer
[0165] 30,530 shielding layer
[0166] 40, 540 insulation layer
[0167] 50 PCB
[0168] 51 Basic film
[0169] 52 Printed Circuit
[0170] 52a Grounding circuit
[0171] 53 Overlay
[0172] 53a Opening
[0173] 560 Volatile components.
Claims
1. An electromagnetic wave shielding film, characterized in that: comprising an adhesive layer and a shielding layer laminated on the adhesive layer, The adhesive layer comprises a resin and porous inorganic particles, The pore volume of the porous inorganic particles exceeds 0.44 mL / g and is 1.80 mL / g or less.
2. An electromagnetic wave shielding film, characterized in that: comprising an adhesive layer and a shielding layer laminated on the adhesive layer, The adhesive layer comprises a resin and porous inorganic particles, The specific surface area of the porous inorganic particles is 280 m 2 / g and below 700m 2 / g.
3. An electromagnetic wave shielding film, characterized in that: comprising an adhesive layer and a shielding layer laminated on the adhesive layer, The adhesive layer comprises a resin and porous inorganic particles, The average pore diameter of the pores of the porous inorganic particles is more than 2.5 nm and is 26 nm or less.
4. The electromagnetic shielding film according to any one of claims 1 to 3, wherein The porous inorganic particles have a DBA value of 50 meq / kg or more and less than 200 meq / kg.
5. The electromagnetic wave shielding film according to any one of claims 1 to 4, wherein The particle size (D 50 ) is 1.0~20.0μm.
6. The electromagnetic shielding film according to any one of claims 1 to 5, wherein The adhesive layer contains a conductive filler, and the particle size (D 50 ) is 4.0~30.0μm.
7. The electromagnetic shielding film according to any one of claims 1 to 6, wherein The adhesive layer includes 1 to 100 parts by weight of the porous inorganic particles based on 100 parts by weight of the resin.
8. The electromagnetic shielding film according to any one of claims 1 to 7, wherein The thickness of the adhesive layer is 5 to 50 μm.
9. The electromagnetic wave shielding film according to any one of claims 1 to 8, wherein An insulating layer is further stacked on the shielding layer.
Citation Information
Patent Citations
Shield film, shielded printed wiring board, and method for manufacturing shield film
WO2013077108A1