Embolism system and preparation method thereof
By using ethylene-vinyl alcohol polymer and dimethyl sulfoxide-ethanol mixture as embolic agents, combined with appropriate packaging materials, the problem of easy solidification of liquid embolic agents is solved, maintaining liquid state at low temperatures, simplifying clinical use and The validity period is extended, stability and transportation convenience are improved.
Patent Information
- Application Number
- CN202410788580.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-22
AI Technical Summary
Due to the easy coagulation of DMSO, existing liquid embolic agents need to be heated and thawed for clinical use, resulting in increased equipment costs and prolonged surgical preparation time. In addition, repeated solidification and melting during long-term storage affect the quality.
Ethylene-vinyl alcohol polymer, contrast agent and dimethyl sulfoxide-ethanol mixture are used as embolic agents, combined with glass or plastic packaging containing side chain olefins, to lower the freezing point of DMSO and improve high and low temperature resistance, making the embolic agent more durable Keep liquid at low temperatures and avoid heating and thawing steps.
It enables the embolic agent to remain liquid under low temperature conditions, simplifying clinical use, reducing equipment requirements, extending the validity period, improving stability and transportation convenience, and avoiding the negative impact of solidification and melting on quality.
Smart Images

Figure CN118806969A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of medical technology, and in particular to an embolization system and a preparation method thereof. Background Art
[0002] Medtronic's Onyx liquid embolic system is used for embolization of peripheral and neurovascular diseases, including arteriovenous malformations and high-vascular aneurysms. The liquid embolic agent in this product is generally composed of ethylene-vinyl alcohol polymer, tantalum powder and dimethyl sulfoxide (DMSO). Since DMSO has good compatibility and good diffusion in the blood, it is a commonly used solvent for liquid embolic agents; in addition, liquid embolic agents are conventionally packaged in glass vials, because the high temperature resistance of glass materials can be adapted to dry heat sterilization or wet heat sterilization.
[0003] However, the freezing point of DMSO is 18.4°C, so the liquid embolic agent prepared with it as a solvent is easy to solidify during routine storage, which brings inconvenience to clinical use. For example, the Onyx liquid embolic system of Medtronic specifically mentions in the product manual that The vial should be dry-heated at 70-80℃ for at least 5 minutes and then shaken. The product instructions of the similar embolic agent LAVA also mention the storage conditions of the product. Before using LAVA, keep the product temperature between 19 and 24℃. If the product solidifies at a lower temperature, thaw it at room temperature before use. This shows that the easy solidification of DMSO requires that the heating and thawing of the product must be considered during clinical use. The operating room needs to be equipped with relevant heating equipment to solve the thawing problem, which not only increases the equipment costs of the hospital, but also the embolic agent needs to be restored to room temperature after heating, which will also extend the surgical preparation time accordingly. Summary of the invention
[0004] The object of the present invention is to provide an embolization system and a preparation method thereof. The embolization system provided by the present invention is not easy to solidify, thus avoiding the cumbersome step of heating the embolic agent when solidifying, and can meet clinical use more conveniently and quickly.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides an embolization system, comprising an embolic agent and a package for encapsulating the embolic agent; the raw materials for preparing the embolic agent include ethylene-vinyl alcohol polymer, a contrast agent and an organic solvent; the organic solvent is a dimethyl sulfoxide-ethanol mixture or dimethyl sulfoxide; the material of the package is glass or an olefin plastic containing a side chain;
[0007] When the organic solvent is a dimethyl sulfoxide-ethanol mixture, the material of the packaging is glass or an olefin plastic containing a side chain; when the organic solvent is dimethyl sulfoxide, the material of the packaging is an olefin plastic containing a side chain.
[0008] Preferably, the side chain is an alkyl group.
[0009] Preferably, the alkyl group is a C3-C7 cycloalkyl group or a C1-C3 chain alkyl group.
[0010] Preferably, the olefin plastic containing a side chain includes COP, CBC, COC or TPX.
[0011] Preferably, when the organic solvent is dimethyl sulfoxide and the packaging material is an olefin plastic containing a side chain, the embolic agent in the embolic system remains in liquid state at a temperature ≥ -20°C.
[0012] Preferably, the volume fraction of ethanol in the dimethyl sulfoxide-ethanol mixture is 0.5-30%.
[0013] Preferably, the volume fraction of ethanol in the dimethyl sulfoxide-ethanol mixture is recorded as C;
[0014] When the packaging material is an olefin plastic containing a side chain, the organic solvent is a dimethyl sulfoxide-ethanol mixture, and 0.5%≤C<5%, the embolic agent in the embolic system remains in liquid state at a temperature>-20°C;
[0015] When the packaging material is an olefin plastic containing a side chain, the organic solvent is a dimethyl sulfoxide-ethanol mixture, and 5%≤C≤30%, the embolic agent in the embolic system remains in liquid state at a temperature ≥-40°C.
[0016] Preferably, the volume fraction of ethanol in the dimethyl sulfoxide-ethanol mixture is recorded as C;
[0017] When the packaging material is glass, the organic solvent is a dimethyl sulfoxide-ethanol mixture, and 0.5%≤C<5%, the embolic agent in the embolic system remains in liquid state at a temperature>10°C;
[0018] When the packaging material is glass, the organic solvent is a dimethyl sulfoxide-ethanol mixture, and 5%≤C≤30%, the embolic agent in the embolic system remains in liquid state under the condition of temperature ≥0°C.
[0019] Preferably, the packaging comprises a vial or a syringe.
[0020] The present invention provides a method for preparing the embolization system described in the above technical solution, comprising the following steps:
[0021] The raw materials for preparing the embolic agent are mixed and then packaged in a package to obtain the embolic system.
[0022] The present invention provides an embolic system, comprising an embolic agent and a package for encapsulating the embolic agent; the raw materials for preparing the embolic agent include ethylene-vinyl alcohol polymer, contrast agent and organic solvent; the organic solvent is a dimethyl sulfoxide-ethanol mixture or dimethyl sulfoxide; the material of the package is glass or an olefin plastic containing a side chain; when the organic solvent is a dimethyl sulfoxide-ethanol mixture, the material of the package is glass or an olefin plastic containing a side chain; when the organic solvent is dimethyl sulfoxide, the material of the package is an olefin plastic containing a side chain. The present invention uses an olefin plastic containing a side chain, which can reduce the nucleation point of dimethyl sulfoxide, so that it is not easy to solidify at a lower temperature, and has good high and low temperature resistance (convenient to meet the requirements of low temperature storage and high temperature sterilization when preparing the embolic system); and the present invention can reduce the solidification point of dimethyl sulfoxide to a certain extent by introducing ethanol. The present invention uses an organic solvent formula and is packaged with suitable materials, so that the embolic agent can remain in a liquid state under low-temperature freezing conditions, solves the problem that conventional liquid embolic agents can only be stored under harsh storage conditions of 19-24°C, avoids the cumbersome steps of heating when the embolic agent solidifies, and can more conveniently and quickly meet clinical use and more safely adapt to transportation conditions; at the same time, it avoids the influence of repeated solidification and melting on the quality of the embolic agent, effectively improves the stability of the embolic agent, and thus prolongs the shelf life of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the DSC test result diagram of 100% pure DMSO;
[0024] Figure 2 This is a DSC test result diagram of 90% DMSO-10% ethanol solvent;
[0025] Figure 3 This is a diagram of the crystallization and dissolution process of DMSO in a glass dish;
[0026] Figure 4 A diagram showing the fixed shapes of the embolic agents prepared for samples No. 6 to 8. DETAILED DESCRIPTION
[0027] The present invention provides an embolization system, comprising an embolic agent and a package for encapsulating the embolic agent; the raw materials for preparing the embolic agent include ethylene-vinyl alcohol polymer, a contrast agent and an organic solvent; the organic solvent is a dimethyl sulfoxide-ethanol mixture or dimethyl sulfoxide; the material of the package is glass or an olefin plastic containing a side chain;
[0028] When the organic solvent is a dimethyl sulfoxide-ethanol mixture, the material of the packaging is glass or an olefin plastic containing a side chain; when the organic solvent is dimethyl sulfoxide, the material of the packaging is an olefin plastic containing a side chain.
[0029] In the prior art, conventional liquid embolic systems using DMSO as an organic solvent and glass as packaging material can only remain liquid at temperatures above 19°C. The freezing point of DMSO is 18.4°C, while the freezing point of anhydrous ethanol is -114.1°C, and anhydrous ethanol has good effectiveness and safety in clinical applications. Therefore, the present invention adds an appropriate amount of anhydrous ethanol to DMSO to form a mixed solvent, which can effectively increase the freezing point of pure DMSO and prevent DMSO from solidifying at room temperature. There is no need to perform heating and thawing operations during clinical use, which is simple and practical; and anhydrous ethanol is cheaper than DMSO, which is conducive to reducing costs. In addition, due to the different surface properties of glass and olefin plastics containing side chains, the crystallization behavior of DMSO will be affected. The glass surface provides more nucleation points, which promotes DMSO crystallization, while the surface of olefin plastics containing side chains is not conducive to nucleation, so that DMSO is not easy to solidify at temperatures below the normal freezing point, that is, it can remain liquid at low temperatures. Therefore, the embolization system provided by the present invention can solve the problem that DMSO is easy to solidify at room temperature, avoid the problem that heating and thawing are required for clinical use, and is easy to use, convenient to transport, and has long-term stability.
[0030] In addition, since the conventional liquid embolic system in the prior art uses DMSO as an organic solvent and the packaging material is glass, it can only remain in a liquid state above 19°C. Therefore, during the long-term storage of the product, it may be in a repeated solid-state and liquid state change of solidification and melting. The EVOH used in the embolic agent is a plastic material, which generally has relatively stable performance and a long shelf life. However, as a liquid embolic agent, it needs to maintain a dense sponge-like gel texture after solidification in clinical application to achieve an embolic effect. The present invention has found through specific experiments that after EVOH is in a long-term frozen solidification state, its molecular arrangement will change, the solidification state in water will change, the texture of the sponge-like colloid formed by solidification will become loose, and its mechanical properties will also decrease. Therefore, EVOH can be stored for a longer time in a liquid environment of an organic solvent, and maintain good mechanical properties, so that the embolic agent has a longer shelf life.
[0031] The embolization system provided by the present invention is described in detail below. In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art.
[0032] The embolic system provided by the present invention includes an embolic agent, and the raw materials for preparing the embolic agent include ethylene-vinyl alcohol polymer, contrast agent and organic solvent. In the present invention, the content of ethylene-vinyl alcohol polymer in the embolic agent is preferably 1-10wt%, more preferably 6-8wt%; the content of the contrast agent is preferably 1-30wt%, more preferably 10-30wt%, and further preferably 20-30wt%; the contrast agent preferably includes tantalum powder, bismuth trioxide or iodinated aryl compound, and the iodinated aryl compound is preferably iodinated aryl-modified polylactic acid (PLA), iodinated aryl-modified polycaprolactone (PCL), iodinated aryl-modified polymethyl methacrylate (PMMA) or iodinated aryl-modified polyethylene glycol (PEG); the compound providing the iodinated aryl preferably includes triiodobenzamide, triiodophenol or triiodobenzoic acid. In the present invention, the organic solvent is a dimethyl sulfoxide-ethanol mixture or dimethyl sulfoxide; the volume fraction of ethanol in the dimethyl sulfoxide-ethanol mixture is preferably 0.5-30%, specifically 0.5%, 1%, 5%, 10%, 15%, 20%, 25% or 30%.
[0033] The embolic system provided by the present invention includes a package for encapsulating the embolic agent, and the package preferably includes a vial or a syringe. In the present invention, the material of the package is glass or an olefin plastic containing a side chain. In the present invention, the glass is preferably borosilicate glass. In the present invention, in the olefin plastic containing a side chain, the side chain is preferably an alkyl group; the alkyl group is preferably a C3-C7 cycloalkyl group or a C1-C3 chain alkyl group; the olefin plastic containing a side chain preferably includes COP, CBC, COC or TPX.
[0034] The present invention selects a suitable packaging material according to the type of organic solvent, which can ensure that the embolic agent in the embolic system remains in liquid form within a wide temperature range, which is described in detail below.
[0035] In the present invention, when the organic solvent is dimethyl sulfoxide, the material of the packaging is an olefin plastic containing a side chain. Specifically, when the organic solvent is dimethyl sulfoxide and the material of the packaging is an olefin plastic containing a side chain, the embolic agent in the embolic system of the present invention remains in liquid form at a temperature ≥-20°C (in this case, the product has a shelf life of 4 to 5 years), and the specific storage temperature may be ≥-20°C, preferably ≥-10°C, and more preferably ≥0°C.
[0036] In the present invention, when the organic solvent is a dimethyl sulfoxide-ethanol mixture, the packaging material is glass or an olefin plastic containing a side chain. The volume fraction of ethanol in the dimethyl sulfoxide-ethanol mixture of the present invention will affect the state of the embolic agent, and thus have a certain impact on the storage temperature of the embolic system. In the present invention, the volume fraction of ethanol in the dimethyl sulfoxide-ethanol mixture is recorded as C. Specifically, when the material of the packaging is an olefin plastic containing a side chain, the organic solvent is a dimethyl sulfoxide-ethanol mixture, and 0.5%≤C<5%, the embolic agent in the embolic system remains in a liquid state at a temperature>-20°C (in this case, the product has a shelf life of 4 to 5 years), and the specific storage temperature may be ≥-20°C, preferably ≥-10°C, and more preferably ≥0°C; when the material of the packaging is an olefin plastic containing a side chain, the organic solvent is a dimethyl sulfoxide-ethanol mixture, and 5%≤C≤30%, the embolic agent in the embolic system remains in a liquid state at a temperature ≥-40°C (in this case, the product has a shelf life of 5 to 6 years), and the specific storage temperature may be ≥-40°C, preferably ≥-30°C, and more preferably ≥-20°C. When the material of the packaging is glass, the organic solvent is a dimethyl sulfoxide-ethanol mixture, and 0.5%≤C<5%, the embolic agent in the embolic system remains liquid at a temperature >10°C (in this case, the product shelf life is 2.5 to 3 years), and the specific storage temperature may be ≥10°C, preferably ≥15°C, and more preferably ≥25°C; when the material of the packaging is glass, the organic solvent is a dimethyl sulfoxide-ethanol mixture, and 5%≤C≤30%, the embolic agent in the embolic system remains liquid at a temperature ≥0°C (in this case, the product shelf life is 3 to 4 years), and the specific storage temperature may be ≥0°C, preferably ≥5°C, and more preferably ≥10°C.
[0037] The present invention provides a method for preparing the embolization system described in the above technical solution, comprising the following steps:
[0038] The raw materials for preparing the embolic agent are mixed and then packaged in a package to obtain the embolic system.
[0039] The present invention does not specifically limit the method for packaging the embolic agent in the package, and a method well known to those skilled in the art can be used. In the present invention, the packaging preferably includes sterilization, and the sterilization method is preferably moist heat sterilization; the moist heat sterilization conditions include: the temperature is preferably 110-130°C, specifically 110°C, 115°C, 121°C, 125°C, 128°C or 130°C; the time is preferably 15-60min, specifically 15min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min or 60min; the relative humidity is preferably 60-90%, specifically 60%, 65%, 70%, 75%, 80%, 85% or 90%.
[0040] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] The high temperature resistance and water absorption performance data of the materials used in the following examples are shown in Table 1.
[0042] Table 1 High temperature resistance and water absorption performance data of materials used in the examples
[0043]
[0044]
[0045] Examples 1 to 5 and Comparative Examples 1 to 4
[0046] The packaging of embolic agents using dimethyl sulfoxide (DMSO) as solvent was investigated by selecting different packaging materials:
[0047] Preparation of embolic agent: 6 g of ethylene-vinyl alcohol polymer (EVOH) was weighed and dissolved in 100 mL of pure DMSO, and then 30 g of tantalum powder was added as a contrast agent to obtain an embolic agent (in liquid state).
[0048] Take 3 mL of the above embolic agents and put them into the 9 packaging forms listed in Table 2, and perform the following steps:
[0049] Step 1: First, the embolic agents in different packages are screened for packaging compatibility. They are placed in a stability acceleration box at 55°C for 7 days and then taken out to observe the compatibility results between the inner wall of the package and the embolic agent.
[0050] Step 2: Place the embolic agent prepared in step 1 in a -20°C freezing environment (freezer layer) for 24 hours. After returning to room temperature, observe the state of the embolic agent in different packages.
[0051] Step 3: The embolic agent prepared in step 2 is placed in a -40°C freezing environment (ultra-low temperature refrigerator) for 7 days. After returning to room temperature, the state of the embolic agent in different packages is observed.
[0052] Table 2 Status of embolic agents packaged in different materials
[0053] Sample source Packaging Step 1 Step 2 Step 3 Example 1 COP Vials Good compatibility Keep it liquid Partial solidification Example 2 CBC vials Good compatibility Keep it liquid Partial solidification Example 3 CBC Syringe Good compatibility Keep it liquid Partial solidification Example 4 COC vials Good compatibility Keep it liquid Partial solidification Example 5 TPX Vials Good compatibility Keep it liquid Partial solidification Comparative Example 1 Glass Vials Good compatibility solidification / Comparative Example 2 Glass Syringe Good compatibility solidification / Comparative Example 3 PP Syringe Good compatibility solidification / Comparative Example 4 PC Syringe Packaging corrosion, precipitation / /
[0054] As shown in Table 2, after the treatment in step 1, PC (polycarbonate) has poor compatibility with DMSO and cannot be used as the packaging of embolic agents. By analogy, polyester materials (such as polyurethane, etc.) are also not suitable for the packaging of embolic agents, and no subsequent verification is performed. After the treatment in step 2, the embolic agents packaged in PP and glass all appeared in a crystalline solid state at -20°C, and no subsequent verification is performed. After the treatment in step 3, the embolic agents packaged in COP (cycloolefin polymer), CBC (cyclic block copolymer), COC (cycloolefin copolymer), and TPX (4-methylpentene polymer) remained liquid at -40°C, meeting the use requirements, and by analogy, the packaging of olefin plastic materials containing side chains may also meet the use requirements.
[0055] In addition, from the experimental results in Table 2, the different packaging forms of the same material in Example 2 and Example 3 have little effect on the state of the embolic agent, indicating that the main factor affecting the morphology of the embolic agent is the packaging material.
[0056] Examples 6 to 9 and Comparative Example 5
[0057] A series of mixed solutions of DMSO and anhydrous ethanol in different volume ratios were selected as solvents, as shown in Table 3, namely 100% pure DMSO solvent, 95% DMSO-5% ethanol solvent, 90% DMSO-10% ethanol solvent, 80% DMSO-20% ethanol solvent, and 70% DMSO-30% ethanol solvent. 3 mL of solvent was respectively transferred and packaged in glass vials. After being placed in a freezing environment of -20°C (freezer layer) for 24 hours, the solvents in different ratios all crystallized and solidified, and recovered to liquid state at room temperature, and the time required to recover to liquid state (i.e., thawing time) was recorded.
[0058] In addition, the corresponding freezing points of solvents with different ratios were detected using a differential scanning calorimeter (DSC). Figure 1 This is the DSC test result of 100% pure DMSO. Figure 2 This is the DSC test result diagram of 90% DMSO-10% ethanol solvent.
[0059] Table 3 Thawing time and freezing point of solvents with different ratios
[0060] Sample source Solvent type Thawing time (min) Freezing point(℃) Comparative Example 5 100% pure DMSO 89.6 18.35 Example 6 95% DMSO-5% ethanol solvent 31.2 9.11 Example 7 90% DMSO-10% ethanol solvent 19.8 4.58 Example 8 80% DMSO-20% ethanol solvent 11.4 2.29 Example 9 70% DMSO-30% ethanol solvent 4.6 -1.73
[0061] It can be seen from the data in Table 3 that as the volume fraction of anhydrous ethanol increases, the mixed solvent is less likely to crystallize. Even after crystallization in a frozen environment, it can be thawed in a very short time without heating. In addition, this embodiment tests the freezing point of solvents with different ratios. The results show that when the volume fraction of anhydrous ethanol is controlled within the range of 0 to 5%, the freezing point of the solvent is about above 10°C. It is speculated that the embolic agent obtained after adding EVOH and contrast agent tantalum powder can be stored in a liquid state at 10 to 25°C; when the volume fraction of anhydrous ethanol is controlled within the range of 5 to 30%, the freezing point of the solvent is above -1°C. It is speculated that the embolic agent obtained after adding EVOH and contrast agent tantalum powder can be stored in a liquid state at 0 to 10°C.
[0062] Figure 3 This is a diagram of the crystallization and dissolution process of DMSO in a glass dish. Specifically, under room temperature conditions, 2 mL of DMSO was taken into a glass dish, and the glass dish containing DMSO was placed on a HCS302 hot and cold table (-60 ~ 400 ° C), and the microscope lens was placed on the DMSO liquid surface to observe microscopic changes. The equipment temperature was set to -20 ° C, and DMSO gradually crystallized and solidified. After DMSO crystallized, the temperature was gradually raised to room temperature, and the DMSO crystals gradually melted. The microscope lens was used to observe the changes in the microscopic state of DMSO during the whole process. Figure 3 A, B, C and D are the process diagrams of DMSO gradually crystallizing and solidifying, and E and F are the process diagrams of DMSO gradually melting. Figure 3 As shown in Figure A, there is no obvious crystal structure in the system, indicating that DMSO is completely in a liquid state. Figure 3 As shown in Figure B, a small amount of crystals appeared in the system and began to precipitate from the solution, but the number was small and the shape was not obvious, indicating that this was the initial stage of DMSO crystallization. Figure 3 As shown in Figure C, the number of crystals in the system increases, and the crystal morphology gradually becomes clearer. Obvious crystal clusters can be seen, and the crystals begin to form larger and more ordered structures, indicating that this is the middle stage of the DMSO crystallization process. Figure 3 As shown in Figure D, a large number of DMSO crystals are formed, and the crystals are closely arranged, showing a high degree of order, indicating that this is the mature stage of the crystallization process, and the crystal structure is stable and clear. Figure 3 As can be seen from Figure E, the number of crystals in the system gradually decreases, indicating that the dissolution process has begun, that is, at this time, the DMSO crystals begin to dissolve. Figure 3As can be seen from Figure F, the number of crystals in the system further decreases and the solution becomes clear again, indicating that this is the final stage of DMSO crystal dissolution.
[0063] Examples 10 to 16 and Comparative Example 6
[0064] The embolic agent that is not easy to solidify is prepared by using vials or syringes made of olefin plastic materials containing side chains such as COP, CBC, COC, and TPX, and a mixed solvent of DMSO and anhydrous ethanol to lower the freezing point of DMSO.
[0065] Preparation of embolic agents: Weigh 0.6 g of EVOH and dissolve it in 10 mL of pure DMSO or a mixed solvent of DMSO and anhydrous ethanol, then add 3 g of tantalum powder as a contrast agent to prepare the embolic agents. Specifically, as shown in Table 4, the sample solvents of No. 1 and 5 are 95% DMSO-5% ethanol solvent, the sample solvents of No. 2 and 6 are 90% DMSO-10% ethanol solvent, the sample solvents of No. 3 and 7 are 70% DMSO-30% ethanol solvent, and the sample solvents of No. 4 and 8 are pure DMSO. Take 3 mL of the above 8 embolic agents and put them into the 8 packaging forms listed in Table 4, and sterilize them with wet heat for 30 minutes at a temperature of 121°C and a relative humidity of 80% to prepare the embolic agents.
[0066] By adjusting the two parameters of the present invention (i.e., solvent composition and packaging material) to conduct an orthogonal test, the accelerated stability is tested, the shelf life of the product under different combinations is obtained, and mechanical testing is performed by simulating the clinical preparation of sponge-like colloids to more rigorously and objectively evaluate the shelf life results of the obtained embolic agent.
[0067] Specifically, the embolic agents prepared in Examples 10 to 16 (corresponding to serial numbers 1 to 7) were placed under accelerated aging conditions at 55°C, and the product shelf life under the corresponding conditions was inferred by referring to the calculation formula of the accelerated aging test for medical devices (based on the Arrhenius reaction rate function). Then, the curing time and mechanical properties of the products after the accelerated aging experiment were tested to further prove the accuracy of the shelf life data, wherein the curing time and mechanical properties testing methods are as follows:
[0068] Solidification time detection: use a 1mL syringe with an 18G injection needle to draw 0.05mL of embolic agent, insert the injection needle 1cm below the surface of the saline solution, start timing from the time the syringe is pushed in until the embolic agent no longer flows in the saline solution, and calculate the solidification time.
[0069] Mechanical property testing: Take a plastic mold with a length of 5 cm and a diameter of 3 mm, inject the embolic agent into it, slowly put it into physiological saline, wait for the embolic agent to slowly solidify in the water to form a sample similar to the shape of the mold, clamp the sample vertically on the tensile testing machine, turn on the tensile testing machine to stretch the sample at a certain rate, and record the value of the sample when it is stretched to break.
[0070] The embolic agent prepared in Comparative Example 6 (corresponding to sequence number 8) was frozen at -40°C for 3 months, and then subjected to an accelerated aging experiment at 55°C according to the aforementioned method, and the curing time and mechanical properties of the product after the experiment were tested.
[0071] Table 4 Validation results of different combinations of embolic agents
[0072]
[0073] The embolic agents prepared in Examples 15 to 16 and Comparative Example 6 were placed in a soft rubber tube of fixed size and frozen in a -20°C refrigerator for 24 hours. The frozen and solidified rubber tube was taken out and placed in physiological saline. The DMSO in the embolic agent was slowly dissolved and the embolic agent was solidified to form a fixed shape. Figure 4 The fixed shape diagram of the embolic agents prepared in Examples 15 to 16 and Comparative Example 6, the sample numbers from top to bottom are 6, 7 and 8.
[0074] From the data in Table 4, it can be seen that the embolic agents prepared in different combinations in Examples 10 to 16 are in a liquid state under storage conditions. Compared with the embolic agent after freezing in Comparative Example 6, although the difference in the solidification time index is not large, in the process of preparing the embolic agent to fix the shape, the embolic agent prepared in Comparative Example 6 is a sponge-like colloid with no fixed shape (such as Figure 4 The mechanical performance indexes finally detected were also significantly lower than those in Examples 10 to 16, indicating the importance of the embolic agent remaining in liquid form during its validity period, which is also a guarantee for the effectiveness and safety of the embolic agent.
[0075] In addition, although the main embolic component of the embolic agent, EVOH, is a plastic material, it is generally believed that the material has good stability and a long shelf life. Some manufacturers believe that the shelf life can reach 2 to 3 years. However, the present invention has found that if the embolic agent is in a solidified state for a long time, even if the room temperature condition is restored, the solidification time of EVOH will not change much. However, if the embolic agent is solidified in water to simulate the clinical state, the longer the solidification time, the more irregular the sponge-like colloid formed after solidification. The mechanical properties of the sponge-like colloid are tested, and the mechanical properties index is significantly reduced (as shown in Table 4). This shows that EVOH is in a solidified state for a long time, which may cause changes in the solidified crystal state due to changes in molecular arrangement. This change may have little effect on the performance of plastic use (such as blown film), but there are still certain risks as an embolic agent for clinical use. The present invention makes the embolic agent remain liquid in a wide temperature range by adjusting the solvent ratio and selecting olefin plastic packaging containing side chains that hinder the solvent nucleation point, avoiding the influence of repeated solidification and melting on the quality of the embolic agent, and extending the shelf life of the embolic agent.
[0076] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An embolization system, characterized in that: It comprises an embolic agent and a package for encapsulating the embolic agent; the raw materials for preparing the embolic agent include ethylene-vinyl alcohol polymer, a contrast agent and an organic solvent; the organic solvent is a dimethyl sulfoxide-ethanol mixture or dimethyl sulfoxide; the material of the package is glass or an olefin plastic containing a side chain; When the organic solvent is a dimethyl sulfoxide-ethanol mixture, the material of the packaging is glass or an olefin plastic containing a side chain; when the organic solvent is dimethyl sulfoxide, the material of the packaging is an olefin plastic containing a side chain.
2. The embolization system according to claim 1, characterized in that: The side chain is an alkyl group.
3. The embolization system according to claim 2, characterized in that: The alkyl group is a C3-C7 cycloalkyl group or a C1-C3 chain alkyl group.
4. The embolization system according to any one of claims 1 to 3, characterized in that: The olefin plastics containing side chains include COP, CBC, COC or TPX.
5. The embolization system according to claim 1, characterized in that: When the organic solvent is dimethyl sulfoxide and the packaging material is an olefin plastic containing a side chain, the embolic agent in the embolic system remains in liquid state at a temperature ≥ -20°C.
6. The embolization system according to claim 1, characterized in that: The volume fraction of ethanol in the dimethyl sulfoxide-ethanol mixture is 0.5-30%.
7. The embolization system according to claim 6, characterized in that: The volume fraction of ethanol in the dimethyl sulfoxide-ethanol mixture is recorded as C; When the packaging material is an olefin plastic containing a side chain, the organic solvent is a dimethyl sulfoxide-ethanol mixture, and 0.5%≤C<5%, the embolic agent in the embolic system remains in liquid state at a temperature>-20°C; When the packaging material is an olefin plastic containing a side chain, the organic solvent is a dimethyl sulfoxide-ethanol mixture, and 5%≤C≤30%, the embolic agent in the embolic system remains in liquid state at a temperature ≥-40°C.
8. The embolization system according to claim 6, characterized in that: The volume fraction of ethanol in the dimethyl sulfoxide-ethanol mixture is recorded as C; When the packaging material is glass, the organic solvent is a dimethyl sulfoxide-ethanol mixture, and 0.5%≤C<5%, the embolic agent in the embolic system remains in liquid state at a temperature>10°C; When the packaging material is glass, the organic solvent is a dimethyl sulfoxide-ethanol mixture, and 5%≤C≤30%, the embolic agent in the embolic system remains in liquid state under the condition of temperature ≥0°C.
9. The embolization system according to claim 1, characterized in that: The packaging forms include vials or syringes.
10. The method for preparing the embolic system according to any one of claims 1 to 9, characterized in that: The following steps are involved: The raw materials for preparing the embolic agent are mixed and then packaged in a package to obtain the embolic system.