Degradable zinc-magnesium composite material, preparation method thereof and anastomosis nail prepared from composite material
Through the two-layer structure of zinc-magnesium composite material and process control, the problem of non-degradability and inconsistent degradation speed of existing staple materials is solved, the complete degradation of staples in the body and sufficient staple force are achieved, and the pain and pain of secondary surgery are avoided. Risk of infection.
Patent Information
- Application Number
- CN202410960315.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-22
AI Technical Summary
Existing staple materials are not degradable, causing long-term presence in the body, causing inflammatory reactions and making secondary surgeries difficult, and the degradation rate cannot meet the requirements of slow first and then fast.
It adopts a two-layer structure of degradable zinc-magnesium composite material. The outer layer is made of medically degradable pure zinc or zinc alloy, and the inner core is made of thread-shaped medically degradable pure magnesium or magnesium alloy. Through metallurgical combination and process control, it is achieved first slowly and then quickly. Degradation speed, combined with composite casting, extrusion, pass rolling, drawing and bending processes to prepare staples.
The staples are completely degraded in the body, and the degradation rate meets the ideal requirements. It is slow in the beginning and accelerated in the later stages, avoiding the pain of secondary surgery and the risk of infection. It also has sufficient staple force and biocompatibility.
Smart Images

Figure CN118807005A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of medical device technology and metal composite materials, and in particular to a degradable zinc-magnesium composite material, a preparation method thereof and anastomotic staples prepared from the composite material. Background Art
[0002] The stapler is a medical device that replaces manual suturing in clinical practice. It can quickly suture the skin or tissue with staples while removing the diseased tissue. It is similar to a stapler and is easy to operate. It sews quickly, is easy to operate, and has few side effects and surgical complications. Staples are similar to staplers. During operation, the stapler clamps the tissue to be stapled between the anvil and the staple magazine that are close to each other, pushes the staples out of the staple magazine, and after the staple tips penetrate the clamped tissue to be stapled, the staples are bent and deformed on the anvil forming groove on the anvil, bending the U-shaped or inverted trapezoidal staples into a B shape, achieving the surgical purpose of stapler tissue.
[0003] The materials of anastomotic staples currently used in clinical practice are mainly pure titanium and titanium alloys, which have the advantages of stable properties and excellent mechanical properties. However, due to their non-degradability, they will remain in the body permanently as foreign bodies, causing continuous inflammatory reactions in the surrounding tissues and having a certain impact on the patient's life after surgery. If a secondary operation is performed to remove the staples, it will cause pain to the patient and increase the cost of the operation and the risk of infection.
[0004] Patent CN 110537949 A discloses a stapler and a stapler with a specially designed nail tip structure, which can have more cutting edges, increase the sharpness of the nail into the human tissue, reduce the resistance encountered when the staple penetrates the human tissue, ensure the stable formation of the staple, and achieve a good anastomosis effect without causing bleeding from the wound, etc. However, the staple is made of non-degradable metal material and still needs a second operation to remove it.
[0005] Patent CN 117770898 A discloses an anastomotic staple with a nano-surface treatment and a preparation method thereof. After two guide nail heads at both ends of the stapler and two guide nail heads corresponding to the two nail bodies are formed into an anastomotic ring under the control of the stapler, the puncture slope at one end of the guide nail head is kept parallel to the stapler seat, so that the thinner part at one end of the guide nail head can be avoided as a structural part of the anastomotic ring, and the structure at the puncture slope does not need to have a high strength, which is simple and convenient. However, the anastomotic staple is made of non-degradable metal material and still needs a second operation to be removed.
[0006] Patent CN 116852043 A discloses a staple processing method and staples, which are made of magnesium alloy, avoiding drawing and forming, ensuring high strength and elongation; at the same time, the processed staples have a lower maximum stress after being implanted in the body, and have better structural stability. However, the staples degrade quickly.
[0007] The ideal clinical requirements for anastomotic staples include: (1) strong stapling force; (2) strong antibacterial properties and not prone to infection; (3) biodegradable, no need for secondary surgery to remove; (4) degradation speed that is slow at first and then fast. The degradation speed is slow within 12 months after implantation to ensure the recovery time of the patient's site, and then the degradation speed becomes faster, preferably completely degrading within 36 months.
[0008] According to the release conditions and staple force requirements of staples, the degradable material that can meet the requirements is degradable metal. Degradable metals include iron-based, magnesium-based and zinc-based materials. The degradation rate of iron-based materials is too slow, the degradation rate of magnesium-based materials is too fast, and the degradation rate of zinc-based materials is between iron-based and magnesium-based materials, which is suitable for staple applications. However, the degradation rate of a single zinc-based material tends to stabilize within 1 month, and it is difficult to meet the requirement of faster degradation after 3 months. Therefore, a new staple solution is urgently needed to meet the above requirements. Summary of the invention
[0009] The purpose of the present invention is to provide a degradable zinc-magnesium composite material, a preparation method of the composite material and an anastomotic staple prepared from the composite material. The anastomotic staple can be completely degraded and has a degradation speed that is slow at first and then fast; and at the same time has sufficient staple force.
[0010] In order to achieve the above object, the present invention adopts the following technical solutions:
[0011] A degradable zinc-magnesium composite material, the composite material has a two-layer structure, the outer layer (i.e., zinc layer) is made of medical degradable pure zinc or zinc alloy, and the inner core (i.e., magnesium core) is made of threaded medical degradable pure magnesium or magnesium alloy. The ratio of the outer layer to the inner core is calculated by volume percentage, the outer layer accounts for 30% to 50% of the total volume of the composite material, and the remainder is the inner core.
[0012] Optionally, the interface between the outer layer and the inner core is metallurgically bonded. The metallurgical bonding means that there is a Zn and Mg atomic interdiffusion layer with a thickness of ≤40 μm at the interface between the outer layer and the inner core.
[0013] Optionally, in the zinc alloy used for the zinc layer, the alloying elements other than zinc are selected from at least one of Mg, Mn, Ca, Li, and Ag, and the mass percentages of these alloying elements are: Mg 0.1% to 8%, Mn 0.1% to 5%, Ca 0.1% to 2%, Li 0.1% to 1%, Ag 0.1% to 4%, and the remainder is pure zinc. For example, when the zinc alloy is a zinc-magnesium alloy, the mass percentage of the magnesium element is 0.1% to 8%, and the remainder is pure zinc.
[0014] Optionally, in the magnesium alloy used in the magnesium core, the alloying elements other than magnesium are selected from at least one of Zn, Mn, Ca, Li, and Ag, and the mass percentages of these alloying elements are: Zn 0.1% to 5%, Mn 0.1% to 2%, Ca 0.1% to 1%, Li 0.1% to 35%, Ag 0.1% to 5%, and the remainder is pure magnesium. For example, when the magnesium alloy is a calcium-magnesium alloy, the mass percentage of the calcium element is 0.1% to 1%, and the remainder is pure magnesium.
[0015] Optionally, the degradation rate of the composite material in the human body environment is slow at first and then fast, and the degradation process is: ① the zinc layer degrades first, and its degradation rate is slow, specifically, the degradation rate is ≤0.2 mm / year, which can maintain the structural integrity and nailing force in the early stage of implantation; ② After the zinc layer degrades to expose the magnesium core, the magnesium core begins to degrade, and its degradation rate is ≥0.5 mm / year.
[0016] Optionally, the selection principle of the zinc-magnesium composite anastomotic staple is: before implantation, the room temperature tensile strength is ≥240 MPa, and the elongation is ≥15%.
[0017] The invention provides a method for preparing the degradable zinc-magnesium composite material, which comprises sequentially performing composite casting, extrusion, groove rolling, drawing, cutting and bending on the raw materials.
[0018] Furthermore, by regulating the thickness of the zinc layer and the size and structure of the magnesium core, the effect of regulating the slow degradation time period and the overall complete degradation time period is achieved. The specific method is as follows: ① For the magnesium core, the reaction rate is controlled by setting different thread outer diameters, inner diameters and pitches; ② At the same time, for the zinc layer, its thickness is adjusted so that the diameter of the zinc-magnesium composite wire for manufacturing the staples of the present invention is ≤0.6 mm.
[0019] Optionally, the composite casting comprises:
[0020] 1) Pure magnesium or magnesium alloy melt is poured into a mold to obtain a cylindrical magnesium ingot.
[0021] 2) The surface of the obtained magnesium ingot is threaded to obtain a magnesium core.
[0022] 3) Place a pure zinc or zinc alloy base at the bottom of the casting mold and fix the magnesium core obtained in step 2) in the center of the base.
[0023] 4) Casting pure zinc or zinc alloy melt into the casting mold of step 3) to obtain a cylindrical Zn-Mg composite material ingot with a zinc layer on the outside and a magnesium core on the inside.
[0024] 5) After heat treatment of the Zn-Mg composite material ingot obtained in step 4), the ingot surface oxide scale is removed by turning.
[0025] Optionally, in step 1), in an inert atmosphere of nitrogen or argon, pure magnesium or magnesium alloy is kept at 670-720°C until the raw materials are completely melted to obtain a pure magnesium or magnesium alloy melt, stirred with a stirring paddle for 5-10 min, allowed to stand for 3-5 min, and then cast at 690°C into a mold with a diameter of Φ50-80 mm to obtain a cylindrical magnesium ingot.
[0026] Optionally, in step 2), the outer diameter of the thread is 50-70 mm, the inner diameter is 30-40 mm, and the pitch is 5-15 mm. After processing, the magnesium core is pre-treated, and the pre-treatment includes grinding, degreasing, deashing, pickling, water washing, and drying. Optionally, a zinc layer is plated on the surface of the magnesium core after pre-treatment, the purpose of which is to prevent oxidation and make the magnesium inner core and the zinc outer layer metallurgically connected more tightly.
[0027] Optionally, in step 4), in an inert atmosphere of nitrogen or argon, pure zinc or zinc alloy is kept at 450-500°C until the raw material is completely melted to obtain a pure zinc or zinc alloy melt, stirred with a stirring paddle for 5-10 minutes, and after standing for 3-5 minutes, cast into the casting mold of step 3) at 480°C (optionally, during casting, air pressure is applied to the upper part of the mold to assist the flow of Zn liquid). A cylindrical Zn-Mg composite ingot is obtained.
[0028] Optionally, in step 5), the heat treatment temperature is 80-150° C. and the time is 2-12 hours.
[0029] Optionally, the extrusion comprises: extruding the ingot obtained by composite casting at 280-320° C. to obtain a rod with a diameter of 10-20 mm.
[0030] Optionally, the groove rolling includes:
[0031] 1) The size of the bar rolled by the groove type is Φ10 mm×60 mm and the surface oxide scale is removed.
[0032] 2) Preheat the rod at a temperature of 250-300 °C for 30 min.
[0033] 3) Take out the bar for rolling at a rolling temperature of 200-300°C, and pass through slots with sizes of 9.7 mm, 9.0 mm, and 8.2 mm in turn. After rolling one pass, rotate 90 degrees and enter another pass for rolling, and roll from left to right in sequence.
[0034] 4) After rolling, air cool the sample to room temperature.
[0035] Optionally, the drawing is a multi-pass cold drawing, and the diameter of the wire in each drawing pass is Φ1mm, 0.9mm, 0.8mm, 0.7mm, 0.65mm, and 0.6mm, respectively, to finally obtain a degradable zinc-magnesium composite wire.
[0036] Optionally, the cutting includes: cutting the drawn wire into a length of 3-6 mm.
[0037] Optionally, the bending includes: bending the cut wire material into a staple shape.
[0038] The present invention also provides a degradable zinc-magnesium composite staple, wherein the staple is made of the degradable zinc-magnesium composite material, the inner layer is a magnesium core, and the outer layer is a zinc layer. The staple comprises: a nail crown and two nail legs, the middle part of the nail legs is a bending part; and the ends of the nail legs are formed with nail tips.
[0039] The stapler maintains sufficient mechanical properties within 10 to 30 days, so that the wound does not break or crack, and the stapler itself does not break; it completely degrades after 3 to 6 months. According to the test of YY0245-2008 "General Technical Requirements for Staplers", the stapler of the present invention can withstand a pressure of ≥3.6 KPa without leakage or tearing.
[0040] The present invention has the following beneficial effects:
[0041] (1) The present invention provides a degradable layered zinc-magnesium composite material, the outer layer is pure zinc or zinc alloy, the core is pure magnesium or magnesium alloy, the ratio of pure zinc or zinc alloy to pure magnesium or magnesium alloy is calculated by volume percentage, pure zinc or zinc alloy accounts for 30% to 50% of the total volume of the material, and the remainder is pure magnesium or magnesium alloy. The composite material can adjust the slow degradation time period and the overall complete degradation time period by adjusting the thickness of the zinc layer and the size and structure of the magnesium core, so as to achieve the degradation rate requirement of slow at the beginning and fast at the end. The slow corrosion rate of the degradable layered zinc-magnesium composite material in the early stage is contributed by the good corrosion resistance of pure zinc or zinc alloy, and the material can ensure sufficient mechanical properties in this process. In the later stage, the bone tissue is about to heal, and the tissue itself can bear most of the mechanical properties. Therefore, even if the degradation rate of the implant material increases, it will not pose a safety hazard to the human body. The preparation process of the present invention is simple, the prepared ingot is dense, and the two metals of zinc and magnesium are metallurgically combined.
[0042] (2) The present invention uses a degradable zinc-magnesium composite material as the anastomosis staple material, which can be naturally degraded in the human body. There is no need to use an instrument to open the marking clip again and remove it in a second operation, thus avoiding the patient's pain and infection risks caused by a second operation.
[0043] (3) The present invention solves the problem that the degradation rate of zinc alloy is too slow and the degradation rate of magnesium alloy is too fast. The degradation rate is adjustable and meets the degradation rate requirements of the anastomotic staples.
[0044] (4) The alloy of the present invention does not contain any element that has toxic side effects on the human body and has good biocompatibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0046] Figure 1 It is a schematic diagram of the structure of the degradable zinc-magnesium composite stapler of the present invention;
[0047] Figure 2 It is a schematic structural diagram of the degradable zinc-manganese composite rod of the present invention;
[0048] Figure 3 It is a schematic diagram of the composite casting process of the degradable zinc-manganese composite rod of the present invention;
[0049] Figure 4 The present invention is a flow chart of the method for processing the degradable zinc-manganese composite anastomotic staple.
[0050] Reference numerals
[0051] 1. Inner core; 11. Thread structure;
[0052] 2. Outer layer;
[0053] 3. Nail crown;
[0054] 4. Nail the legs. DETAILED DESCRIPTION
[0055] The exemplary embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art.
[0056] Example 1
[0057] like Figure 1 As shown, this embodiment provides a medical degradable zinc-magnesium composite stapler, which is in an inverted trapezoidal shape and made of medical degradable zinc-magnesium composite metal. The stapler material has a two-layer structure, the inner core 1 (i.e., the magnesium core) is a threaded medical degradable pure magnesium or magnesium alloy, and the outer layer 2 (i.e., the zinc layer) is a medical degradable pure zinc or zinc alloy; the interface between the inner core 1 and the outer layer 2 is metallurgically bonded. The degradable zinc-magnesium alloy stapler of this embodiment is made of medical degradable zinc-magnesium composite metal. The zinc-magnesium composite metal has excellent mechanical properties, a degradation rate that meets medical requirements, and uniform corrosion, which avoids the problem that the existing inert titanium stapler needs to be removed by a second surgery. No secondary surgery is required for removal, which significantly reduces the patient's pain and medical expenses.
[0058] The medical degradable zinc-magnesium composite anastomotic staple of the present embodiment comprises a nail crown 3, both ends of which are nail legs 4; a bending portion is provided in the middle of the nail legs 4; and the nail tip is obtained by cutting the ends of the nail legs 4.
[0059] Preferably, the connection between the staple legs 4 and the staple crown 3 of the staple may adopt an arc transition structure.
[0060] Furthermore, the nail tip angle is 20° to 45°, so that the end of the formed staple is more conducive to puncturing the muscle and other tissues of the organism and anastomosing the wound.
[0061] Furthermore, the two nail tip sections of the anastomotic staple are symmetrically arranged to avoid tilting toward one side when implanted into a biological body, thereby ensuring the accuracy of the implantation position.
[0062] Furthermore, the bending of the zinc-magnesium composite wire includes a first bending and a second bending. The first bending is used to make the angle α between the two ends and the middle section of the zinc-magnesium composite wire be 90° to 105°, that is, the stapler is U-shaped as a whole after forming.
[0063] Furthermore, the second bending is used to make the angle β between the ends of the zinc-magnesium composite substrate and the position close to the middle section be 155° to 165°, that is, the ends of the two ends of the staples after forming are inclined toward the inner side. By setting the staple legs of the staples in two sections, the stress concentration problem of the staples after bending can be effectively reduced.
[0064] The anastomotic staple of the present invention is made of a medical degradable zinc-magnesium composite metal material.
[0065] Example 2
[0066] like Figure 2As shown: a degradable zinc-magnesium composite rod, the composite rod has an inner core 1 of a magnesium core, an outer layer 2 of a zinc layer, and a thread structure 11 processed on the inner core 1. The thread outer diameter of the inner core 1 is 50-70 mm, the inner diameter is 30-40 mm, and the pitch is 5-15 mm. The thickness of the outer layer 2 is 10-20 mm.
[0067] Example 3
[0068] like Figure 3 and 4 As shown, this embodiment provides a processing method for a degradable zinc-magnesium composite stapler, and the method is used to manufacture a degradable zinc-magnesium composite stapler, and the processing method includes composite casting, extrusion, hole rolling, drawing, cutting, and bending. This embodiment uses composite casting and hole rolling technology to process staplers. The zinc-magnesium composite rod obtained by composite casting can adjust the degradation speed autonomously. The zinc degradation speed is slow in the early stage, and the magnesium degradation speed is fast in the later stage, which can meet the use requirements of staplers. The zinc-magnesium composite rod obtained by hole rolling has high production efficiency and the rod diameter can be freely adjusted.
[0069] like Figure 3 and 4 As shown, the processing method of the degradable zinc-magnesium composite stapler comprises the following steps:
[0070] S1, the composite casting;
[0071] 1) In 10 -3 Under vacuum conditions of 1.377 Pa, argon protective atmosphere was introduced, and pure magnesium was kept at 700°C until the raw materials were completely melted to obtain a pure magnesium melt. The melt was stirred with a stirring paddle for 10 min, allowed to stand for 5 min, and then cast into a mold with a diameter of Φ 60 mm at 690°C to obtain a cylindrical magnesium ingot.
[0072] 2) The obtained magnesium ingot is threaded to obtain a magnesium core, with a thread outer diameter of 50 mm, an inner diameter of 30 mm, and a pitch of 5 mm. After processing, the magnesium core is pre-treated, including grinding, degreasing, deashing, pickling, water washing, and drying. Optionally, a zinc layer is plated on the surface of the pre-treated magnesium core, the purpose of which is to prevent oxidation and make the magnesium inner core and the zinc outer layer metallurgically connected more tightly.
[0073] 3) Place a pure zinc or zinc alloy base at the bottom of the casting mold and fix the processed magnesium core obtained in step 2) in the center of the base.
[0074] 4) In 10 -3Under the vacuum condition of 1000 Pa, an argon protective atmosphere is introduced, and the Zn-0.4Mn-0.2Mg material is kept at 450°C until the raw material is completely melted to obtain a Zn-0.4Mn-0.2Mg alloy melt, which is stirred with a stirring paddle for 10 minutes, and after standing for 5 minutes, is cast into the mold of step 3) at 480°C. During casting, air pressure is applied to the upper part of the mold to assist the flow of Zn liquid. A degradable layered Zn-Mg composite ingot with a cylindrical outer zinc layer and an inner magnesium core is obtained.
[0075] 5) The degradable layered Zn-Mg composite material ingot obtained in step 4) is heat treated at 150° C. for 10 h, and then the oxide scale on the surface of the ingot is removed by turning.
[0076] S2, extrusion, extruding the ingot obtained by composite casting at 300° C. into a rod with a diameter of 20 mm, to obtain a degradable layered Zn-Mg composite material rod with an outer zinc layer and an inner magnesium core in an extruded state.
[0077] S3. In the process, the size of the bar rolled in the pass is Φ10 mm × 60 mm and the surface oxide scale is removed. The bar is preheated before rolling at a temperature of 300 ° C for 30 min. After heat preservation, the bar is taken out for rolling at a rolling temperature of 300 ° C, and passes through slots of 9.7 mm, 9.0 mm, and 8.2 mm in size. After rolling one pass, it is rotated 90 degrees and enters another pass for rolling, and rolling is performed from left to right. After rolling, the sample is air-cooled to room temperature.
[0078] S4, the drawing is a multi-pass cold drawing, and the diameter of each drawing pass is Φ1mm, 0.9mm, 0.8mm, 0.7mm, 0.65mm, and 0.6mm, respectively. Finally, a degradable zinc-magnesium composite wire is obtained.
[0079] S5, the cutting, cutting the drawn wire into 5 mm pieces.
[0080] S6, bending, bending the cut wire material into a staple shape.
[0081] Example 4
[0082] A degradable zinc-magnesium composite stapler is prepared using the zinc-magnesium composite wire material of Example 3. The outer layer (i.e., zinc layer) is a Zn-0.4Mn-0.2Mg alloy, and the inner core (i.e., magnesium core) is a threaded pure magnesium. The stapler has a diameter of 0.6 mm, a zinc layer thickness of 0.1 mm, and a magnesium core thickness of 0.4 mm.
[0083] The room temperature tensile strength of the staple before implantation was 250 MPa, and the elongation was 15%. When immersed in simulated body fluid, the degradation rate of the zinc layer was 0.4 mm / year, and the degradation rate of the magnesium core was 0.8 mm / year. The staple was immersed in simulated body fluid for 3 months. The zinc layer degraded to the boundary depth with the magnesium core in 1 month, at which time the magnesium core was exposed to the solution environment and the degradation rate accelerated. The entire staple was completely degraded in 3 months. The composition of the simulated body fluid is shown in Table 1, which records the content of raw materials 1 to 10 in 1000 ml SBF buffer.
[0084] Table 1
[0085]
[0086] The overall degradation rate of the stapler is lower than that of biodegradable pure magnesium and magnesium alloys, but higher than that of biodegradable pure zinc and zinc alloys. It can provide a sufficiently long-lasting anastomotic force during wound healing, and will not remain in the human body for a long time due to too slow degradation.
[0087] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A degradable zinc-magnesium composite material, characterized in that: The composite material has a two-layer structure, the outer layer is made of medically biodegradable pure zinc or zinc alloy, and the inner core is made of threaded medically biodegradable pure magnesium or magnesium alloy; the ratio of the outer layer to the inner core is calculated by volume percentage, the outer layer accounts for 30% to 50% of the total volume of the composite material, and the remainder is the inner core.
2. The degradable zinc-magnesium composite material according to claim 1, characterized in that: The interface between the outer layer and the inner core is metallurgically bonded, that is, there is a Zn and Mg atomic interdiffusion layer with a thickness of ≤40 μm at the interface between the outer layer and the inner core.
3. The degradable zinc-magnesium composite material according to claim 1, characterized in that: In the zinc alloy used for the zinc layer, the alloying elements other than zinc are selected from at least one of Mg, Mn, Ca, Li, and Ag, and the mass percentages of these alloying elements are: Mg 0.1%-8%, Mn 0.1%-5%, Ca 0.1%-2%, Li 0.1%-1%, Ag 0.1%-4%, and the balance is pure zinc; Optionally, in the magnesium alloy used in the magnesium core, alloy elements other than magnesium are selected from at least one of Zn, Mn, Ca, Li, and Ag, and the mass percentages of these alloy elements are: Zn 0.1%~5%, Mn 0.1%~2%, Ca 0.1%~1%, Li 0.1%~35%, Ag 0.1%~5%, and the remainder is pure magnesium.
4. The method for preparing the degradable zinc-magnesium composite material according to any one of claims 1 to 3, characterized in that: The process includes composite casting, extrusion, hole rolling, drawing, cutting and bending of the raw materials in sequence.
5. The preparation method according to claim 4, characterized in that: The composite casting comprises: 1) pouring pure magnesium or magnesium alloy melt into a casting mold to obtain a cylindrical magnesium ingot; 2) performing thread processing on the surface of the obtained magnesium ingot to obtain a magnesium core; 3) placing a pure zinc or zinc alloy base at the bottom of the casting mold, and fixing the magnesium core obtained in step 2) in the center of the base; 4) casting pure zinc or zinc alloy melt into the casting mold of step 3) to obtain a cylindrical Zn-Mg composite material ingot, which has a zinc layer on the outside and a magnesium core on the inside; 5) After heat treatment of the Zn-Mg composite material ingot obtained in step 4), the ingot surface oxide scale is removed by turning.
6. The preparation method according to claim 5, characterized in that: In step 1), in an inert atmosphere of nitrogen or argon, pure magnesium or magnesium alloy is kept at 670-720° C. until the raw material is completely melted to obtain a pure magnesium or magnesium alloy melt, stirred with a stirring paddle for 5-10 min, allowed to stand for 3-5 min, and then cast at 690° C. into a mold with a diameter of Φ50-80 mm to obtain a cylindrical magnesium ingot; Optionally, in step 2), the outer diameter of the thread is 50-70 mm, the inner diameter is 30-40 mm, and the pitch is 5-15 mm; Optionally, in step 4), in an inert atmosphere of nitrogen or argon, pure zinc or zinc alloy is kept at 450-500° C. until the raw material is completely melted to obtain a pure zinc or zinc alloy melt, stirred with a stirring paddle for 5-10 min, allowed to stand for 3-5 min, and then cast into the casting mold of step 3) at 480° C. to obtain a cylindrical Zn-Mg composite material ingot; Optionally, in step 5), the heat treatment temperature is 80-150° C. and the time is 2-12 hours.
7. The preparation method according to claim 4, characterized in that: The extrusion comprises: extruding the ingot obtained by composite casting at 280-320° C. to obtain a rod with a diameter of 10-20 mm.
8. The preparation method according to claim 4, characterized in that: The groove rolling comprises: 1) The size of the bar rolled by the groove type is Φ10 mm×60 mm and the surface oxide scale is removed; 2) Preheat the rod to a temperature of 250-300 °C for 30 min; 3) Take out the bar for rolling at a rolling temperature of 200-300°C, and pass through slots with sizes of 9.7 mm, 9.0 mm, and 8.2 mm in sequence. After one pass of rolling, rotate 90 degrees and enter another pass for rolling, and roll from left to right in sequence; 4) After rolling, air cool the sample to room temperature.
9. The preparation method according to claim 4, characterized in that: The drawing is a multi-pass cold drawing, and the diameters of the wires in each drawing pass are Φ1mm, 0.9mm, 0.8mm, 0.7mm, 0.65mm, and 0.6mm respectively, and finally a degradable zinc-magnesium composite wire is obtained.
10. A degradable zinc-magnesium composite stapler, characterized in that: The material of the anastomotic staple is the degradable zinc-magnesium composite material described in any one of claims 1 to 3 or the degradable zinc-magnesium composite material prepared by the method described in any one of claims 4 to 9. The anastomotic staple comprises a nail crown and two nail legs, and the middle part of the nail legs is a bending part; the ends of the nail legs are formed with nail tips.
Citation Information
Patent Citations
Anastomosing nail and anastomat
CN110537949A
Processing method of anastomosis nail and anastomosis nail
CN116852043A
Surface nanocrystallization treated anastomosis nail and preparation method thereof
CN117770898A