Metal fire extinguishing agent and preparation method and application thereof

By modifying the core-shell structure of nano-TiO2 and liquid metal, combined with the trans-crystalline endotherm of nano-TiO2 and the heat transfer properties of liquid metal, the problem of extinguishing class D metal fires is solved, and efficient metal fire extinguishing effects are achieved, providing A novel fire extinguishing agent design and process.

CN118807167AActive Publication Date: 2024-10-22SOUTHWEAT UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410793632.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-22
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively extinguish Class D metal fires, such as fires caused by the burning of potassium, sodium, magnesium and other metals. Conventional fire extinguishing agents cannot meet their high temperatures and harmfulness, resulting in difficulty in extinguishing fires and the lack of mature Class D dry powder fire extinguishing systems.

Method used

A core-shell structure using modified nano-TiO2 as the core and liquid metal as the outer shell is used to design a metal fire extinguishing agent by utilizing the crystallization endotherm of nano-TiO2 and the excellent heat transfer properties of liquid metal. By coating the liquid metal in nano-TiO2 The outer surface prevents agglomeration, improves dispersion, and achieves efficient fire extinguishing.

Benefits of technology

It achieves effective fire extinguishing of Class D metal fires with simple process flow and low cost. It provides a new idea for efficient extinguishing of Class D metal fires and significantly improves the fire extinguishing effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807167A_ABST
    Figure CN118807167A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fire extinguishing materials, in particular to a metal fire extinguishing agent and a preparation method and application thereof. The metal fire extinguishing agent comprises modified nano TiO2 and liquid metal, wherein the outer surface of the modified nano TiO2 is at least partially coated with the liquid metal; the modified nano TiO2 comprises nano TiO2 and a surface modifier, the outer surface of the nano TiO2 is at least partially coated with the surface modifier, and the crystal form of the nano TiO2 is anatase. According to the metal fire extinguishing agent, the D-type metal fire extinguishing effect is achieved through crystal transformation and heat absorption of nano TiO2 and the excellent heat transfer property of liquid metal, and the fire extinguishing effect is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fire extinguishing materials, and in particular to a metal fire extinguishing agent and a preparation method and application thereof. Background Art

[0002] With the advancement of science and technology, metal materials such as potassium, sodium, aluminum, magnesium, and zinc are gaining more and more attention, and their application areas are constantly expanding. These metals can easily react violently with other substances to cause combustion or explosion, which is difficult and dangerous to extinguish. Some toxic substances will also be released during the combustion process, which places high demands on firefighting personnel and facilities. If foreign metal fire accidents occur frequently, it will cause serious casualties and economic losses.

[0003] At present, there are good solutions for extinguishing Class A, Class B, Class C fires, but there is no good solution for extinguishing Class D fires (such as fires caused by the combustion of metals such as potassium, sodium, and magnesium). Because metal fires have the characteristics of high combustion temperature and great fire hazards, conventional general-purpose fire extinguishing agents cannot be used. Class D fires are one of the more difficult fires to extinguish, so research on Class D fire extinguishing is very important.

[0004] Although there is an application market for Class D dry powder fire extinguishing agents, the necessary system design data has not been obtained due to insufficient depth of engineering application research. The dry powder fire extinguishing systems with more mature engineering applications are Class B and C dry powder fire extinguishing systems, and Class D dry powder fire extinguishing systems are not technically mature enough. With the development of domestic industry, it is now imperative to study how to extinguish metal fires efficiently.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The first object of the present invention is to provide a metal fire extinguishing agent, the fire extinguishing agent has a modified nano-TiO 2 The core-shell structure is made of liquid metal as the shell. 2 The heat absorption of crystal transformation and the excellent heat transfer properties of liquid metal can achieve the fire extinguishing effect of Class D metal fire.

[0007] The second object of the present invention is to provide a method for preparing the metal fire extinguishing agent as described above, which has a simple process flow, mild and easy-to-control reaction conditions, low production cost, and the prepared extinguishing agent has a good extinguishing effect on metal fires.

[0008] The third object of the present invention is to provide an application of the metal fire extinguishing agent as described above in extinguishing metal fires.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] A metal fire extinguishing agent comprising modified nano-TiO 2 and at least partially coated on the modified nano-TiO 2 Liquid metal on the outer surface;

[0011] The modified nano-TiO 2 Including nano-TiO 2 and at least partially coated with the nano-TiO 2 The surface modifier of the outer surface, the nano-TiO 2 The crystal form is anatase.

[0012] A method for preparing the metal fire extinguishing agent as described above comprises the following steps:

[0013] In modified nano-TiO 2 The outer surface of the product is coated with liquid metal to obtain the metal fire extinguishing agent.

[0014] An application of the metal fire extinguishing agent as described above in extinguishing metal fires.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] (1) The metal fire extinguishing agent provided by the present invention is modified nano-TiO 2 As the core, it is conducive to the coating of liquid metal. Liquid metal has excellent heat transfer properties, which is conducive to the transfer of external heat and is coated on nano-TiO 2 The outer surface of the nanomaterials can prevent agglomeration, making the fire extinguishing agent have better dispersion. 2 When the anatase type is transformed into the rutile type, the crystal transformation will absorb heat. When the fire is extinguished, the liquid metal transfers the external heat to the anatase type nano-TiO 2 , Anatase nano-TiO 2 The metal fire extinguishing agent provided by the present invention has a good fire extinguishing effect on Class D metal fires.

[0017] (2) The process of the method of the present invention is simple, the reaction conditions are mild and easy to control, the manufacturing cost is low, and the nano-TiO 2 The use of heat absorption during crystallization and the excellent heat transfer properties of liquid metal to extinguish fire provides a new idea for the design and research of Class D metal fire extinguishing agents. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 A schematic diagram of the structure of a metal fire extinguishing agent provided by an embodiment of the present invention;

[0020] Figure 2 This is a diagram showing the fire extinguishing effect of the metal fire extinguishing agent prepared in Example 5 of the present invention.

[0021] Reference numerals:

[0022] 1-Liquid metal; 2-Surface modifier; 3-Nano-TiO 2 . DETAILED DESCRIPTION

[0023] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0024] like Figure 1 The first aspect of the present invention provides a metal fire extinguishing agent, comprising modified nano-TiO 2 and at least partially coated on the modified nano-TiO 2 Liquid metal 1 on the outer surface;

[0025] The modified nano-TiO 2 Including nano-TiO 2 3 and at least partially coated with the nano-TiO 2 3. External surface modifier 2, the nano-TiO 2 The crystal form of 3 is anatase.

[0026] The metal fire extinguishing agent provided by the present invention has a modified nano-TiO 2 The core-shell structure is a liquid metal shell with a core as the core. The liquid metal has good thermal conductivity and is coated on the modified nano-TiO2 External preparation into a core-shell structure can improve the nano-TiO 2 The heat absorption of nano materials is easy to agglomerate, and the core-shell structure fire extinguishing agent has good dispersibility. The present invention mainly utilizes nano TiO 2 The heat absorption of crystal transformation (from anatase to rutile) and the excellent heat transfer performance of liquid metal can achieve the effect of extinguishing Class D metal fires. During the fire extinguishing, the external heat is transferred to the anatase nano-TiO through the liquid metal. 2 , nano-TiO 2 It absorbs the heat transferred by the liquid metal and transforms it into crystal, reducing the temperature of the burning metal to below the ignition point, thus extinguishing the fire.

[0027] In some specific embodiments of the present invention, the liquid metal includes an alloy composed of one or more of metal gallium, metal indium, and metal tin.

[0028] In some preferred embodiments of the present invention, the liquid metal includes gallium-based liquid metal, such as metal gallium, gallium-indium alloy, gallium-indium-tin alloy, etc. Gallium-based liquid metal has very low toxicity, very low vapor pressure at room temperature, and extremely high safety; and compared with common thermal interface materials, it has higher thermal conductivity and lower interface contact thermal resistance. The thermal conductivity of gallium-based liquid metal thermal interface materials is much higher than that of most commercially available thermal conductive silicone greases, showing excellent thermal conductivity, which is conducive to transferring external heat to nano-TiO 2 .

[0029] In some specific embodiments of the present invention, the surface modifier includes oleic acid and / or F2311 (an equimolecular copolymer of vinylidene fluoride and chlorotrifluoroethylene), and oleic acid and / or F2311 are used to treat nano-TiO 2 The purpose of modification is to allow the liquid metal to better cover the nano-TiO 2 , thereby improving the fire extinguishing effect.

[0030] In some preferred embodiments of the present invention, the surface modifier is oleic acid, and the nano-TiO 2 The prepared fire extinguishing agent has a better fire extinguishing effect on metal fires.

[0031] In some specific embodiments of the present invention, the nano-TiO 2 The particle size is 20-500 nm, for example, any point value among 20 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, and 500 nm, or a range value consisting of any two point values.

[0032] If the particle size is too small, it is difficult for the liquid metal to cover it; if the particle size is too large, the prepared powder is difficult to spray out. Therefore, it is necessary to reasonably control the size of nano-TiO 2 Particle size.

[0033] A second aspect of the present invention provides a method for preparing the metal fire extinguishing agent according to any one of the aforementioned embodiments, comprising the following steps:

[0034] In modified nano-TiO 2 The outer surface of the product is coated with liquid metal to obtain the metal fire extinguishing agent.

[0035] The method of the invention has a simple process flow, mild and easy-to-control reaction conditions, low manufacturing cost, and utilizes nano-TiO 2 The use of heat absorption during crystallization and the excellent heat transfer properties of liquid metal to extinguish fire provides a new idea for the design and research of Class D metal fire extinguishing agents.

[0036] In some specific embodiments of the present invention, in the modified nano-TiO 2 The method of coating the outer surface with liquid metal comprises the following steps:

[0037] Modified nano-TiO 2 The mixture is dispersed in a first solvent, the liquid metal is added, mixed evenly, and dried to obtain the mixture.

[0038] In some specific embodiments of the present invention, when preparing the fire extinguishing agent, the amount of liquid metal used accounts for 1:1 of the modified nano-TiO 2 The mass percentage of the dosage is 1%-10%, for example, any point value among 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or a range value consisting of any two point values.

[0039] Too much liquid metal will lead to too large core-shell structure particles, while too little will lead to uneven coating, which will affect the fire extinguishing performance of the fire extinguishing agent. It is necessary to reasonably control the liquid metal and modified nano-TiO 2 ratio to achieve better fire extinguishing effect.

[0040] In some specific embodiments of the present invention, the first solvent comprises ethanol, preferably anhydrous ethanol.

[0041] In some specific embodiments of the present invention, after adding the liquid metal, the mixing method includes stirring mixing and / or ultrasonic mixing.

[0042] In some specific embodiments of the present invention, the liquid metal is gallium-based liquid metal, preferably gallium-indium-tin alloy.

[0043] In some specific embodiments of the present invention, the mass ratio of gallium, indium and tin in the gallium-indium-tin alloy is 62.5-68:21.5-22:10-16, for example, 62.5:21.5:16, 68:22:10 and the like.

[0044] In some specific embodiments of the present invention, the method for preparing the gallium indium tin alloy comprises the following steps:

[0045] Gallium, indium and tin are placed in a reactor in proportion, heated and stirred to melt and mix, alkaline solution is added to wash away metal oxides such as gallium oxide, indium oxide and tin oxide on the surface of the liquid metal, and liquid metal is obtained by ultrasound.

[0046] In some specific embodiments of the present invention, when preparing the gallium indium tin alloy, heating is performed in a water bath at a temperature of 60-70°C.

[0047] In some specific embodiments of the present invention, the alkali solution includes at least one of a lithium hydroxide solution, a sodium hydroxide solution, a potassium hydroxide solution, a rubidium hydroxide solution, and a cesium hydroxide solution.

[0048] In some specific embodiments of the present invention, the concentration of the alkali solution is 0.5-5 mol / L.

[0049] In some specific embodiments of the present invention, the modified nano-TiO 2 The preparation method comprises the following steps:

[0050] Nano-TiO 2 and the surface modifier are dispersed in the second solvent, and after the reaction is completed, TiO 2 - modifier dispersion, TiO 2 - The modifier dispersion is dropped into the non-solvent, allowed to stand, filtered, and dried to obtain modified nano-TiO 2 .

[0051] In some specific embodiments of the present invention, nano-TiO 2 The method of dispersing the surface modifier into the second solvent includes ultrasonic dispersion and / or stirring dispersion.

[0052] In some embodiments of the present invention, TiO 2 -The preparation method of the modifier dispersion comprises the following steps: firstly, 2 Add it into the second solvent, disperse it by ultrasonication and stirring, then add the surface modifier, stir and react to obtain the product.

[0053] In some other embodiments of the present invention, TiO 2 -The preparation method of the modifier dispersion comprises the following steps: firstly, the surface modifier is dispersed in the second solvent by stirring, and then nano-TiO 2 , ultrasonic dispersion, stirring reaction, and the product is obtained.

[0054] In some specific embodiments of the present invention, when the surface modifier is oleic acid, the second solvent is cyclohexane and / or n-hexane; when the surface modifier is F2311, the second solvent is DMF (N,N-dimethylformamide) and / or DMAc (N,N-dimethylacetamide).

[0055] In some specific embodiments of the present invention, in the preparation of modified nano-TiO 2 When the surface modifier is used, the amount of nano-TiO 2 The mass percentage of the dosage is 1%-5%, for example, any value among 1%, 2%, 3%, 4%, 5% or a range consisting of any two values.

[0056] Surface Modifier and Nano-TiO 2 Too low a ratio will lead to nano-TiO 2 Uneven modification or too high a ratio will result in excessive modifier residue, making subsequent separation and removal inconvenient, which will affect the performance of the fire extinguishing agent.

[0057] In some specific embodiments of the present invention, when preparing TiO 2 - When the modifier dispersion is prepared, the reaction temperature is 50-60°C, for example, any value among 50°C, 52°C, 55°C, 58°C, 60°C, or a range consisting of any two values; the reaction time is 1-3h, for example, any value among 1h, 2h, 3h, or a range consisting of any two values; the heating method of the reaction process is preferably water bath heating.

[0058] In some specific embodiments of the present invention, the non-solvent includes ethanol and / or methanol, and the ethanol used is preferably anhydrous ethanol.

[0059] TiO 2 The purpose of dropping the modifier dispersion into the non-solvent is to use the solvent-non-solvent method to coat the surface modifier on the nano-TiO 2 Surface modification.

[0060] In some specific embodiments of the present invention, the volume ratio of the second solvent to the non-solvent is 1:2-1:30, for example, any point value among 1:2, 1:5, 1:10, 1:12, 1:15, 1:20, 1:25, 1:30 or a range value consisting of any two point values.

[0061] In some specific embodiments of the present invention, TiO 2 The rotation speed when the modifier dispersion is dripped into the non-solvent is 400-1200 rpm, for example, any point value among 400 rpm, 600 rpm, 800 rpm, 1000 rpm, 1200 rpm or a range value consisting of any two point values.

[0062] Use of the metal fire extinguishing agent described in any one of the aforementioned embodiments or the metal fire extinguishing agent prepared by the method for preparing the metal fire extinguishing agent described in any one of the aforementioned embodiments in extinguishing metal fires.

[0063] The following is a detailed description of some embodiments of the present invention in conjunction with specific examples. The raw materials used in the examples can be purchased from the market unless otherwise specified.

[0064] Example 1

[0065] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added and the mixture was stirred and mixed at 600 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0066] Nano-TiO 2 Modification: First, 0.5002g of nano-TiO with a particle size of 200nm was added 2 Add 15 mL of cyclohexane and disperse at 200 W ultrasonic for 10 minutes, stir and disperse at 600 rpm for 10 minutes to make it dispersed evenly, then add 0.0050 g of oleic acid (nano-TiO 2 1wt%), stirred at 600rpm in a 60℃ water bath for 2 hours, and finally dripped into 150mL of anhydrous ethanol at 400rpm while stirring to satisfy the volume ratio of cyclohexane to anhydrous ethanol of 1:10, and allowed to stand, filtered, and volatilized naturally to obtain modified nano-TiO 2 .

[0067] Preparation of metal fire extinguishing agent: 0.4621g modified nano-TiO 2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.0047 g of liquid metal to meet the requirements of liquid metal on the modified nano-TiO 2 The mass percentage of the modified nano-TiO was 1%, stirred at 600 rpm for 2 hours, ultrasonicated at 200 W for 3 times, each time for 5 minutes, and dried to obtain the modified nano-TiO 2 @Metal fire extinguishing agent with liquid metal core-shell structure.

[0068] Example 2

[0069] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added and the mixture was stirred and mixed at 600 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, about 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0070] Nano-TiO 2 Modification: First, 0.4997 g of nano-TiO with a particle size of 200 nm was added. 2 Add 15 mL of cyclohexane and disperse at 200 W ultrasonic for 10 minutes, stir and disperse at 600 rpm for 10 minutes to make it evenly dispersed, then add 0.0047 g of oleic acid (nano-TiO 2 1wt%), stirred at 600rpm in a 60℃ water bath for 2 hours, and finally dripped into 150mL of anhydrous ethanol at 400rpm while stirring to satisfy the volume ratio of cyclohexane to anhydrous ethanol of 1:10, and allowed to stand, filtered, and volatilized naturally to obtain modified nano-TiO 2 .

[0071] Preparation of metal fire extinguishing agent: 0.4592g modified nano-TiO 2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.0142 g of liquid metal to meet the requirements of liquid metal on the modified nano-TiO 2 The mass percentage of the modified nano-TiO was 3%, and the mixture was stirred at 600 rpm for 2 hours, accompanied by 200 W ultrasound for 3 times, each time for 5 minutes, and dried to obtain the modified nano-TiO 2 @Metal fire extinguishing agent with liquid metal core-shell structure.

[0072] Example 3

[0073] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added and the mixture was stirred and mixed at 600 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, about 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0074] Nano-TiO 2 Modification: First, 0.5004 g of nano-TiO with a particle size of 200 nm was added.2 Add 15 mL of cyclohexane and disperse at 200 W ultrasonic for 10 minutes, stir and disperse at 600 rpm for 10 minutes to make it dispersed evenly, then add 0.0052 g of oleic acid (nano-TiO 2 1wt%), stirred at 600rpm in a 60℃ water bath for 2 hours, and finally dripped into 150mL of anhydrous ethanol at 400rpm while stirring to satisfy the volume ratio of cyclohexane to anhydrous ethanol of 1:10, and allowed to stand, filtered, and volatilized naturally to obtain modified nano-TiO 2 .

[0075] Preparation of metal fire extinguishing agent: 0.4692g modified nano-TiO 2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.02470 g of liquid metal to meet the requirements of liquid metal on the modified nano-TiO 2 The mass percentage of the modified nano-TiO was 5%, and the mixture was stirred at 600 rpm for 2 hours, accompanied by 200 W ultrasound for 3 times, each time for 5 minutes, and dried to obtain the modified nano-TiO 2 @Metal fire extinguishing agent with liquid metal core-shell structure.

[0076] Example 4

[0077] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added and the mixture was stirred and mixed at 600 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, about 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0078] Nano-TiO 2 Modification: First, 0.4999 g of nano-TiO with a particle size of 200 nm was added. 2 Add 15 mL of cyclohexane and disperse at 200 W ultrasonic for 10 minutes, stir and disperse at 600 rpm for 10 minutes to make it dispersed evenly, then add 0.0152 g of oleic acid (nano-TiO 2 3wt%), stirred at 600rpm in a 60℃ water bath for 2 hours, and finally dripped into 150mL of anhydrous ethanol at 400rpm while stirring to satisfy the volume ratio of cyclohexane to anhydrous ethanol of 1:10, and allowed to stand, filtered, and volatilized naturally to obtain modified nano-TiO 2 .

[0079] Preparation of metal fire extinguishing agent: 0.4578g modified nano-TiO2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.0045 g of liquid metal to meet the requirements of liquid metal on the modified nano-TiO 2 The mass percentage of the mixture was 1%, and the mixture was stirred at 600 rpm for 2 hours, accompanied by 200 W ultrasound for 3 times, each time for 5 minutes, and dried to obtain modified nano-TiO 2 @Metal fire extinguishing agent with liquid metal core-shell structure.

[0080] Example 5

[0081] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added and the mixture was stirred and mixed at 600 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, about 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0082] Nano-TiO 2 Modification: First, 0.4993 g of nano-TiO with a particle size of 200 nm was added. 2 Add 15 mL of cyclohexane and disperse at 200 W ultrasonic for 10 minutes, stir and disperse at 600 rpm for 10 minutes to make it evenly dispersed, then add 0.0155 g of oleic acid (nano-TiO 2 3wt%), stirred at 600rpm in a 60℃ water bath for 2 hours, and finally dripped into 150mL of anhydrous ethanol at 400rpm while stirring to satisfy the volume ratio of cyclohexane to anhydrous ethanol of 1:10, and allowed to stand, filtered, and volatilized naturally to obtain modified nano-TiO 2 .

[0083] Preparation of metal fire extinguishing agent: 0.4635 g modified nano-TiO 2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.0142 g of liquid metal to meet the requirements of liquid metal on the modified nano-TiO 2 The mass percentage of the modified nano-TiO was 3%, and the mixture was stirred at 600 rpm for 2 hours, accompanied by 200 W ultrasound for 3 times, each time for 5 minutes, and dried to obtain the modified nano-TiO 2 @Metal fire extinguishing agent with liquid metal core-shell structure.

[0084] Example 6

[0085] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added, and the mixture was stirred and mixed at 60 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, about 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0086] Nano-TiO 2 Modification: First, 0.4999 g of nano-TiO with a particle size of 200 nm was added. 2 Add 15 mL of cyclohexane and disperse at 200 W ultrasonic for 10 minutes, stir and disperse at 600 rpm for 10 minutes to make it evenly dispersed, then add 0.0155 g of oleic acid (nano-TiO 2 3wt%), stirred at 600rpm in a 60℃ water bath for 2 hours, and finally dripped into 150mL of anhydrous ethanol at 400rpm while stirring to satisfy the volume ratio of cyclohexane to anhydrous ethanol of 1:10, and allowed to stand, filtered, and volatilized naturally to obtain modified nano-TiO 2 .

[0087] Preparation of metal fire extinguishing agent: 0.4594 g modified nano-TiO 2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.0246 g of liquid metal to meet the requirements of liquid metal in the modified nano-TiO 2 The mass percentage of the modified nano-TiO was 5%, and the mixture was stirred at 600 rpm for 2 hours, accompanied by 200 W ultrasound for 3 times, each time for 5 minutes, and dried to obtain the modified nano-TiO 2 @Metal fire extinguishing agent with liquid metal core-shell structure.

[0088] Example 7

[0089] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added and the mixture was stirred and mixed at 600 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, about 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0090] Nano-TiO 2 Modification: First, 0.5003g of nano-TiO with a particle size of 200nm was added2 Add 15 mL of cyclohexane and disperse at 200 W ultrasonic for 10 minutes, stir at 600 rpm for 10 minutes to make it dispersed evenly, then add 0.0262 g of oleic acid (nano-TiO 2 5wt%), stirred at 600rpm in a 60℃ water bath for 2 hours, and finally dripped into 150mL of anhydrous ethanol at 400rpm while stirring to satisfy the volume ratio of cyclohexane to anhydrous ethanol of 1:10, and allowed to stand, filtered, and volatilized naturally to obtain modified nano-TiO 2 .

[0091] Preparation of metal fire extinguishing agent: 0.4623g modified nano-TiO 2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.0047 g of liquid metal to meet the requirements of liquid metal on the modified nano-TiO 2 The mass percentage of the mixture was 1%, and the mixture was stirred at 600 rpm for 2 hours, accompanied by 200 W ultrasound for 3 times, each time for 5 minutes, and dried to obtain modified nano-TiO 2 @Metal fire extinguishing agent with liquid metal core-shell structure.

[0092] Example 8

[0093] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added and the mixture was stirred and mixed at 600 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, about 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0094] Nano-TiO 2 Modification: First, 0.5000g of nano-TiO with a particle size of 200nm was added 2 Add 15 mL of cyclohexane and disperse at 200 W ultrasonic for 10 minutes, stir and disperse at 600 rpm for 10 minutes to make it evenly dispersed, then add 0.0259 g of oleic acid (nano-TiO 2 5wt%), stirred at 600rpm in a 60℃ water bath for 2 hours, and finally dripped into 150mL of anhydrous ethanol at 400rpm while stirring to satisfy the volume ratio of cyclohexane to anhydrous ethanol of 1:10, and allowed to stand, filtered, and volatilized naturally to obtain modified nano-TiO 2 .

[0095] Preparation of metal fire extinguishing agent: 0.4614 g modified nano-TiO2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.0145 g of liquid metal to meet the requirements of liquid metal on the modified nano-TiO 2 The mass percentage of the modified nano-TiO was 3%, and the mixture was stirred at 600 rpm for 2 hours, accompanied by 200 W ultrasound for 3 times, each time for 5 minutes, and dried to obtain the modified nano-TiO 2 @Metal fire extinguishing agent with liquid metal core-shell structure.

[0096] Example 9

[0097] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added and the mixture was stirred and mixed at 600 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, about 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0098] Nano-TiO 2 Modification: First, 0.5001g of nano-TiO with a particle size of 200nm was added. 2 Add 15 mL of cyclohexane and disperse at 200 W ultrasonic for 10 minutes, stir at 600 rpm for 10 minutes to make it dispersed evenly, then add 0.0262 g of oleic acid (nano-TiO 2 5wt%), stirred at 600rpm in a 60℃ water bath for 2 hours, and finally dripped into 150mL of anhydrous ethanol at 400rpm while stirring to satisfy the volume ratio of cyclohexane to anhydrous ethanol of 1:10, and allowed to stand, filtered, and volatilized naturally to obtain modified nano-TiO 2 .

[0099] Preparation of metal fire extinguishing agent: 0.4665 g modified nano-TiO 2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.0253 g of liquid metal to meet the requirements of liquid metal on the modified nano-TiO 2 The mass percentage of the modified nano-TiO was 5%, and the mixture was stirred at 600 rpm for 2 hours, accompanied by 200 W ultrasound for 3 times, each time for 5 minutes, and dried to obtain the modified nano-TiO 2 @Metal fire extinguishing agent with liquid metal core-shell structure.

[0100] Example 10

[0101] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added and the mixture was stirred and mixed at 600 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, about 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0102] Nano-TiO 2 Modification: First, 0.0097 g of F2311 and 4 mL of DMF were stirred at 600 rpm for 1 hour, and 0.4997 g of nano-TiO with a particle size of 200 nm was added. 2 , ensuring that F2311 has nano-TiO 2 The mass percentage of F2311 in the mixture was 2%. After 10 minutes of ultrasound at 200W, the mixture was stirred at 600rpm in a 60℃ water bath for 2 hours. Finally, 60mL of anhydrous ethanol was added dropwise at a speed of 400rpm while stirring to satisfy a volume ratio of F2311 to anhydrous ethanol of 1:15. The mixture was allowed to stand, filtered, and evaporated naturally to obtain modified nano-TiO 2 .

[0103] Preparation of metal fire extinguishing agent: 0.5584 g modified nano-TiO 2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.0055 g of liquid metal to meet the requirements of liquid metal on the modified nano-TiO 2 The mass percentage of the mixture was 1%, and the mixture was stirred at 600 rpm for 2 hours, accompanied by 200 W ultrasound for 3 times, each time for 5 minutes, and dried to obtain modified nano-TiO 2 @Metal fire extinguishing agent with liquid metal core-shell structure.

[0104] Embodiment 11

[0105] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added and the mixture was stirred and mixed at 600 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, about 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0106] Nano-TiO 2Modification: First, 0.0103 g of F2311 and 4 mL of DMF were stirred at 600 rpm for 1 hour, and 0.5003 g of nano-TiO with a particle size of 200 nm was added. 2 , ensuring that F2311 has nano-TiO 2 The mass percentage of F2311 in the mixture was 2%. After 10 minutes of ultrasound at 200W, the mixture was stirred at 600rpm in a 60℃ water bath for 2 hours. Finally, 60mL of anhydrous ethanol was added dropwise at a speed of 400rpm while stirring to satisfy a volume ratio of F2311 to anhydrous ethanol of 1:15. The mixture was allowed to stand, filtered, and evaporated naturally to obtain modified nano-TiO 2 .

[0107] Preparation of metal fire extinguishing agent: 0.5624 g modified nano-TiO 2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.0185 g of liquid metal to meet the requirements of liquid metal on the modified nano-TiO 2 The mass percentage of the modified nano-TiO was 3%, and the mixture was stirred at 600 rpm for 2 hours, accompanied by 200 W ultrasound for 3 times, each time for 5 minutes, and dried to obtain the modified nano-TiO 2 @Metal fire extinguishing agent with liquid metal core-shell structure.

[0108] Example 12

[0109] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added and the mixture was stirred and mixed at 600 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, about 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0110] Nano-TiO 2 Modification: First, 0.0096 g of F2311 and 4 mL of DMF were stirred at 600 rpm for 1 hour, and 0.5000 g of nano-TiO with a particle size of 200 nm was added. 2 , ensuring that F2311 has nano-TiO 2 The mass percentage of F2311 in the mixture was 2%. After 10 minutes of ultrasound at 200W, the mixture was stirred at 600rpm in a 60℃ water bath for 2 hours. Finally, 60mL of anhydrous ethanol was added dropwise at a speed of 400rpm while stirring to satisfy a volume ratio of F2311 to anhydrous ethanol of 1:15. The mixture was allowed to stand, filtered, and evaporated naturally to obtain modified nano-TiO 2 .

[0111] Preparation of metal fire extinguishing agent: 0.5498g modified nano-TiO 2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.0291 g of liquid metal to meet the requirements of liquid metal on the modified nano-TiO 2 The mass percentage of the modified nano-TiO was 5%, and the mixture was stirred at 600 rpm for 2 hours, accompanied by 200 W ultrasound for 3 times, each time for 5 minutes, and dried to obtain the modified nano-TiO 2 @Metal fire extinguishing agent with liquid metal core-shell structure.

[0112] Comparative Example 1

[0113] Preparation of liquid metal: First, Ga / In / Sn was weighed in a ratio of 68:22:10, 6.7962 g of Ga and 2.2078 g of In were stirred and mixed at 600 rpm in a 70°C water bath for 20 minutes, 0.9976 g of Sn was added and the mixture was stirred and mixed at 600 rpm in a 70°C water bath for 40 minutes, 1 mol / L NaOH solution was prepared, about 10 mL of NaOH solution was added to the above metal mixture, and ultrasonicated at 200 W for 5 minutes to obtain liquid metal.

[0114] Preparation of metal fire extinguishing agent: 0.5005g of nano-TiO with a particle size of 200nm 2 Add 20 mL of anhydrous ethanol, stir and disperse at 600 rpm for 20 minutes, then add 0.0155 g of liquid metal to meet the requirement of liquid metal in nano-TiO 2 The mass percentage of the mixture was 3%, and the mixture was stirred at 600 rpm for 2 hours, with 200 W ultrasound for 3 times, each time for 5 minutes, and dried. No nano-TiO 2 @Liquid metal core-shell structure complex.

[0115] Comparative Example 2

[0116] The difference between Comparative Example 2 and Example 4 is that liquid metal coating is not performed, and the other conditions are the same as those of Example 4, that is, 3 wt% oleic acid-modified nano-TiO 2 As a fire extinguishing agent.

[0117] Test example

[0118] The fire extinguishing performance of the fire extinguishing agents prepared in each embodiment and each comparative example was tested, and the test method and test conditions were as follows:

[0119] A magnesium strip with a size of 120 mm × 1.3 mm × 0.2 mm was spread flat, and 5 g of the prepared fire extinguishing agent was evenly spread on the magnesium strip. The strip was ignited with a Ni-Cr wire, and the length of the remaining magnesium strip after the combustion was completed was measured. Each sample was tested 3 times, and the average value was calculated. The longer the remaining unburned length, the better the fire extinguishing effect. The test results are shown in Table 1.

[0120] Table 1

[0121]

[0122]

[0123] It can be seen from the data in Table 1 that the metal fire extinguishing agent prepared by the method of the present invention has a good fire extinguishing effect; Figure 2 This is a fire extinguishing effect diagram of the fire extinguishing agent prepared in Example 5 of the present invention. After covering the fire extinguishing agent prepared in this example, the 12 cm magnesium strip burns, and the remaining unburned magnesium strip can reach a length of 10 cm, while the magnesium strip (12 cm) without the fire extinguishing agent is completely burned, showing an excellent fire extinguishing effect.

[0124] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A metal fire extinguishing agent, characterized in that: It comprises modified nano-TiO2 and liquid metal at least partially coated on the outer surface of the modified nano-TiO2; The modified nano-TiO2 comprises nano-TiO2 and a surface modifier at least partially coated on the outer surface of the nano-TiO2. The crystal form of the nano-TiO2 is anatase.

2. The metal fire extinguishing agent according to claim 1, characterized in that: The liquid metal includes an alloy composed of one or more of metal gallium, metal indium and metal tin.

3. The metal fire extinguishing agent according to claim 1, characterized in that: The surface modifier includes oleic acid and / or F2311.

4. The metal fire extinguishing agent according to claim 1, characterized in that: The particle size of the nano-TiO2 is 20-500nm.

5. The method for preparing the metal fire extinguishing agent according to any one of claims 1 to 4, characterized in that: The following steps are involved: The metal fire extinguishing agent is obtained by coating the surface of the modified nano-TiO2 with liquid metal.

6. The method for preparing a metal fire extinguishing agent according to claim 5, characterized in that: The method for coating liquid metal comprises the following steps: The modified nano-TiO2 is dispersed in a first solvent, and the liquid metal is added, mixed, and dried to obtain the product.

7. The method for preparing a metal fire extinguishing agent according to claim 6, characterized in that: Contains at least one of the following characteristics: (1) The mass percentage of the liquid metal to the modified nano-TiO2 is 1%-10%; (2) The first solvent includes ethanol.

8. The method for preparing a metal fire extinguishing agent according to claim 5, characterized in that: The preparation method of the modified nano-TiO2 comprises the following steps: The nano-TiO2 and the surface modifier are dispersed in a second solvent, and after the reaction is completed, a TiO2-modifier dispersion is obtained. The TiO2-modifier dispersion is dropped into a non-solvent under stirring, allowed to stand, filtered, and dried to obtain the modified nano-TiO2.

9. The method for preparing a metal fire extinguishing agent according to claim 8, characterized in that: Contains at least one of the following characteristics: (1) When the surface modifier is oleic acid, the second solvent includes cyclohexane and / or n-hexane; when the surface modifier is F2311, the second solvent includes DMF and / or DMAc; (2) The mass percentage of the surface modifier to the nano-TiO2 is 1%-5%; (3) The reaction temperature is 50-60° C. and the reaction time is 1-3 h; (4) The non-solvent comprises ethanol and / or methanol; (5) the volume ratio of the second solvent to the non-solvent is 1:2-1:30; (6) The rotation speed when dropping the TiO2-modifier dispersion into the non-solvent is 400-1200 rpm.

10. Use of the metal fire extinguishing agent according to any one of claims 1 to 4 in extinguishing metal fires.

Citation Information

Patent Citations

  • Metal surface cross-linked protective film

    CN107674479A

  • Preparation method of flame-retardant composition based on titanium dioxide

    CN107952201A

  • Liquid metal flame-retardant Be-containing titanium alloy for 500-1200 degrees

    CN109136650A

  • Fire extinguishants

    GB1596045A

  • Fire extinguisher for metal fire and its production