Preparation method and application of self-assembled carboxyl type cationic membrane

Through the preparation of in-situ self-assembled carboxyl-type cationic membranes on the surface of PVDF, the problem of poor recovery performance of powdered MOFs in liquid phase separation is solved, and high selectivity and stability of rare earth ions are achieved, making it suitable for industrial applications.

CN118807480AActive Publication Date: 2024-10-22UNIV OF SCI & TECH OF CHINA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410798141.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-22
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

Powdered metal-organic framework materials are difficult to recycle in liquid phase separation and have poor recycling performance. The existing MOFs composite membrane is unevenly attached to the carrier, resulting in insufficient stability and mechanical strength, limiting its large-scale application.

Method used

The MIL-101-NH2 type MOFs material was prepared using a solvothermal method, and functional groups with specific recognition properties were introduced through post-modification, and then grafted onto the surface of PVDF activated with acrylic acid through in-situ self-assembly to form self-assembled carboxyl groups type cationic membrane, which enhances the chemical bond between MOFs and the membrane.

Benefits of technology

It achieves high selectivity and recyclability of rare earth ions, improves the stability and application potential of the membrane, and the preparation method is simple and easy to implement, suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807480A_ABST
    Figure CN118807480A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a self-assembled carboxyl type cationic membrane, and the preparation method comprises the following preparation steps: firstly, preparing an MIL-101-NH2 type MOFs material by adopting a solvothermal method, and then carrying out post-modification on MIL-101-NH2 type MOFs through small molecules containing functional groups with specific recognition characteristics on rare earth ions, so as to obtain the self-assembled carboxyl type cationic membrane. And then, grafting the carboxyl cation membrane to the PVDF surface activated by acrylic acid in an in-situ self-assembly manner to obtain the self-assembled carboxyl cation membrane. The self-assembled carboxyl type cationic membrane prepared by the invention shows relatively good selectivity, rejection rate and stability to rare earth elements in the waste FCC catalyst, the rejection rate of the composite membrane can reach 95% within 30 minutes in a simulated acid leaching solution with the pH value of 6, the rejection efficiency can still be kept at 90% or above after four times of recycling, and the membrane is simple to prepare, controllable in cost and suitable for industrial production. A new thought is provided for efficient recycling of solid waste resources, and the method has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method of a self-assembled carboxyl type cationic membrane and application thereof in efficient separation, extraction and utilization of rare earth elements in waste FCC catalysts, belonging to the field of membrane preparation and application. Background Art

[0002] Rare earth elements are considered to be key strategic resources necessary for the development of high-tech industries. However, the reserves of rare earth elements are scarce and unevenly distributed worldwide. Therefore, the search, discovery and extraction of rare earth elements are of great strategic significance to the development of national science and technology industries. Fluid catalytic cracking (FCC) catalysts are important catalysts in the petrochemical industry. They are used in huge quantities, and tens of thousands of tons of such catalysts are discarded every year. Waste FCC catalysts use alumina as a carrier and rare earth elements as catalytic active ingredients. The rare earth content is about 2%, and it is rich in metal elements with recycling value such as lanthanum and cerium. The rational and comprehensive utilization of this waste catalyst can not only realize the secondary recycling of valuable metal elements, thereby protecting the environment, but also meet the national policy requirements for the scientific treatment of hazardous solid wastes, and at the same time have good economic, environmental and social benefits.

[0003] Metal-organic framework materials (MOFs) have the advantages of high porosity, low density, large specific surface area, regular pores, adjustable pore size, topological structure diversity and easy modification, which makes them have important applications in the fields of gas storage, chemical separation, sensing, etc. Introducing some specific functional groups into MOFs materials can not only improve the adsorption performance and hydrophilicity of MOFs, but also improve their ion selectivity. However, powdered metal organic framework materials are difficult to recover in liquid phase separation and have poor recycling performance, which limits their large-scale application. Membrane separation technology has become a new separation technology that integrates high efficiency, environmental protection and precision. It is easy to operate and cost-controlled, and is more suitable for industrial applications. MOF composite membranes have attracted widespread attention for their good selectivity and high adsorption performance. The characteristics of MOFs materials that are easy to modify and have adjustable pore size provide guarantees for the efficient and selective separation of MOF membranes. By enhancing the interaction between guest molecules and multifunctional metal central ions or organic ligands, the separation performance of the membrane is improved and the applicability of MOFs materials is broadened. Most of the existing MOFs composite membranes are based on metal oxides or tubular objects, and MOFs particles are large, so it is difficult to form a continuous growth trend on such supports, and it is impossible to ensure that the membrane has good mechanical strength attached to the carrier. Polyvinylidene fluoride (PVDF) is an organic polymer material with unique advantages, showing high thermal stability, mechanical strength and chemical inertness. Its superiority as a membrane material is reflected in its easy film formation, simple preparation process, low cost and convenience for large-scale manufacturing. It is one of the most promising porous polymer membranes and is widely used in ultrafiltration, microfiltration and separation and concentration. In recent years, membranes based on PVDF have been successively applied to oil-water separation and metal ion separation (including heavy metals, rare earth metals and platinum group metals). The application of MOFs materials in the field of organic / inorganic hybrid membranes can effectively improve the compatibility of hybrid particles and polymer membranes. The introduction of synthesized post-modified MOFs with specific recognition properties into PVDF membranes can not only improve the separation performance and stability of the composite membrane, but also improve the adsorption specificity of PVDF membranes for rare earth ions and improve the adsorption performance. However, the PVDF-MOFs composite membranes reported so far are usually prepared by blending. Since MOFs particles are large, they are unevenly dispersed and have weak interaction forces after blending with PVDF, which makes them unstable and affects their performance. Therefore, the key to overcoming this problem is to first modify the PVDF carrier and then prepare the MOFs membrane by chemical bonding. Summary of the invention

[0004] In order to improve the problem that powdered metal organic framework materials are difficult to recover and have poor recycling performance in liquid phase separation, the technical problem to be solved by the present invention is to provide a self-assembled carboxyl cationic membrane that is easy to produce and prepare and has specific selectivity and recyclability for rare earth ions, aiming to produce chemical bonds between the MOFs material and the substrate, making the connection tighter and the resulting membrane more uniform.

[0005] The technical solution of the present invention to solve the above technical problems is as follows:

[0006] The present invention firstly discloses a method for preparing a self-assembled carboxyl type cationic membrane, which is characterized in that: firstly, a solvent thermal method is used to prepare MIL-101-NH 2 type MOFs materials, and then MIL-101-NH 2 The MOFs were post-modified and then grafted onto the surface of PVDF activated by acrylic acid by in-situ self-assembly to obtain a self-assembled carboxyl cationic membrane. The results showed that the membrane had good selectivity, retention rate and recyclability for rare earth ions, indicating that the self-assembled carboxyl cationic membrane prepared by the present invention had good stability and practical application potential in the recovery of rare earth ions.

[0007] Preferably, the method for preparing the self-assembled carboxyl type cationic membrane comprises the following steps:

[0008] 1) Add chromium nitrate, 2-aminoterephthalic acid and sodium hydroxide to water, stir at room temperature to mix them thoroughly, transfer the resulting solution to a stainless steel reactor, and keep the reaction at 150-200°C for 12-36 hours. After the reaction is completed, centrifuge and filter the resulting reaction solution, wash with DMF and ethanol solution in turn, and dry in a vacuum oven at 60°C-80°C to obtain green MIL-101-NH 2 Type MOFs material powder.

[0009] 2) MIL-101-NH obtained in step 1) 2 The MOFs material was mixed with small molecules containing functional groups with specific recognition characteristics for rare earth ions, and then N,N-dicyclohexylcarbodiimide (DCC) was added, and DMF was added as solvent. 2 After the reaction, the obtained reactant was centrifuged, washed with anhydrous ethanol for 3-5 times, and dried at 60-80°C for 6-12h to obtain a green powdery post-modified MIL-101-NH 2 Type MOFs.

[0010] 3) Immerse the PVDF powder in the AIBN acetone solution, stir evenly, add acrylic acid, and 2 The reaction was carried out at 50-100°C for 4-8 hours under protection to generate a large number of carboxyl groups on its surface; after the reaction, the post-modified MIL-101-NH obtained in step 2) was added to the reaction solution. 2After stirring for 30-60 min, the porogen PPA was added and the reaction was continued in an oil bath at 50℃-80℃ for 12-24 h to make the post-modified MIL-101-NH 2 The MOFs are grafted onto the PVDF surface by in-situ self-assembly, so that a chemical bond is generated between the MOFs material and the membrane, making the connection tighter. The obtained casting solution is ultrasonically degassed for 1-3 hours, and a film is pushed on a clean glass plate with a film casting device according to a certain thickness, and then the glass plate is immediately placed steadily in deionized water. After the film automatically falls off, the glass plate is taken out, and the fallen film is soaked in water for 24-48 hours to obtain a self-assembled carboxyl cationic membrane.

[0011] Preferably, the small molecule containing a functional group with specific recognition characteristics for rare earth ions is N-(phosphonomethyl) methylenediacetic acid hydrate, referred to as PMIDA, and the prepared post-modified MOFs are PMIDA-M1N type MOFs particles (abbreviated as PMIDA-M1N). 2 The MOFs were post-modified to introduce abundant phosphate groups.

[0012] Preferably, in step 1), the molar ratio of chromium nitrate, 2-aminoterephthalic acid and sodium hydroxide is 1:(1-1.2):(1-2).

[0013] Preferably, in step 2), the MIL-101-NH 2 The molar ratio of type MOFs material, small molecule, and N,N-dicyclohexylcarbodiimide is 1:(1-1.5):(1-2).

[0014] Preferably, in step 3), PVDF, AIBN, acrylic acid, PPA and post-modified MIL-101-NH 2 The dosage ratio of type MOFs is 4g:(0.5-2)g:(2-4)mL:(0.2-0.8)g:(2-4)g.

[0015] Preferably, in step 3), the thickness of the push film is 20-100 μm.

[0016] The self-assembled carboxyl type cationic membrane prepared by the preparation method can be used for rare earth element recovery, especially for efficient separation, extraction and utilization of rare earth elements in waste FCC catalysts.

[0017] The beneficial effects of the present invention are:

[0018] (1) In the self-assembled carboxyl-type cationic membrane prepared by the present invention, a chemical bond is generated between the MOFs material and the membrane, the connection is tighter, and the membrane is more uniform;

[0019] (2) The preparation method of the self-assembled carboxyl cationic membrane of the present invention is simple and easy to operate, the raw materials used are cheap, and it can be produced in large quantities, which is suitable for industrial application;

[0020] (3) The composite membrane prepared by the present invention has specific selectivity for rare earth ions and has good stability and recyclability. In addition, the membrane material obtained by the present invention can not only exert the chelation effect of the functional group on rare earth ions and the pore size screening of MOFs on ions, but also make full use of the high efficiency and green environmental protection advantages of membrane separation. The material can be used in the separation process of rare earth ions and has unique advantages in practical application. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A schematic diagram of the preparation process of a self-assembled carboxyl-type cationic membrane of the present invention;

[0022] Figure 2 This is the XRD analysis diagram of the self-assembled carboxyl type cationic membrane prepared in Example 1 of the present invention;

[0023] Figure 3 is an infrared spectrum of the self-assembled carboxyl type cationic membrane prepared in Example 1 of the present invention;

[0024] Figure 4 The SEM analysis of the self-assembled carboxyl-type cationic membrane prepared in Example 1 of the present invention, wherein a is the surface SEM analysis of PMIDA-M1N@PVDF, and b is the cross-sectional analysis of the membrane;

[0025] Figure 5 This is a chemical stability analysis diagram of the self-assembled carboxyl-type cationic membrane prepared in Example 1 of the present invention;

[0026] Figure 6 ion selectivity analysis diagram of the self-assembled carboxyl-type cationic membrane prepared in Example 1 of the present invention;

[0027] Figure 7 The effect of the thickness of the self-assembled carboxyl type cationic membrane prepared in Example 1 of the present invention on the rejection rate and water flux;

[0028] Figure 8 This is a recycling analysis diagram of the self-assembled carboxyl type cationic membrane prepared in Example 1 of the present invention;

[0029] Fig. 9 This is an XRD stability analysis diagram of the self-assembled carboxyl cationic membrane prepared in Example 1 of the present invention after recycling, wherein a is the structure of PMIDA-M1N, b is the structure of PMIDA-M1N@PVDF before recycling, and c is the structure of PMIDA-M1N@PVDF after recycling. DETAILED DESCRIPTION

[0030] In order to more fully understand the present invention, this embodiment describes the present invention in more detail through the following non-limiting examples or comparative examples, and provides detailed implementation methods and specific operating processes, but the protection scope of the present invention is not limited to the following examples.

[0031] Example 1: Preparation of self-assembled carboxyl-type cationic membrane

[0032] 1) MIL-101-NH 2 Preparation of MOFs: Chromium nitrate, 2-aminoterephthalic acid and sodium hydroxide were added to water in a molar ratio of 1:1:2, stirred at room temperature for 30 minutes to fully mix, and the resulting solution was transferred to a stainless steel reactor and kept at 150°C for 12 hours. After the reaction was completed, the resulting reaction solution was centrifuged and filtered, washed with DMF and ethanol solution in turn, and dried in a vacuum oven at 60°C for 12 hours to obtain green MIL-101-NH 2 Type MOFs material powder, named M1N.

[0033] 2) PMIDA post-modification of MIL-101-NH 2 Preparation of MOFs: MIL-101-NH 2 The MOFs material, PMIDA (N-(phosphonomethyl) methylenediacetic acid hydrate), and DCC (N,N-dicyclohexylcarbodiimide) were added into a three-necked flask at a molar ratio of 1:1.5:2, and DMF was added as solvent. 2 Under protection, the reaction was carried out at 150°C for 48 hours. When the reaction was completed, the reactant was separated by centrifugation, washed with anhydrous ethanol 4 times, and dried in a vacuum drying oven at 60°C for 6 hours to obtain a green powder product named PMIDA-M1N.

[0034] 3) Prepare the self-assembled carboxyl cationic membrane by in situ self-assembly method: 4 g of dry PVDF powder was immersed in 10 mL of acetone solution containing 1.8 g of AIBN in a three-necked flask and stirred for 30 min; then 3 mL of acrylic acid (AA) was added to the flask and stirred under N 2 The reaction was carried out in an oil bath at 70°C for 5 hours under the protection of a flask. After the reaction, 3g of PMIDA-M1N was added to the three-necked flask, and 0.6g of porogen PPA was added after stirring for 30 minutes. The mixture was stirred in an oil bath at 60°C for 24 hours to form a uniform casting solution. The casting solution was ultrasonically degassed for 1 hour, and a film was cast on a clean glass plate with a film casting device according to a certain thickness (20-100μm). Then, the glass plate was immediately placed steadily in deionized water. After the film automatically fell off, the glass plate was taken out, and the fallen film was soaked in water for 48 hours to obtain PMIDA-M1N@PVDF cationic membrane.

[0035] Example 2: Characterization of self-assembled carboxyl-type cationic membranes

[0036] The XRD analysis of PMIDA-M1N@PVDF ion membrane prepared in Example 1 is as follows: Figure 2 As shown, a is M1N, b is PMIDA-M1N, and c is PMIDA-M1N@PVDF membrane. After PMIDA-M1N and PVDF are formed into a film, the characteristic diffraction peaks are consistent with those of MOFs materials, indicating that the composite membrane made by this method does not damage the crystal structure of MOFs materials, preliminarily proving the successful preparation of PMIDA-M1N@PVDF.

[0037] The FT-IR analysis of the PMIDA-M1N@PVDF cationic membrane prepared in Example 1 is as follows: Figure 3 As shown in the figure, from the comparison of a, b, and c, it can be seen that the characteristic peak of PVDF CF bond appears at 1400cm -1 and 1180cm -1 , respectively -CF 2 The deformation vibration peak and stretching vibration peak are 875cm -1 It is the characteristic absorption peak of the amorphous region of polyvinylidene fluoride. From the comparison between PMIDA-M1N MOFs material and PMIDA-M1N@PVDF cationic membrane, it can be seen that the MOFs material has been successfully grafted with the PVDF membrane.

[0038] The SEM image of PMIDA-M1N@PVDF cationic membrane prepared in Example 1 is as follows: Figure 4 As shown by Figure 4 a It can be seen that PMIDA-M1N@PVDF cationic membrane has a good porous structure. Figure 4 The cross-sectional view of b shows that there are through holes inside the membrane. The cross-linked structure generated between the substrate and MOF can greatly enhance the hardness and compressive resistance of the fiber, which can be regarded as an ion transmission channel, indicating that PMIDA-M1N@PVDF cationic membrane has good ion transmission potential.

[0039] The chemical stability analysis of PMIDA-M1N@PVDF cationic membrane prepared in Example 1 is as follows Figure 5 As shown, the composite membrane was cut into the same size and immersed in acid or alkaline solutions of pH 2, 4, 6, 8, 10, and 12 for 12 hours respectively. After being taken out and dried, XRD scanning was performed. It can be clearly seen that there are characteristic diffraction peaks of MOFs at 2θ=8-10° and characteristic diffraction peaks of PVDF near 2θ=20°. The PMIDA-M1N@PVDF cationic membrane material can maintain a complete crystal structure under different acid and alkaline conditions and has good chemical stability and structural stability.

[0040] Example 3: Application of PMIDA-M1N@PVDF cationic membrane

[0041] Example 1 Analysis of ion selectivity of PMIDA-M1N@PVDF cationic membrane prepared: In order to understand the selectivity of the synthesized composite membrane to rare earth ions La and Ce, a simulated acid leaching solution of spent FCC catalyst (K + , Ca 2+ 、Zn 2+ ,La 3+ 、Ce 3+ 、Ni 3+ , Fe 3+ The concentrations of La and Ce are 15.85 mg / L and 1.995 mg / L respectively, and K + , Ca 2+ 、Zn 2+ 、Ni 3+ , Fe 3 + The concentrations were 38.06mg / L, 84.08mg / L, 13.09mg / L, 15.79mg / L, 15.79mg / L), respectively. Test K + , Ca 2+ 、Zn 2 + ,La 3+ 、Ce 3+ 、Ni 3+ , Fe 3+ The retention of ions through the low-pressure membrane flux tester is as follows: Figure 6 As shown, the ordinate is the separation coefficient β, and the calculation formula is shown in formula (1) and (2):

[0042]

[0043]

[0044] Where R is the ion retention rate of the membrane, C 0 is the initial concentration of the ion, C is the equilibrium concentration after interception, β A / B is the separation coefficient of ion A to B, obtained by comparing the retention rates of the two. Figure 6 It can be seen that among these metal ions, PMIDA-M1N@PVDF cationic membrane has the highest 3+ The interception rate of 3+ , and the third is Fe 3+ , the separation coefficients β of La, Ce and coexisting ions all follow β La / Zn >β La / Ca >β La / K >β La / Ni >βLa / Fe The order of the maximum separation factor for Zn ions can reach 31.9. The results show that PMIDA-M1N@PVDF cationic membrane can effectively separate the rare earth element La in the acid leaching simulation solution of the spent catalyst. 3+ 、Ce 3+ It has good separation selectivity.

[0045] Example 1 Effect of PMIDA-M1N@PVDF cationic membrane thickness on rejection rate R and water flux J: Membranes with thicknesses of 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, and 90 μm were placed in a low-pressure membrane flux tester, and a waste FCC catalyst acid leaching simulation solution (i.e., La 3+ and Ce 3+ A mixed solution of La and Ce (with concentrations of 15.85 mg / L and 1.995 mg / L, respectively) was passed through a low-pressure membrane flux tester. A certain amount of sample solution was taken out at 30 min, filtered, and diluted to measure ICP. The effect of membrane thickness on the retention rate and water flux of PMIDA-M1N@PVDF cationic membrane for rare earth ions La and Ce was explored. The results are shown in Figure 7 The interception rate is calculated according to formula (1), and the water flux is calculated according to formula (3). The water flux and the interception rate of rare earth ions La and Ce of PMIDA-M1N@PVDF cationic membrane increase with the increase of membrane thickness. When the thickness increases to more than 40μm, the interception rate of rare earth ions La and Ce of PMIDA-M1N@PVDF cationic membrane decreases with the increase of membrane thickness, indicating that the thicker the membrane, the more adsorption sites there are. However, if the membrane is too thick, the steric hindrance is too large, which is not conducive to the adsorption and interception of the membrane, which reflects the trade-off effect of the membrane.

[0046]

[0047] Where: J is water flux, unit: mL·min -1 cm -2 ; t is the filtration time, in min; Q is the volume of solution that passes through in t time, in mL; A is the filtration area of ​​the membrane, in cm 2 .

[0048] Example 1 Recyclability of PMIDA-M1N@PVDF cationic membrane prepared: After the PMIDA-M1N@PVDF cationic membrane was first adsorbed with La and Ce ions for 30 minutes by a membrane separation device, it was immersed in 1 mol / L dilute hydrochloric acid for 24 hours to fully elute the adsorbed metal ions, and then immersed in pure water for 24 hours and naturally dried before the next adsorption. The above experimental process was repeated 4 times for the dried membrane. The results are as follows Figure 8As shown, the ordinate is the relative retention rate A%, and the calculation formula is shown in (4).

[0049]

[0050] Where R 1 is the retention rate of the membrane during the first adsorption, R n is the retention rate of the membrane when it is used for the nth time.

[0051] As can be seen from the figure, after four repeated cycles, the relative interception rate of PMIDA-M1N@PVDF cationic membrane for rare earth ions La and Ce is still above 90%, which shows that the prepared PMIDA-M1N@PVDF cationic membrane has good recyclability. The membrane used in four cycles was dried and then subjected to XRD analysis. The results are as follows Fig. 9 As shown, a is the structure of PMIDA-M1N, b is the structure of PMIDA-M1N@PVDF before recycling, and c is the structure of PMIDA-M1N@PVDF after recycling. After recycling, the membrane still maintains its original crystal structure, indicating that the membrane has good cycle stability.

[0052] The above description is only an exemplary embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a self-assembled carboxyl type cationic membrane, characterized in that: Firstly, the MIL-101-NH2 type MOFs material was prepared by a solvothermal method, and then the MIL-101-NH2 type MOFs was post-modified by small molecules containing functional groups with specific recognition characteristics for rare earth ions, and then grafted onto the surface of PVDF activated by acrylic acid by in situ self-assembly to obtain a self-assembled carboxyl cationic membrane.

2. The preparation method according to claim 1, characterized in that: The following steps are involved: 1) adding chromium nitrate, 2-aminoterephthalic acid and sodium hydroxide to water, stirring at room temperature to fully mix, transferring the resulting solution to a stainless steel reactor, and keeping the temperature at 150-200° C. for reaction for 12-36 hours; after the reaction is completed, centrifugally filtering, washing and vacuum drying the resulting reaction solution to obtain a MIL-101-NH2 type MOFs material; 2) Mixing the MIL-101-NH2 MOFs material obtained in step 1) with a small molecule containing a functional group having specific recognition characteristics for rare earth ions, adding N,N-dicyclohexylcarbodiimide, and adding DMF as a solvent, reacting at 120-150° C. for 24-48 hours under N2 protection; after the reaction, centrifugally separating, washing, and drying the obtained reactant to obtain post-modified MIL-101-NH2 MOFs; 3) immersing the PVDF powder in an acetone solution of AIBN, stirring evenly, adding acrylic acid, reacting at 50-100°C for 4-8h under N2 protection to generate a large number of carboxyl groups on its surface; after the reaction is completed, adding the post-modified MIL-101-NH2 type MOFs obtained in step 2) to the reaction solution, stirring for 30-60min, and then adding the porogen PPA, and continuing to stir and react in an oil bath at 50-80°C for 12-24h, so that the post-modified MIL-101-NH2 type MOFs are grafted onto the PVDF surface by in-situ self-assembly to obtain a casting solution; ultrasonically degassing the casting solution for 1-3h, using a film casting device to push a film on a clean glass plate according to the required thickness, and then immediately placing the glass plate stably in deionized water, and after the film automatically falls off, taking out the glass plate, and soaking the fallen film in water for 24-48h to obtain a self-assembled carboxyl cationic membrane.

3. The preparation method according to claim 2, characterized in that: In step 1), the molar ratio of chromium nitrate, 2-aminoterephthalic acid and sodium hydroxide is 1:1-1.2:1-2.

4. The preparation method according to claim 1 or 2, characterized in that: The small molecule is N-(phosphonomethyl)methylenediacetic acid hydrate.

5. The preparation method according to claim 2, characterized in that: In step 2), the molar ratio of the MIL-101-NH2 type MOFs material, small molecules, and N,N-dicyclohexylcarbodiimide is 1:1-1.5:1-2.

6. The preparation method according to claim 2, characterized in that: In step 3), the usage ratio of PVDF, AIBN, acrylic acid, PPA and post-modified MIL-101-NH2 type MOFs is 4g: 0.5-2g: 2-4mL: 0.2-0.8g: 2-4g.

7. The preparation method according to claim 2, characterized in that: In step 1), the washing is carried out with DMF and ethanol solution in sequence, and the vacuum drying temperature is 60°C-80°C; in step 2), the washing is carried out with anhydrous ethanol, and the vacuum drying temperature is 60°C-80°C.

8. The preparation method according to claim 2, characterized in that: In step 3), the thickness of the push film is 20-100 μm.

9. A self-assembled carboxyl type cationic membrane prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the self-assembled carboxyl type cationic membrane according to claim 9 in the recovery of rare earth elements.

Citation Information

Patent Citations

  • Preparation and novel application of a type of MIL-101(Cr) adsorbent modified by virtue of post translation

    CN105107467A

  • Membrane material with adsorption function, and preparation method and application thereof

    CN108927010A

  • MIL-101 (Cr) series MOFs material as well as preparation method and application thereof

    CN117205903A

  • KR20200128770A