Chemical reaction system for synthesizing multilayer core-shell structure material and control method thereof

Through the fully automatic chemical co-precipitation reaction system, the problem of difficulty in forming a multi-layer core-shell structure with existing technology has been solved, and a metal oxide cathode material with high specific capacity and improved stability has been achieved, which is suitable for the industrial production of lithium-ion batteries.

CN118807657APending Publication Date: 2024-10-22HEBEI UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410745651.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing metal oxide cathode material preparation methods are difficult to form a multi-layer core-shell structure, resulting in the material's specific capacity not matching the anode material, high operating voltage and poor thermal stability, which limits the development of lithium-ion batteries.

Method used

A fully automatic chemical co-precipitation reaction system is designed. Through the cooperation of a high-precision peristaltic pump and a pH electrode, the pH value and flow rate of the reaction solution are accurately controlled. Combined with a stirring and heating device, a stable multi-layer core-shell structure is formed. Material.

Benefits of technology

It achieves high specific capacity, stability and safety improvement of metal oxide cathode materials, which is suitable for large-scale industrial production, reduces manual intervention, and improves the performance and output of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807657A_ABST
    Figure CN118807657A_ABST
Patent Text Reader

Abstract

The invention discloses a chemical reaction system for synthesizing a multilayer core-shell structure material and a control method thereof, the reaction system comprises: a kettle body having a reaction chamber; the at least two liquid storage tanks are respectively communicated with the kettle body; wherein at least one liquid storage tank is used for storing a metal salt solution, and at least another liquid storage tank is used for storing an alkali solution; the at least two high-precision peristaltic pumps are in one-to-one correspondence with the liquid storage tanks, and each high-precision peristaltic pump is arranged between the corresponding liquid storage tank and the kettle body and is configured to be used for pumping the reaction liquid in the corresponding liquid storage tank into the kettle body; the pH electrode is arranged in the reaction cavity and is configured to be used for sensing the pH value of reaction liquid in the reaction cavity; and the controller is respectively coupled with the high-precision peristaltic pumps and the pH electrode, and is configured to adjust the flow of each high-precision peristaltic pump pumped into the reaction cavity by the corresponding liquid storage tank based on the change of the pH value of the reaction liquid in the reaction cavity in the kettle body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of production equipment for lithium ion battery material precursors, and in particular to a fully automatic chemical coprecipitation reaction system for synthesizing multi-layer core-shell structure materials. Background Art

[0002] At present, as mankind enters the era of intelligent industry, energy shortage has become one of the urgent problems to be solved. Moreover, the greenhouse effect and environmental pollution caused by traditional energy that people have been using for a long time are becoming more and more serious. In order to achieve sustainable development, we must reduce dependence on traditional energy. Therefore, finding clean new energy has become one of the main tasks at present.

[0003] Lithium-ion batteries have been developing rapidly since their emergence due to their advantages such as high mass-to-volume specific energy, low pollution, excellent cycle stability and reliable safety performance. Nowadays, lithium-ion batteries have been widely used in electric vehicles, energy storage power supplies and 3C digital products, and will be widely used in advanced fields such as smart grids and large-scale energy storage systems in the future.

[0004] At present, the specific capacity of positive electrode materials of lithium-ion batteries cannot match that of negative electrode materials, which has become a decisive factor restricting the development of lithium-ion batteries. Therefore, the development of new positive electrode materials with higher specific capacity is the key to the development of lithium-ion batteries. The metal oxide positive electrode material with the general formula xLi2MnO3·(1-x)LMO2 (M=Mn, Co, Ni, Fe, etc.) has a theoretical specific capacity of more than 300mAh / g and an actual specific capacity of more than 200mAh / g. It is regarded as one of the candidates for the next generation of positive electrode materials for lithium-ion batteries and has received widespread attention from researchers. However, this type of battery material also has some disadvantages. It has a high operating voltage and is more likely to react with the electrolyte to destroy the surface structure of the material. In addition, in the completely delithiated state, the thermal stability of the material deteriorates, resulting in reduced battery safety. These problems seriously hinder the practical application of this type of positive electrode material in high-energy lithium-ion batteries.

[0005] In response to the above problems, some scholars have proposed a core-shell structured cathode material precursor, which has a suitable pore size and reasonable distribution, provides abundant active sites, prevents the aggregation of active substances, and provides convenient channels for electrons and Li + The transport characteristics of lithium-ion batteries have significantly improved the rate performance and capacity retention of lithium-ion batteries. However, due to the complex synthesis process, low efficiency, and high requirements for supporting equipment, its further development has been seriously hindered.

[0006] At present, the mainstream method for preparing metal oxide positive electrode material precursors is to use soluble metal (Ni, Co, Mn) salts and sodium carbonate to undergo co-precipitation reaction through a chelating agent. However, the formation of a core-shell structure material with multi-layer components requires individual regulation of the ratio and pH value of each component, and the currently used co-precipitation system is difficult to meet this requirement.

[0007] The core-shell structure is an ordered assembly structure formed by one material encapsulating another material through chemical bonds or other forces. Due to its unique structural characteristics, the core-shell structure integrates the properties of two or more internal and external materials and complements each other's deficiencies. It has been an important research direction in recent years in which morphology determines properties, and has broad application prospects in catalysis, photocatalysis, batteries, gas storage and separation. Summary of the invention

[0008] In response to the problems and needs raised above, this solution proposes a chemical reaction system for synthesizing multilayer core-shell structure materials and its control method. Due to the adoption of the following technical features, the above technical objectives can be achieved and many other technical effects can be brought about.

[0009] An object of the present invention is to provide a chemical reaction system for synthesizing a multilayer core-shell structure material, comprising:

[0010] A kettle body having a reaction chamber;

[0011] At least two liquid storage tanks, at least two of which are respectively connected to the kettle body, at least one of which stores a metal salt solution, and at least another of which stores an alkali solution;

[0012] at least two high-precision peristaltic pumps, corresponding to the liquid storage tanks one by one, and each of the high-precision peristaltic pumps is disposed between the liquid storage tank and the kettle body, and is configured to pump the reaction liquid in the liquid storage tank into the kettle body respectively; a pH electrode is disposed in the reaction chamber, and is configured to sense the pH value of the reaction liquid in the reaction chamber;

[0013] A controller is coupled to the high-precision peristaltic pump and the pH electrode respectively, and is configured to adjust the flow rate of each high-precision peristaltic pump to pump its corresponding liquid storage tank into the reaction chamber based on the change of the pH value of the reaction liquid in the reaction chamber in the kettle body.

[0014] In addition, the chemical reaction system for synthesizing the multilayer core-shell structure material according to the present invention may also have the following technical features:

[0015] In one example of the present invention, the stirring device further comprises:

[0016] Drive motor;

[0017] The stirring impeller is connected to the output shaft of the driving motor and is configured to stir the reaction liquid in the reaction chamber and make it react fully.

[0018] In one example of the present invention, it further includes: a heating device,

[0019] It is connected to the kettle body and is configured to heat the kettle body to adjust the reaction temperature of the reaction liquid in the reaction chamber;

[0020] The heating device is coupled to the controller and is configured to adjust the heating temperature of the heating device based on temperature information set by the controller.

[0021] In one example of the present invention, it further includes: a temperature sensor,

[0022] It is installed on the kettle body and is configured to sense the temperature information of the reaction liquid in the kettle body;

[0023] The temperature sensor is coupled to the controller and is configured such that the temperature sensor feeds back the temperature information of the kettle body to the controller, and the controller adjusts the heating temperature of the heating device based on the temperature of the kettle body.

[0024] In one example of the present invention, the heating device comprises:

[0025] A hydrothermal interlayer, which is coated on the outside of the kettle;

[0026] A heating boiler is communicated with the hydrothermal interlayer and is configured to heat the hydrothermal interlayer.

[0027] In one example of the present invention,

[0028] The controller is configured to generate a prompt instruction,

[0029] The reaction system further comprises a control panel, which is coupled to the controller and configured to transmit the prompt instruction generated by the controller to the control panel.

[0030] In one example of the present invention,

[0031] The controller is configured as follows:

[0032] When the actual pH value of the reaction solution in the kettle detected by the pH electrode is less than the set target pH value, a prompt instruction is generated for the high-precision peristaltic pump corresponding to the liquid storage tank storing the alkaline solution to reduce the rotation speed;

[0033] When the actual pH value of the reaction solution in the kettle detected by the pH electrode is greater than or equal to the set target pH value, a prompt instruction is generated for the high-precision peristaltic pump corresponding to the liquid storage tank storing the alkaline solution to increase the rotation speed.

[0034] Another object of the present invention is to provide a control method for a chemical reaction system for synthesizing a multilayer core-shell structure material as described above, comprising the following steps:

[0035] S10: using a pH electrode to sense the actual pH value of the reaction solution in the reaction chamber;

[0036] S20: The controller uses a PID control algorithm to select corresponding PID parameters and calculate the speed adjustment amount of the high-precision peristaltic pump according to the set target pH value and the current actual pH value fed back by the pH electrode;

[0037] S30: According to the obtained rotation speed adjustment amount of the high-precision peristaltic pump, the rotation speed of the high-precision peristaltic pump is automatically adjusted to maintain the actual flow rate of pumping the reaction liquid into the kettle body.

[0038] In one example of the present invention, the expression of the PID control algorithm is as follows:

[0039]

[0040] Where u(t) is the output signal of PID; e(t) is the difference between the given value r(t) and the measured value y(t); k p is the proportional gain; T is the integral time constant; T d is the differential time constant.

[0041] In one example of the present invention, calculating the speed adjustment amount of the high-precision peristaltic pump according to the set target pH value and the current actual pH value fed back by the pH electrode includes the following steps:

[0042] Set the target pH value, and make the difference between the target pH value and the actual pH value;

[0043] Calculate the difference between the actual pH value and the target pH value;

[0044] The difference is used as input, corresponding PID parameters are selected, and the speed adjustment amount of the high-precision peristaltic pump is calculated in the PID control algorithm.

[0045] The best embodiment for carrying out the present invention will be described in more detail below with reference to the accompanying drawings so that the features and advantages of the present invention can be easily understood. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings of the embodiments of the present invention, wherein the drawings are only used to illustrate some embodiments of the present invention, but not to limit all embodiments of the present invention thereto.

[0047] Figure 1 A structural principle diagram of a chemical reaction system for synthesizing a multilayer core-shell structure material according to an embodiment of the present invention;

[0048] Figure 2 A flow chart of a chemical reaction system control method for synthesizing a multi-layer core-shell structure material according to an embodiment of the present invention;

[0049] Figure 3 is a schematic structural diagram of a control panel according to an embodiment of the present invention;

[0050] Figure 4 is a scanning electron microscope image of a core-shell material according to an embodiment of the present invention;

[0051] Figure 5 This is a graph showing a charge and discharge test of a lithium-rich positive electrode material at a constant current density according to an embodiment of the present invention.

[0052] List of reference numerals:

[0053] Reaction system 100;

[0054] Kettle body 110;

[0055] Reaction chamber 111;

[0056] Liquid storage tank 120;

[0057] High precision peristaltic pump 130;

[0058] pH electrode 140;

[0059] Controller 150;

[0060] Control panel 151;

[0061] A stirring device 160;

[0062] Driving motor 161;

[0063] A stirring impeller 162;

[0064] Heating device 170;

[0065] Heating boiler 171;

[0066] hydrothermal interlayer 172;

[0067] Temperature sensor 180. DETAILED DESCRIPTION

[0068] In order to make the purpose, technical solution and advantages of the technical solution of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described in conjunction with the drawings of specific embodiments of the present invention. The same figure marks in the drawings represent the same parts. It should be noted that the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0069] Unless otherwise defined, the technical terms or scientific terms used herein shall have the usual meanings understood by persons of ordinary skill in the field to which the present invention belongs. The words "first", "second" and similar words used in the patent application specification and claims of the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one" or "one" do not necessarily indicate a quantity limitation. Words such as "include" or "comprise" mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. Words such as "connect" or "connected" are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0070] According to the first aspect of the present invention, a chemical reaction system 100 for synthesizing a multilayer core-shell structure material is as follows: Figure 1 As shown, including:

[0071] The kettle body 110 has a reaction chamber 111;

[0072] At least two liquid storage tanks 120, at least two of the liquid storage tanks 120 are respectively connected to the kettle body 110, wherein at least one of the liquid storage tanks 120 stores a metal salt solution, and at least another of the storage tanks 120 stores an alkali solution;

[0073] At least two high-precision peristaltic pumps 130, corresponding to the liquid storage tanks 120 one by one, and each of the high-precision peristaltic pumps 130 is disposed between the liquid storage tank 120 and the kettle body 110, and is configured to pump the reaction liquid in the liquid storage tank 120 into the kettle body 110 respectively;

[0074] A pH electrode 140 is disposed in the reaction chamber 111 and is configured to sense the pH value of the reaction solution in the reaction chamber 111;

[0075] The controller 150 is coupled to the high-precision peristaltic pump 130 and the pH electrode 140 respectively, and is configured to adjust the flow rate of each high-precision peristaltic pump 130 to pump its corresponding liquid storage tank 120 into the reaction chamber 111 based on the change in the pH value of the reaction liquid in the reaction chamber 111 in the kettle body 110.

[0076] The pH electrode 140 is used to sense the actual pH value of the reaction liquid in the reaction chamber 111; the controller 150 uses a PID control algorithm to calculate the speed adjustment amount of the high-precision peristaltic pump 130 according to the set target pH value and the current actual pH value fed back by the pH electrode 140; and the speed of the high-precision peristaltic pump 130 is automatically adjusted according to the obtained speed adjustment amount of the high-precision peristaltic pump 130 to maintain the actual flow rate of pumping the reaction liquid into the kettle body 110.

[0077] The present invention provides a fully automatic chemical co-precipitation reaction system 100 for synthesizing multi-layer core-shell structure materials. Different components and pH values ​​can be freely combined through multiple automatic feeding systems to stably synthesize multi-layer core-shell structure materials. The precursor of the metal oxide positive electrode material prepared by the present invention has a clear core-shell structure, good spherical morphology, reasonable particle size distribution, stable performance, high yield, reduced manual intervention, high repeatability, and is suitable for large-scale industrial production.

[0078] In one example of the present invention, the stirring device 160 is further included, which includes:

[0079] Driving motor 161;

[0080] A stirring impeller 162, which is connected to the output shaft of the driving motor 161 and is configured to stir the reaction liquid in the reaction chamber 111 to make it fully react;

[0081] By providing the stirring device 160 , the reaction speed of the reaction solution in the kettle body 110 can be accelerated, thereby greatly improving the reaction effect.

[0082] In one example of the present invention, it further includes: a heating device 170,

[0083] It is connected to the kettle body 110 and is configured to heat the kettle body 110 to adjust the reaction temperature of the reaction liquid in the reaction chamber 111;

[0084] The heating device 170 is coupled to the controller 150 and is configured to adjust the heating temperature of the heating device 170 based on the temperature information set by the controller 150;

[0085] The kettle body 110 can be effectively heated by providing the heating device 170 , thereby providing the kettle body 110 with an environment suitable for the reaction of the reaction solution.

[0086] In one example of the present invention, it further includes: a temperature sensor 180,

[0087] It is installed on the kettle body 110 and is configured to sense the temperature information of the reaction liquid in the kettle body 110;

[0088] The temperature sensor 180 is coupled to the controller 150 and configured such that the temperature sensor 180 feeds back the temperature information of the kettle body 110 to the controller 150, and the controller 150 adjusts the heating temperature of the heating device 170 based on the temperature of the kettle body 110;

[0089] That is to say, a specified temperature is preset by the controller 150, and the temperature sensor 180 senses the temperature information of the kettle body 110 in real time. When the temperature value measured by the temperature sensor 180 is less than the specified temperature, the controller 150 controls the heating device 170 to heat the kettle body 110 until the specified temperature is reached; and when the temperature value measured by the temperature sensor 180 is greater than or equal to the specified temperature, the controller 150 controls the heating device 170 to stop heating the kettle body 110; by setting the temperature sensor 180, the temperature of the kettle body 110 can be effectively controlled.

[0090] In one example of the present invention, the heating device 170 includes:

[0091] A hydrothermal interlayer 172, which is coated on the outside of the kettle body 110;

[0092] A heating boiler 171, which is in communication with the hydrothermal interlayer 172 and is configured to heat the hydrothermal interlayer 172;

[0093] A specified temperature is preset by the controller 150, and the temperature information of the kettle body 110 is sensed in real time by the temperature sensor 180. When the temperature value measured by the temperature sensor 180 is less than the specified temperature, the controller 150 controls the heating boiler 171 to heat the hydrothermal interlayer 172 and then heats the kettle body 110 until the specified temperature is reached; and when the temperature value measured by the temperature sensor 180 is greater than or equal to the specified temperature, the controller 150 controls the heating boiler 171 to stop heating the kettle body 110.

[0094] In one example of the present invention,

[0095] The controller 150 is configured to generate a prompt instruction,

[0096] The reaction system 100 further includes a control panel 151 , which is coupled to the controller 150 and configured to transmit the prompt instruction generated by the controller 150 to the control panel 151 ;

[0097] The control panel 151 can intuitively display the prompt instructions generated by the controller 150 , thereby facilitating the operator to view the operating status of the reaction system 100 in real time.

[0098] For example, the analog current signal output by the PLC is transmitted to the peristaltic pump so as to pump the alkali solution into the heatable reactor body 110, and the actual pH value of the reaction is fed back to the control panel 151 through real-time collection by the pH electrode 140. And the actual flow rate of the peristaltic pump is fed back to the control panel 151 in real time through the flow rate conversion of the output signal.

[0099] In one example of the present invention,

[0100] The controller 150 is configured as follows:

[0101] When the pH electrode 140 detects that the actual pH value of the reaction solution in the kettle 110 is less than the set target pH value, a prompt instruction is generated for the high-precision peristaltic pump 130 corresponding to the liquid storage tank 120 storing the alkaline solution to reduce the rotation speed;

[0102] When the pH electrode 140 detects that the actual pH value of the reaction solution in the kettle 110 is greater than or equal to the set target pH value, a prompt instruction is generated for the high-precision peristaltic pump 130 corresponding to the liquid storage tank 120 storing the alkaline solution to increase the rotation speed;

[0103] That is, the controller 150 controls the pumping amount of the alkaline solution in the liquid storage tank 120 more accurately based on the pH value of the reaction solution in the kettle 110 detected by the pH electrode 140, so as to better complete the co-precipitation reaction.

[0104] According to the second aspect of the present invention, a control method of the chemical reaction system 100 for synthesizing a multilayer core-shell structure material as described above is as follows: Figure 2 As shown, the following steps are included:

[0105] S10: Using the pH electrode 140 to sense the actual pH value of the reaction solution in the reaction chamber 111;

[0106] S20: The controller 150 uses a PID control algorithm to select corresponding PID parameters and calculate the speed adjustment amount of the high-precision peristaltic pump 130 according to the set target pH value and the current actual pH value fed back by the pH electrode 140;

[0107] S30 : According to the obtained rotation speed adjustment amount of the high-precision peristaltic pump 130 , the rotation speed of the high-precision peristaltic pump 130 is automatically adjusted to maintain the actual flow rate of pumping the reaction liquid into the kettle body 110 .

[0108] The control method of the reaction system 100 can freely combine different components and pH values ​​through multiple automatic feeding systems, thereby stably synthesizing multi-layer core-shell structure materials. The precursor of the metal oxide positive electrode material prepared by the present invention has a clear core-shell structure, good spherical morphology, reasonable particle size distribution, stable performance, high yield, reduced manual intervention, high repeatability, and is suitable for large-scale industrial production.

[0109] In one example of the present invention, the expression of the PID control algorithm is as follows:

[0110]

[0111] Where u(t) is the output signal of PID; e(t) is the difference between the given value r(t) and the measured value y(t); k p is the proportional gain; T is the integral time constant; T d is the differential time constant.

[0112] Specifically,

[0113] u(t)=h p (t)+h i (t)+h d (t)

[0114] h p (t) = k p *e(t)=k p *(r(t)-y(t))

[0115]

[0116]

[0117] Where, u(t) is the output signal of PID; h p (t) is the proportional link; h i (t) is the integral link; h d (t) is the integral-differential link; e(t) is the difference between the given value r(t) and the measured value y(t); k p is the proportional gain; T is the integral time constant; T s is the sampling time; h i0 (t) is the last integral sum; T d is the differential time constant; e0(t) is the last deviation.

[0118] In one example of the present invention, the speed adjustment amount of the high-precision peristaltic pump 130 is calculated according to the set target pH value and the current actual pH value fed back by the pH electrode 140, including the following steps:

[0119] Set the target pH value, and make the difference between the target pH value and the actual pH value;

[0120] Calculate the difference between the actual pH value and the target pH value;

[0121] The difference is used as input, corresponding PID parameters are selected, and the speed adjustment amount of the high-precision peristaltic pump 130 is calculated in the PID control algorithm.

[0122] Specific examples

[0123] Example 1

[0124] The device was used to prepare Mn at different pH values. 0.75 Ni 0.25 CO3@Mn 0.625 Ni 0.375 Core-shell material of CO3. According to the molar ratio of metal ions of 6:2 and 5:3, a certain amount of nickel sulfate and manganese sulfate are weighed and mixed to form a 1M solution and placed in two liquid storage tanks 120; different concentrations of complexing agents are placed in the two liquid storage tanks 120; a certain concentration of alkaline solution is placed in the liquid storage tank 120; 3L of deionized water is added to the heatable reactor body 110 as the base liquid, and the corresponding high-precision peristaltic pump 130 is inserted into the reactor body 110, and the control line is connected to the controller 150.

[0125] like Figure 3 As shown, it is a schematic diagram of the control panel 151 of the five-pump automatic adjustment, and its parameter settings are as follows:

[0126] In the first stage of the synthesis of the inner core, pH 1 was set to 7.6, the initial flow rate of the high-precision peristaltic pump 1 corresponding to the liquid storage tank 120 where the molar ratio of the metal ions was 6:2 was set to 3 ml / min, the initial flow rate of the high-precision peristaltic pump 2 corresponding to the liquid storage tank 120 where the complexing agent 1 was located was set to 1 ml / min, and the end time of the first stage was set to 128 min.

[0127] In the synthesis of the second stage shell, pH2 was set to 8.4, the initial flow rate of the high-precision peristaltic pump 3 corresponding to the liquid storage tank 120 where the molar ratio of the metal ions in the second stage was set to 5:2 was set to 3 ml / min, the initial flow rate of the liquid storage tank 120 where the complexing agent 2 was located to the high-precision peristaltic pump 4 was set to 3 ml / min, the start time of the second stage was set to 188 min, and the end time of the second stage was set to 220 min.

[0128] The reaction target temperature was set to 50°C, the PID parameters corresponding to pH = 8 were selected, and the final reaction time was set to 220 min.

[0129] The pH value of the reaction is monitored by the pH electrode 140 and the rotation speed of the high-precision peristaltic pump 130 corresponding to the alkali solution is controlled by the PID algorithm of the controller 150 to perform a chemical coprecipitation reaction.

[0130] like Figure 4 As shown in the scanning electron microscope picture, it can be seen that Mn 0.75 Ni 0.25 CO3(pH=7.6)@Mn 0.625 Ni 0.375 The core-shell material of CO3 (pH=8.4) is composed of spherical tiny particles, which are round and have high tap density. The particle size is in the range of 10 to 20 μm.

[0131] like Figure 5 As shown, the obtained core-shell material is mixed with excess lithium carbonate and sintered to form a lithium-rich positive electrode material. Using the NEWARE TC53 battery test system, the charge and discharge test was carried out at a constant current density, with a charge and discharge voltage range of 2.0 to 4.8V and a charge and discharge current of 400mA / g. It can be seen that the battery has good cycle performance.

[0132] Example 2 (Core-shell at different pH)

[0133] The core-shell structure of Mn with different pH values ​​was prepared by this device 0.75 Ni 0.25 CO3@Mn 0.75 Ni 0.25 CO3 material. According to the molar ratio of metal ions of 6:2, a certain amount of nickel sulfate and manganese sulfate are weighed and mixed and placed in the first liquid storage tank 120 and the second liquid storage tank 120 to prepare a 1M solution; 1M sodium carbonate and ammonia solution are prepared and placed in the fourth liquid storage tank 120; 3L of deionized water is added to the heatable reactor body 110 as the base liquid, and the first high-precision peristaltic pump 130, the second high-precision peristaltic pump 130, and the fourth high-precision peristaltic pump 130 are inserted into the reactor body 110, and the control line is connected to the controller 150.

[0134] The control panel 151 is used to preset a temperature of 50° C., the water-heating interlayer 172 is heated by the heating boiler 171, and the temperature is monitored by the temperature sensor 180; the control panel 151 is used to set the operating time and speed of the first high-precision peristaltic pump 130 and the second high-precision peristaltic pump 130;

[0135] The pH values ​​of the two stages are set to 7.8 and 8.2 using the control panel 151. The pH value of the reaction is monitored using the pH electrode 140 and the rotation speed of the fourth high-precision peristaltic pump 130 is controlled by the PID algorithm of the controller 150 to perform a chemical coprecipitation reaction.

[0136] Example 3 (Core-shell structure materials under different complexation conditions)

[0137] The core-shell structure material under different complexing conditions is prepared by using the device. According to the different molar ratios of metal ions, a certain amount of nickel sulfate and manganese sulfate are weighed and mixed to form a 1M solution and placed in two liquid storage tanks 120; different concentrations of complexing agents are placed in the two liquid storage tanks 120; a certain amount of alkaline solution is placed in the liquid storage tank 120; 3L of deionized water is added to the heatable reactor body 110 as the bottom liquid, and the corresponding high-precision peristaltic pump 130 is inserted into the reactor body 110, and the control line is connected to the controller 150.

[0138] The controller 150 is used to preset a temperature of 50° C., the hydrothermal interlayer 172 is heated by the heating boiler 171, and the temperature is monitored by the temperature sensor 180; the controller 150 is used to set the operating time and speed of the high-precision peristaltic pump 130 corresponding to the metal ion solution and the complexing agent;

[0139] The pH value is set by the controller 150. The pH value of the reaction is monitored by the pH electrode 140 and the rotation speed of the high-precision peristaltic pump 130 corresponding to the alkali solution is controlled by the PID algorithm of the controller 150 to perform a chemical coprecipitation reaction.

[0140] Example 4 (Four layers of gradient material at the same pH)

[0141] The device is used to prepare four layers of gradient materials with different components under the same pH condition. According to the different molar ratios of metal ions, a certain amount of nickel sulfate and manganese sulfate are weighed and mixed to form a 1M solution and placed in four liquid storage tanks 120; a complexing agent and an alkaline solution are placed in the liquid storage tank 120; 3L of deionized water is added to the heatable reactor body 110 as the base liquid, a high-precision peristaltic pump 130 is inserted into the reactor body 110, and a control line is connected to the controller 150.

[0142] The controller 150 is used to preset a temperature of 50° C., the hydrothermal interlayer 172 is heated by the heating boiler 171, and the temperature is monitored by the temperature sensor 180; the controller 150 is used to set the operating time and speed of the high-precision peristaltic pump 130 corresponding to the metal ion solution and the complexing agent;

[0143] The pH value is set by the controller 150. The pH value of the reaction is monitored by the pH electrode 140 and the rotation speed of the high-precision peristaltic pump 130 corresponding to the alkali solution is controlled by the PID algorithm of the controller 150 to perform a chemical coprecipitation reaction.

[0144] Example 5 (Four-layer gradient material with different pH)

[0145] The device is used to prepare four layers of gradient materials with different components and different pH values. A certain amount of nickel sulfate and manganese sulfate are weighed according to the different molar ratios of metal ions, mixed into a 1M solution and placed in four liquid storage tanks 120; a complexing agent and an alkaline solution are placed in the liquid storage tank 120; 3L of deionized water is added to the heatable reactor body 110 as the base liquid, a high-precision peristaltic pump 130 is inserted into the reactor body 110, and the control line is connected to the programmable control system.

[0146] The system control panel 151 is used to preset the temperature to 50°C, the hydrothermal interlayer 172 is heated by the heating boiler 171104, and the temperature is monitored by the temperature sensor 180; the controller 150 is used to set the operating time and speed of the high-precision peristaltic pump 130 corresponding to the metal ion solution and the complexing agent;

[0147] The pH value of four stages is set by the controller 150. The pH value of the reaction is monitored by the pH electrode 140 and the rotation speed of the high-precision peristaltic pump 130 corresponding to the alkali solution is controlled by the PID algorithm of the controller 150 to perform a chemical coprecipitation reaction.

[0148] The above describes in detail an exemplary implementation of the chemical reaction system 100 for synthesizing a multi-layer core-shell structure material and its control method proposed in the present invention with reference to a preferred embodiment. However, those skilled in the art will appreciate that, without departing from the concept of the present invention, various modifications and variations may be made to the above-mentioned specific embodiments, and various technical features and structures proposed in the present invention may be combined in various ways without exceeding the protection scope of the present invention, which is determined by the appended claims.

Claims

1. A chemical reaction system for synthesizing multilayer core-shell structure materials, It is characterized in that include: A kettle body (110) having a reaction chamber (111); at least two liquid storage tanks (120), wherein at least two of the liquid storage tanks (120) are respectively connected to the kettle body (110), wherein at least one of the liquid storage tanks (120) stores a metal salt solution, and wherein at least another of the storage tanks (120) stores an alkali solution; at least two high-precision peristaltic pumps (130), corresponding one to one with the liquid storage tank (120), and each of the high-precision peristaltic pumps (130) is disposed between the liquid storage tank (120) and the kettle body (110), and is configured to pump the reaction liquid in the liquid storage tank (120) into the kettle body (110); A pH electrode (140) is disposed in the reaction chamber (111) and is configured to sense the pH value of the reaction liquid in the reaction chamber (111); A controller (150) is coupled to the high-precision peristaltic pump (130) and the pH electrode (140) respectively, and is configured to adjust the flow rate of each high-precision peristaltic pump (130) pumping its corresponding liquid storage tank (120) into the reaction chamber (111) based on the change in the pH value of the reaction liquid in the reaction chamber (111) in the kettle body (110).

2. The chemical reaction system for synthesizing a multilayer core-shell structure material according to claim 1, It is characterized in that Also included is a stirring device (160), which includes: A driving motor (161); The stirring impeller (162) is connected to the output shaft of the driving motor (161) and is configured to stir the reaction liquid in the reaction chamber (111) and enable it to react fully.

3. The chemical reaction system for synthesizing a multilayer core-shell structure material according to claim 1, It is characterized in that Also includes: a heating device (170), It is connected to the kettle body (110) and is configured to heat the kettle body (110) to adjust the reaction temperature of the reaction liquid in the reaction chamber (111); The heating device (170) is coupled to the controller (150) and is configured to adjust the heating temperature of the heating device (170) based on temperature information set by the controller (150).

4. The chemical reaction system for synthesizing a multilayer core-shell structure material according to claim 3, It is characterized in that Also includes: a temperature sensor (180), It is installed on the kettle body (110) and is configured to sense the temperature information of the reaction liquid in the kettle body (110); The temperature sensor (180) is coupled to the controller (150), and is configured such that the temperature sensor (180) feeds back temperature information of the kettle body (110) to the controller (150), and the controller (150) adjusts the heating temperature of the heating device (170) based on the temperature of the kettle body (110).

5. The chemical reaction system for synthesizing a multilayer core-shell structure material according to claim 4, It is characterized in that The heating device (170) comprises: A hydrothermal interlayer (172) covering the outside of the kettle body (110); A heating boiler (171) is connected to the hydrothermal interlayer (172) and is configured to heat the hydrothermal interlayer (172).

6. The control method of the chemical reaction system for synthesizing multilayer core-shell structure materials according to claim 1, It is characterized in that The controller (150) is configured to generate a prompt instruction, The reaction system further comprises a control panel (151), which is coupled to the controller (150) and is configured to transmit the prompt instruction generated by the controller (150) to the control panel (151).

7. The control method of the chemical reaction system for synthesizing multilayer core-shell structure materials according to claim 6, It is characterized in that The controller (150) is configured as follows: When the actual pH value of the reaction solution in the kettle (110) detected by the pH electrode (140) is lower than the set target pH value, a prompt instruction is generated for the high-precision peristaltic pump (130) corresponding to the liquid storage tank (120) storing the alkaline solution to reduce the rotation speed; When the actual pH value of the reaction solution in the kettle (110) detected by the pH electrode (140) is greater than or equal to the set target pH value, a prompt instruction is generated for the high-precision peristaltic pump (130) corresponding to the liquid storage tank (120) storing the alkaline solution to increase the rotation speed.

8. A method for controlling a chemical reaction system for synthesizing a multilayer core-shell structure material according to any one of claims 1 to 7, It is characterized in that The steps include: S10: using a pH electrode (140) to sense the actual pH value of the reaction liquid in the reaction chamber (111); S20: The controller (150) uses a PID control algorithm to select corresponding PID parameters and calculate a speed adjustment amount of the high-precision peristaltic pump (130) according to a set target pH value and a current actual pH value fed back by the pH electrode (140); S30: Automatically adjust the rotation speed of the high-precision peristaltic pump (130) according to the obtained rotation speed adjustment amount of the high-precision peristaltic pump (130) to maintain the actual flow rate of pumping the reaction liquid into the kettle body (110).

9. The control method of the chemical reaction system for synthesizing multilayer core-shell structure materials according to claim 8, It is characterized in that The expression of the PID control algorithm is as follows: Where u(t) is the output signal of PID; e(t) is the difference between the given value r(t) and the measured value y(t); k p is the proportional gain; T is the integral time constant; T d is the differential time constant.

10. The control method of the chemical reaction system for synthesizing multi-layer core-shell structure materials according to claim 8, It is characterized in that Calculating the speed adjustment amount of the high-precision peristaltic pump (130) according to the set target pH value and the current actual pH value fed back by the pH electrode (140) comprises the following steps: Set the target pH value, and make the difference between the target pH value and the actual pH value; Calculate the difference between the actual pH value and the target pH value; The difference is used as input, corresponding PID parameters are selected, and the speed adjustment amount of the high-precision peristaltic pump (130) is calculated in the PID control algorithm.

Citation Information

Cited By

  • Core-shell structure ceramic powder and preparation method and preparation system thereof