Alkali-modified steel slag adsorption phosphorus removal filler as well as preparation method and application thereof
Through the combination of modified steel slag powder, cement, diatomaceous earth and sodium alginate treatment, an alkali-modified steel slag adsorption and phosphorus removal filler was prepared, which solved the problem of clogging and loss of powdered steel slag in sewage treatment and improved the phosphorus removal efficiency. and resource utilization.
Patent Information
- Application Number
- CN202411012686.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing technology, powdered steel slag easily blocks equipment in sewage treatment, resulting in serious material loss. There is little research on modified steel slag fillers, making it difficult to effectively utilize steel slag resources, and the phosphorus removal efficiency is low.
By soaking steel slag powder in NaOH solution and mixing it with cement and diatomaceous earth, adding sodium alginate and then granulating, an alkali-modified steel slag adsorption and phosphorus removal filler was prepared. The raw material ratio and granulation process were optimized to improve chemical bond adsorption. ability.
The phosphorus removal capacity is significantly improved, the filler preparation cost is reduced, the resource utilization of steel slag is realized, and the comprehensive performance and phosphorus removal efficiency of the filler are improved.
Smart Images

Figure BDA0004964843550000041 
Figure BDA0004964843550000042 
Figure BDA0004964843550000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sewage treatment, and more particularly to an alkali-modified steel slag adsorption and phosphorus removal filler and a preparation method and application thereof. Background Art
[0002] The total amount of phosphorus emissions in today's society is increasing. If it is not handled in time, it will lead to problems such as eutrophication of lakes, damage the environment and affect human health. Steel slag is an industrial waste slag produced in the process of steel smelting. At present, the total amount of steel slag stockpiled in my country is 400 million tons, and the utilization rate is less than 22%. It will also cause large-scale environmental pollution and endanger human health. It is urgent to recycle steel slag. Exploring the potential of steel slag in the field of environmental protection and achieving harm by harm has become a research hotspot for the treatment of phosphorus-containing wastewater. Steel slag is mainly composed of CaO, Al2O3, Fe2O3, MgO and SiO2. After alkali modification, it can provide sufficient OH- and Ca 2 It forms calcium phosphate (Ca-PO4) precipitation, which is a good adsorbent for wastewater phosphorus removal. However, since powdered steel slag is difficult to separate from solid and liquid after adsorption treatment, it is easy to clog equipment and cause serious material loss, making it unsuitable for actual engineering applications. At the same time, there is little research on modified steel slag fillers at this stage, so it is a better research direction. Summary of the invention
[0003] In view of this, in order to improve the phosphorus removal efficiency of the filler, the present invention starts from the modification of industrial waste steel slag, modifies the surface composition of the steel slag according to the composition and surface structure of the steel slag, improves the chemical bond adsorption capacity of the steel slag, and optimizes the raw material ratio.
[0004] To achieve the above object, the present invention adopts the following technical solution:
[0005] A method for preparing an alkali-modified steel slag adsorption and dephosphorization filler comprises the following steps:
[0006] (1) Soak the steel slag powder in a NaOH solution, wash it with tap water and dry it naturally;
[0007] (2) The steel slag, cement and diatomaceous earth treated in step (1) are mixed into powder in a weight percentage of 60.9%, 26.1% and 13.0%, and then the sodium alginate solution is added and stirred evenly. The mixture is then put into a granulator for granulation. The prepared filler is dried in the shade and sprayed with distilled water every day for curing during the drying process.
[0008] Preferably, the concentration of the NaOH solution in step (1) is 3 mol / L, and the soaking time is 24 h.
[0009] Preferably, the steel slag particle size is 60-80 mesh.
[0010] Preferably, the cement is 525 black cement and the diatomaceous earth model is K812219.
[0011] Preferably, the volume concentration of the sodium alginate solution is 2%, and the amount of sodium alginate added is 20% of the total weight of the powder.
[0012] Preferably, the granulation in step (2) is specifically:
[0013] After starting the granulator, set the speed to 40rpm, and gradually spray distilled water (10% of the total weight of the powder) at a speed of 3mL / s. Then change the speed to 15rpm, pour in distilled water (10% of the total weight), roll the powder into granules, and take it out when the filler particle size is 3-5mm.
[0014] Preferably, the amount of distilled water sprayed during the shade drying process in step (2) is: 50 mL / kg per day based on the weight of the filler.
[0015] The present invention also provides an alkali-modified steel slag adsorption and phosphorus removal filler prepared by the method described in the above technical solution.
[0016] And an alkali-modified steel slag adsorption dephosphorization filler prepared by the method described in the above technical solution or the use of the alkali-modified steel slag adsorption dephosphorization filler in wastewater denitrification and dephosphorization.
[0017] Preferably, the hydraulic retention time when using alkali-modified steel slag adsorption phosphorus removal filler for sewage treatment is 4-10h.
[0018] It can be seen from the above technical solution that, compared with the prior art, the present invention discloses a method for preparing an alkali-modified steel slag adsorption dephosphorization filler, which has the following beneficial effects:
[0019] The alkali-modified steel slag filler and the preparation method thereof in the present invention use steel slag, cement and diatomaceous earth as raw materials, have sufficient reserves and low cost, can achieve the purpose of treating waste with waste, and realize resource utilization of industrial waste;
[0020] The present invention adopts a non-burning method to prepare the filler, which saves energy consumption and further reduces the preparation cost of the filler. At the same time, the pretreatment is simple and the treatment conditions are mild. The surface functional groups of the steel slag are changed by alkali modification to improve the chemical adsorption and ion exchange capabilities, and the phosphorus removal capacity is significantly improved compared with that before modification.
[0021] The present invention provides an optimal ratio of each component, thereby improving the unit processing capacity of the filler, further reducing the cost of the dephosphorization filler, improving the comprehensive performance of the filler, and realizing the resource recycling of steel slag. DETAILED DESCRIPTION
[0022] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Example
[0024] The preparation method of alkali-modified steel slag adsorption dephosphorization filler comprises the following steps:
[0025] (1) Soak steel slag powder with a particle size of 60-80 mesh in a 3 mol / L NaOH solution for 24 h, wash with tap water and dry naturally;
[0026] (2) The steel slag treated in step (1), 525 black cement and K812219 diatomaceous earth are mixed in proportion to form powder, and then a sodium alginate solution (sodium alginate volume concentration of 2%) with a concentration of 20% by weight of the total weight of the powder is added and stirred evenly, and then the mixture is put into a granulator for granulation. The granulation is specifically performed as follows:
[0027] After starting the granulator, set the speed to 40rpm, and gradually spray distilled water (10% of the total weight of the powder) at a speed of 3mL / s. Then change the speed to 15rpm, pour in distilled water (10% of the total weight), roll the powder into granules, and take out the filler when the particle size is 3-5mm;
[0028] The taken out filler is dried in the shade, and during the drying process, an appropriate amount of distilled water is sprayed on it every day for maintenance. The amount of water sprayed is 50mL / kg per day based on the weight of the filler.
[0029] Experimental Example 1
[0030] Design an orthogonal experiment with three factors and three levels. The experimental conditions are as follows:
[0031] Table 1 Orthogonal experimental factors
[0032]
[0033] According to the three-factor three-level orthogonal table, fillers were prepared according to the proportions, and about 0.5g of fillers were accurately weighed and placed in a 50mL centrifuge tube. 50mL of potassium dihydrogen phosphate solution with an initial concentration of 50mg / L was added, and the sample bottle was placed in a shaker with a speed of 130rpm / min and shaken at 28℃ for 24h. After balance, the sample was filtered and sampled with a syringe to measure the phosphorus concentration. The experimental results are as follows:
[0034] Table 2 Orthogonal experiment results
[0035]
[0036]
[0037] From the table above, we can see that the best experimental solution is (A Ⅱ , B Ⅲ , C Ⅲ ), add the second level of factor A, the third level of factor B and the third level of factor C, and calculate their proportions of the total, respectively, to obtain (steel slag: cement: diatomaceous earth = 60.9%: 26.1%: 13.0%).
[0038] Experimental Example 2
[0039] The laboratory was equipped with simulated wastewater with a phosphorus concentration of 50 mg / L. The alkali-modified filler, unmodified filler and pure steel slag filler prepared by the above optimal technical solution were placed respectively. The phosphorus concentration was measured after 24 hours. The equilibrium adsorption amount of the alkali-modified filler was 4.16 mg / g, and the equilibrium adsorption amount of the modified steel slag calculated by the quasi-first-order kinetic model was 3.98 mg / g; the equilibrium adsorption amount of the unmodified filler was 2.96 mg / g, and the equilibrium adsorption amount of the modified steel slag calculated by the quasi-first-order kinetic model was 2.87 mg / g. The equilibrium adsorption amount of the pure steel slag filler was 1.82 g / g, and the equilibrium adsorption amount of the modified steel slag calculated by the quasi-first-order kinetic model was 2.01 mg / g. It was calculated that the adsorption amount of the alkali-modified filler was 1.39 times that of the unmodified filler and 1.98 times that of the pure steel slag filler.
[0040] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments, and the same and similar parts between the embodiments can be referred to each other. The above description of the disclosed embodiments enables professionals and technicians in this field to implement or use the present invention. Various modifications to these embodiments will be obvious to professionals and technicians in this field, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to these embodiments shown in this article, but will comply with the widest range consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing an alkali-modified steel slag adsorption and dephosphorization filler, It is characterized in that The following steps are involved: (1) Soak the steel slag powder in a NaOH solution, wash it with tap water and dry it naturally; (2) The steel slag, cement and diatomaceous earth treated in step (1) are mixed into powder in a weight percentage of 60.9%, 26.1% and 13.0%, and then the sodium alginate solution is added and stirred evenly. The mixture is then put into a granulator for granulation. The prepared filler is dried in the shade and sprayed with distilled water every day for curing during the drying process.
2. The method for preparing an alkali-modified steel slag adsorption dephosphorization filler according to claim 1, It is characterized in that The concentration of the NaOH solution in step (1) is 3 mol / L, and the soaking time is 24 h.
3. The method for preparing an alkali-modified steel slag adsorption dephosphorization filler according to claim 1, It is characterized in that The particle size of the steel slag is 60-80 meshes.
4. The method for preparing an alkali-modified steel slag adsorption and dephosphorization filler according to claim 1, It is characterized in that The cement is 525 black cement and the diatomaceous earth model is K812219.
5. The method for preparing an alkali-modified steel slag adsorption and dephosphorization filler according to claim 1, It is characterized in that The volume concentration of the sodium alginate solution is 2%, and the amount of sodium alginate added is 20% of the total weight of the powder.
6. The method for preparing an alkali-modified steel slag adsorption dephosphorization filler according to claim 1, It is characterized in that The granulation in step (2) is specifically as follows: After starting the granulator, set the speed to 40rpm, and gradually spray distilled water (10% of the total weight of the powder) at a speed of 3mL / s. Then change the speed to 15rpm, pour in distilled water (10% of the total weight), roll the powder into granules, and take it out when the filler particle size is 3-5mm.
7. The method for preparing an alkali-modified steel slag adsorption and dephosphorization filler according to claim 1, It is characterized in that The amount of distilled water sprayed during the drying process in step (2) is: 50 mL / kg per day based on the weight of the filler.
8. An alkali-modified steel slag adsorption phosphorus removal filler prepared by the method according to any one of claims 1 to 7.
9. Use of the alkali-modified steel slag adsorption phosphorus removal filler prepared by the method according to any one of claims 1 to 7 or the alkali-modified steel slag adsorption phosphorus removal filler according to claim 7 in wastewater denitrification and phosphorus removal.
10. The use according to claim 9, It is characterized in that The hydraulic retention time when using alkali-modified steel slag adsorption phosphorus removal filler for sewage treatment is 4-10h.
Citation Information
Patent Citations
Industrial residue based compound dephosphorization material
CN101172687A
Phosphorus removal modified slag haycite and preparation method and application thereof
CN106943991A
Preparation method of sewage dephosphorization filter material and dephosphorization technology
CN107473357A
Phosphorus removal filler and preparation method thereof
CN110526327A
Artificial filler with nitrogen and phosphorus removal function and preparation method thereof
CN112939355A