Bimetal MIL-101 / GO composite material as well as preparation method and application thereof

By doping graphene oxide into MIL-101 (Fe, Cu) materials, a bimetallic MIL-101/GO composite material is formed, which solves the problem of insufficient adsorption capacity of existing MILs materials in removing UO2+ and achieves higher uranium Adsorption capacity and stability, suitable for uranium wastewater treatment.

CN118807705AInactive Publication Date: 2024-10-22NANHUA UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410854706.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing MILs materials have poor adsorption capacity for UO2+ removal from uranium wastewater and cannot meet actual needs.

Method used

A bimetallic MIL-101/GO composite material doped with graphene oxide was designed. By doping graphene oxide inside and on the pores of MIL-101 (Fe, Cu), its adsorption capacity was improved. The preparation method of the composite material includes dissolving FeCl3·6H2O, Cu(NO3)2·3H2O and terephthalic acid in DMF, adding graphene oxide, performing a constant temperature reaction and preparing it by a solvothermal method.

Benefits of technology

It increases the specific surface area and pore volume of the composite material, increases the uranium adsorption capacity, and can maintain high adsorption efficiency under different pH values ​​and temperature conditions. It is suitable for the treatment of uranium wastewater and resource recovery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807705A_ABST
    Figure CN118807705A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of water treatment, and particularly relates to a bimetallic MIL-101 / GO composite material doped with graphene oxide as well as a preparation method and application of the bimetallic MIL-101 / GO composite material. The preparation method comprises the following steps: dissolving ferric chloride, copper nitrate and terephthalic acid in DMF (Dimethyl Formamide), and uniformly stirring to obtain a mixed solution; adding graphene oxide into ethanol, and uniformly stirring to obtain a dispersed solution; mixing the mixed solution and the dispersion solution, putting the mixture into a reaction kettle for reaction, and separating to obtain a solvothermal product; washing the solvothermal product with DMF and absolute ethyl alcohol, and centrifuging to obtain a solid product; and drying the solid product to obtain a final product. The MIL-101 / GO composite material prepared by the invention has a larger specific surface area, more uranium-philic functional groups and more excellent uranyl ion adsorption efficiency, and has a wide application prospect in the practical application of removing uranyl ions in uranium-containing wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water treatment, and specifically relates to a bimetallic MIL-101 / GO composite material doped with graphene oxide, and a preparation method and application thereof. Background Art

[0002] With the widespread application of nuclear energy, uranium mining and smelting will produce a large amount of uranium-containing wastewater. As a radioactive nuclide, uranium has the characteristics of high radioactivity and strong chemical toxicity, which will cause harm to the ecological environment and human health. Therefore, it is necessary to recover and remove UO2 from uranium wastewater. 2+ It is a necessary task. At present, the commonly used methods for treating uranium-containing wastewater mainly include chemical precipitation, filtration, ion exchange, evaporation concentration, adsorption, biological reduction, membrane separation, etc. The adsorption method has the advantages of simple operation, low operating cost and good treatment effect. It has received extensive attention in the treatment of low-concentration radioactive wastewater. The most important thing in the application of adsorption technology is the selection of adsorbent materials.

[0003] MILs (Materials of Institute Lavoisier) is a type of MOFs material that has been widely used and used. Different MILs materials can be synthesized by changing the metal center or using different organic ligands. MOFs materials have the prospect of being used as adsorbents, but the existing MILs materials are not very effective in removing UO2. 2+ The adsorption capacity of the two aspects is poor, far from meeting the requirements for adsorption of UO2 2+ Capacity requirements.

[0004] Therefore, it is necessary to design a new method to recover and remove UO2 from uranium wastewater. 2+ materials. Summary of the invention

[0005] The purpose of the present invention is to provide a bimetallic MIL-101 / GO composite material doped with graphene oxide and a preparation method and application thereof, so as to solve the problem of removing UO2 from the existing MILs material mentioned in the background technology. 2+ The adsorption capacity of all aspects is poor.

[0006] To achieve the above-mentioned object, the present invention provides a bimetallic MIL-101 / GO composite material doped with graphene oxide, comprising a carrier MIL-101 (Fe, Cu) and graphene oxide doped inside the pores of MIL-101 (Fe, Cu) and loaded on the surface of MIL-101 (Fe, Cu).

[0007] The present invention also provides a method for preparing a bimetallic MIL-101 / GO composite material doped with graphene oxide, comprising the following steps:

[0008] Step 1, dissolving FeCl3·6H2O, Cu(NO3)2·3H2O and terephthalic acid in DMF, stirring evenly to obtain a mixed solution;

[0009] Step 2, adding graphene oxide to ethanol and stirring evenly to obtain a dispersed solution;

[0010] Step 3, the mixed solution obtained in step 1 and the dispersed solution obtained in step 2 are mixed evenly and placed in a reaction kettle for constant temperature reaction at 100-150° C. After the reaction is completed, a solvent thermal product is separated;

[0011] Step 4, washing the solvothermal product obtained in step 3 with DMF and anhydrous ethanol, and centrifuging to obtain a solid product;

[0012] Step 5: Dry the solid product obtained in step 4 at 50-70° C. to obtain the final product.

[0013] In a specific embodiment, in step 1, the concentration of FeCl3·6H2O in the mixed solution is 0.173-0.183 mol / L, the concentration of Cu(NO3)2·3H2O is 0.041-0.051 mol / L, and the concentration of terephthalic acid is 0.161-0.171 mol / L.

[0014] In a specific embodiment, in step 2, the mass of graphene oxide added is 2% to 8% of the total mass of FeCl3·6H2O, Cu(NO3)2·3H2O and terephthalic acid.

[0015] In a specific embodiment, in step 3, the volume of the mixed solution obtained in step 1 and the dispersed solution obtained in step 2 accounts for 35-45% of the volume of the reactor.

[0016] In a specific embodiment, in step 3, the isothermal reaction time is 10 to 15 hours; in step 4, the solvent thermal product is washed with DMF and anhydrous ethanol 2 to 5 times respectively; in step 5, the drying time is 12 to 24 hours.

[0017] The present invention also provides a bimetallic MIL-101 / GO composite material doped with graphene oxide prepared according to the aforementioned method for preparing the bimetallic MIL-101 / GO composite material doped with graphene oxide.

[0018] The present invention also provides an application of a bimetallic MIL-101 / GO composite material doped with graphene oxide prepared according to the aforementioned method for preparing the bimetallic MIL-101 / GO composite material doped with graphene oxide in removing uranyl ions from uranium-containing wastewater, wherein the dosage of the bimetallic MIL-101 / GO composite material doped with graphene oxide in the uranium-containing wastewater is 0.1 to 0.6 g / L.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) Compared with the bimetallic MIL-101 (Fe, Cu), the surface of the novel bimetallic MIL-101 (Fe, Cu) / GO composite material prepared in the present invention becomes rougher and the pore volume becomes larger. 3 / g increases to 0.1037~0.1146cm of MIL-101(Fe,Cu) / GO-2~5% 3 / g, the specific surface area also increased from 698.56m 2 / g increases to 711.64~814.70m / g for MIL-101(Fe,Cu) / GO-2~5% 2 / g, and the preparation method is simple and the crystallinity is high.

[0021] (2) The bimetallic MIL-101 (Fe, Cu) / GO composite material doped with graphene oxide prepared by the present invention has abundant uranium-philic oxygen-containing functional groups such as hydroxyl and carboxyl. Compared with the uranium adsorption capacity of MIL-101 (Fe, Cu) of 325.12 mg / g, the uranium adsorption capacity of MIL-101 (Fe, Cu) / GO can reach up to 365.61 mg / g. In addition, under different pH values ​​and different temperature conditions, the uranium adsorption capacity of MIL-101 (Fe, Cu) / GO-2~5% composite material remains higher than that of bimetallic MIL-101 (Fe, Cu), and has broad application prospects in the fields of treatment of uranium-containing wastewater and recovery of uranium resources.

[0022] In addition to the above-described objects, features and advantages, the present invention has other objects, features and advantages. The present invention is further described in detail below. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0024] Figure 1This is the SEM spectrum of MIL-101 (Fe, Cu) obtained in Example 1.

[0025] Figure 2 This is the SEM spectrum of MIL-101(Fe,Cu) / GO-2% obtained in Example 2.

[0026] Figure 3 This is the SEM spectrum of MIL-101(Fe,Cu) / GO-4% obtained in Example 3.

[0027] Figure 4 This is the SEM spectrum of MIL-101(Fe,Cu) / GO-5% obtained in Example 4.

[0028] Figure 5 These are the XRD patterns of MIL-101(Fe,Cu), MIL-101(Fe,Cu) / GO-2%, MIL-101(Fe,Cu) / GO-4%, MIL-101(Fe,Cu) / GO-5% and MIL-101(Fe,Cu) / GO-8% obtained in Examples 1 to 5.

[0029] Figure 6 These are the N2 adsorption-desorption isotherms of graphene oxide and MIL-101(Fe, Cu), MIL-101(Fe, Cu) / GO-2%, MIL-101(Fe, Cu) / GO-4%, and MIL-101(Fe, Cu) / GO-5% obtained in Examples 1 to 4.

[0030] Figure 7 Pore ​​size distribution diagram of graphene oxide and MIL-101(Fe,Cu) / GO-2%, MIL-101(Fe,Cu) / GO-4%, and MIL-101(Fe,Cu) / GO-5% obtained in Examples 1 to 4.

[0031] Figure 8 FTIR spectra of MIL-101(Fe,Cu) / GO-2%, MIL-101(Fe,Cu) / GO-4% and MIL-101(Fe,Cu) / GO-5% obtained in Examples 2 to 4.

[0032] Fig. 9 This is the XPS spectrum of MIL-101(Fe,Cu) / GO-5% obtained in Example 4 before and after the adsorption of uranyl.

[0033] Fig.10 This is the FI-IR spectrum of MIL-101(Fe,Cu) / GO-5% obtained in Example 4 before and after the adsorption of uranyl.

[0034] Fig.11This is a graph showing the adsorption performance of uranyl ions at different initial uranium concentrations for MIL-101(Fe, Cu), MIL-101(Fe, Cu) / GO-2%, MIL-101(Fe, Cu) / GO-4% and MIL-101(Fe, Cu) / GO-5% obtained in Examples 1 to 4.

[0035] Fig.12 This is a graph showing the adsorption performance of uranyl ions under different pH conditions for MIL-101(Fe, Cu), MIL-101(Fe, Cu) / GO-2%, MIL-101(Fe, Cu) / GO-4% and MIL-101(Fe, Cu) / GO-5% obtained in Examples 1 to 4.

[0036] Fig.13 This is a graph showing the adsorption performance of uranyl ions of MIL-101(Fe, Cu), MIL-101(Fe, Cu) / GO-2%, MIL-101(Fe, Cu) / GO-4% and MIL-101(Fe, Cu) / GO-5% obtained in Examples 1 to 4 at different temperatures. DETAILED DESCRIPTION

[0037] The embodiments of the present invention are described in detail below. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0038] The invention provides a bimetallic MIL-101 / GO composite material doped with graphene oxide, comprising a carrier MIL-101 (Fe, Cu) and graphene oxide doped inside the pores of MIL-101 (Fe, Cu) and loaded on the surface of MIL-101 (Fe, Cu).

[0039] Example 1

[0040] Preparation of MIL-101(Fe,Cu):

[0041] 0.831 g of terephthalic acid, 1.461 g of ferric chloride hexahydrate and 0.336 g of copper nitrate trihydrate were added to 30 mL of DMF, stirred at room temperature for 30 min, and then ultrasonicated for 30 min. The obtained mixture was transferred to a 100 mL high-pressure reactor lined with a polytetrafluoroethylene liner, kept at 120°C for 12 h, then taken out, centrifuged three times on a centrifuge with a speed of 10000 r / min, and then washed three times with DMF and anhydrous ethanol, and placed in a 60°C oven to dry until the mass no longer decreased, thereby obtaining MIL-101 (Fe, Cu).

[0042] Example 2

[0043] Preparation of MIL-101(Fe,Cu) / GO-2%:

[0044] 0.831g of terephthalic acid, 1.461g of ferric chloride hexahydrate and 0.336g of copper nitrate trihydrate were added to 30mL of DMF, stirred at room temperature for 30min, and then ultrasonicated for 30min. Then 0.053g of graphene oxide (GO), which accounts for 2% of the total mass of terephthalic acid, ferric chloride hexahydrate and copper nitrate trihydrate, was added to 8mL of anhydrous ethanol and ultrasonicated for 30min. The two were mixed, and the obtained mixture was transferred to a 100mL high-pressure reactor lined with polytetrafluoroethylene liner, kept at 120℃ for 12h, then taken out, centrifuged three times on a centrifuge with a speed of 10000r / min, and then washed three times with DMF and anhydrous ethanol respectively, and placed in a 60℃ oven to dry until the mass no longer decreased, and the MIL-101(Fe,Cu) / GO-2% composite material was obtained.

[0045] Example 3

[0046] Preparation of MIL-101(Fe,Cu) / GO-4%:

[0047] 0.831g of terephthalic acid, 1.461g of ferric chloride hexahydrate and 0.336g of copper nitrate trihydrate were added to 30mL of DMF, stirred at room temperature for 30min, and then ultrasonicated for 30min. Then 0.105g of graphene oxide, which accounts for 4% of the total mass of terephthalic acid, ferric chloride hexahydrate and copper nitrate trihydrate, was added to 8mL of anhydrous ethanol and ultrasonicated for 30min. The two were mixed, and the obtained mixture was transferred to a 100mL high-pressure reactor lined with polytetrafluoroethylene liner, kept at 120℃ for 12h, then taken out, centrifuged three times on a centrifuge with a speed of 10000r / min, and then washed three times with DMF and anhydrous ethanol respectively, and placed in a 60℃ oven to dry until the mass no longer decreased, and the MIL-101(Fe,Cu) / GO-4% composite material was obtained.

[0048] Example 4

[0049] Preparation of MIL-101(Fe,Cu) / GO-5%:

[0050] 0.831g of terephthalic acid, 1.461g of ferric chloride hexahydrate and 0.336g of copper nitrate trihydrate were added to 30mL of DMF, stirred at room temperature for 30min, and then ultrasonicated for 30min. Then 0.132g of graphene oxide, which accounts for 5% of the total mass of terephthalic acid, ferric chloride hexahydrate and copper nitrate trihydrate, was added to 8mL of anhydrous ethanol and ultrasonicated for 30min. The two were mixed, and the obtained mixture was transferred to a 100mL high-pressure reactor lined with a polytetrafluoroethylene liner, kept at 120°C for 12h, then taken out, centrifuged three times on a centrifuge with a speed of 10000r / min, and then washed three times with DMF and anhydrous ethanol, and placed in a 60°C oven to dry until the mass no longer decreased, and the MIL-101 (Fe, Cu) / GO-5% composite material was obtained.

[0051] Example 5

[0052] Preparation of MIL-101(Fe,Cu) / GO-8%

[0053] 0.831g of terephthalic acid, 1.461g of ferric chloride hexahydrate and 0.336g of copper nitrate trihydrate were added to 30mL of DMF, stirred at room temperature for 30min, and then ultrasonicated for 30min. Then 0.210g of graphene oxide, which accounts for 8% of the total mass of terephthalic acid, ferric chloride hexahydrate and copper nitrate trihydrate, was added to 8mL of anhydrous ethanol and ultrasonicated for 30min. The two were mixed, and the obtained mixture was transferred to a 100mL high-pressure reactor lined with polytetrafluoroethylene liner, kept at 120°C for 12h, then taken out, centrifuged three times on a centrifuge with a speed of 10000r / min, and then washed three times with DMF and anhydrous ethanol, and placed in a 60°C oven to dry until the mass no longer decreased, and the MIL-101 (Fe, Cu) / GO-8% composite material was obtained.

[0054] Figures 1 to 4 These are the SEM spectra of MIL-101(Fe,Cu), MIL-101(Fe,Cu) / GO-2%, MIL-101(Fe,Cu) / GO-4% and MIL-101(Fe,Cu) / GO-5% obtained in Examples 1 to 4, respectively. Figure 1 It is shown that MIL-101(Fe,Cu) exhibits a smooth, uniform orthorhombic octahedral structure with sharp corners. Figures 2 to 4 It shows that the surface of the new MIL-101 (Fe, Cu) / GO-2 ~ 5% composite material doped with graphene oxide begins to become rough, and is connected to synthesize a new composite material with a compact structure.

[0055] Figure 5The XRD spectra of MIL-101(Fe,Cu), MIL-101(Fe,Cu) / GO-2%, MIL-101(Fe,Cu) / GO-4%, MIL-101(Fe,Cu) / GO-5% and MIL-101(Fe,Cu) / GO-8% obtained in Examples 1 to 5 are shown in FIG. Figure 5 It can be seen that MIL-101(Fe,Cu) has been successfully synthesized and has a complete and good crystal structure. In addition, the crystal form of MIL-101(Fe,Cu) is almost unaffected by the addition of 2-5% graphene oxide (GO), and the intensity of the diffraction peak decreases when 8% graphene oxide (GO) is added.

[0056] Figure 6 and Figure 7 The N2 adsorption-desorption isotherms and pore size distribution diagrams of graphene oxide and MIL-101(Fe,Cu) / GO-2%, MIL-101(Fe,Cu) / GO-4% and MIL-101(Fe,Cu) / GO-5% obtained in Examples 1 to 4 are shown respectively. Figure 6 and Figure 7 It can be seen that the adsorption of N2 in MIL-101(Fe,Cu) and MIL-101(Fe,Cu) / GO-2~5% composite materials increases rapidly when P / P0=0.0-0.1, belonging to the type I isotherm with H4 hysteresis loop, and there are micropores and mesopores. In addition, the specific surface area of ​​MIL-101(Fe,Cu) / GO-2~5% composite materials (711.64~814.70m 2 / g) is greater than MIL-101(Fe,Cu)(698.56m 2 / g), and the pore volume of MIL-101(Fe,Cu) / GO-2~5% (0.1037~0.1146cm 3 / g) is larger than MIL-101(Fe,Cu)(0.0963cm 3 / g).

[0057] Figure 8 FTIR spectra of MIL-101(Fe,Cu) / GO-2%, MIL-101(Fe,Cu) / GO-4% and MIL-101(Fe,Cu) / GO-5% obtained in Examples 2 to 4. Figure 8 It can be seen that the MIL-101(Fe,Cu) / GO-2~5% composite material has abundant uranium-philic oxygen-containing functional groups at 542 cm -1 and 747cm -1 The absorption peak at 1384-1662 cm -1The peak between them belongs to the characteristic absorption peak of -COOH, at 3439cm -1 The peak at belongs to the absorption peak of -OH.

[0058] Example 6

[0059] This embodiment provides an application of a bimetallic MIL-101 (Fe, Cu) / GO composite material doped with graphene oxide for removing uranyl ions from uranium-containing wastewater.

[0060] The uranium adsorption performance of MIL-101(Fe, Cu), MIL-101(Fe, Cu) / GO-2%, MIL-101(Fe, Cu) / GO-4%, MIL-101(Fe, Cu) / GO-5% and MIL-101(Fe, Cu) / GO-8% obtained in Examples 1 to 5 was compared and analyzed at different initial uranium concentrations. The method is as follows:

[0061] First, use a negligible volume of 0.1 mol / L nitric acid solution or 0.1 mol / L sodium hydroxide solution to control the pH of the entire solution to 5.5. Then, 10 mg of the MIL-101(Fe, Cu), MIL-101(Fe, Cu) / GO-2%, MIL-101(Fe, Cu) / GO-4% and MIL-101(Fe, Cu) / GO-5% adsorbents obtained in Examples 1 to 4 were dispersed in 40 mL of uranium-containing solutions with different initial uranium concentrations, and then transferred to a constant temperature shaker at 25°C and shaken at 230 rpm for 150 minutes. Finally, 1 mL of the supernatant was filtered through a 0.22 um nylon membrane and the concentration of uranyl ions before and after adsorption was detected by azoarsenic III spectrophotometry.

[0062] Specifically, the initial uranium concentrations were 10, 20, 30, 40, 50, 60, 70, and 80 mg / L, respectively.

[0063] Fig. 9 The X-ray photoelectron spectrum of MIL-101(Fe,Cu) / GO-5% obtained in Example 4 before and after uranium adsorption, Fig. 9 The U peak obviously appears in the graphite, indicating that uranium is successfully attached to the composite material. Fig.10 This is the FI-IR spectrum of MIL-101(Fe,Cu) / GO-5% obtained in Example 4 before and after uranium adsorption. Fig.10 MIL-101(Fe,Cu) / GO-5% represents the FI-IR image before uranium adsorption, and MIL-101(Fe,Cu) / GO-5%-U represents the FI-IR image after uranium adsorption. From MIL-101(Fe,Cu) / GO-5%-U, it can be found that the absorption peak of uranyl ion appears at 930cm -1 The successful adsorption of uranium was further confirmed.

[0064] Fig.11 The adsorption performance of MIL-101(Fe,Cu), MIL-101(Fe,Cu) / GO-2%, MIL-101(Fe,Cu) / GO-4% and MIL-101(Fe,Cu) / GO-5% for uranyl ions at different initial uranium concentrations obtained in Examples 1 to 4. It can be clearly seen that compared with the uranium adsorption capacity of 325.12 mg / g of MIL-101(Fe,Cu), the MIL-101(Fe,Cu) / GO-2~5% composite material has a larger uranium adsorption capacity, which can reach 346.56~365.61 mg / g.

[0065] Table 1 is a comparison of the adsorption capacity of uranium for MIL-101(Fe, Cu), MIL-101(Fe, Cu) / GO-2%, MIL-101(Fe, Cu) / GO-4%, MIL-101(Fe, Cu) / GO-5%, MIL-101(Fe, Cu) / GO-8% obtained in Examples 1 to 5 and other MIL-101 and its composites and graphene oxide (GO) and its composites at the optimal pH.

[0066] Table 1 Uranium adsorption capacity of different adsorbent materials

[0067] Adsorption material Optimum pH Adsorption capacity (mg / g) MIL-101(Fe,Cu) 5.5 325.12 MIL-101(Fe,Cu) / GO-2% 5.5 346.56 MIL-101(Fe,Cu) / GO-4% 5.5 351.82 MIL-101(Fe,Cu) / GO-5% 5.5 365.61 MIL-101(Fe,Cu) / GO-8% 5.5 120.21 MIL-101 5.5 20 <![CDATA[MIL-101-NH2]]> 5.5 90 MIL-101-ED 5.5 200 GO 7 94.61 PEI / GO 7 145.14 AS-GO 4 180.6

[0068] It can be seen from Table 1 that when the doping amount of GO is 2-5%, the uranium adsorption capacity of MIL-101(Fe,Cu) / GO-2-5% is significantly higher than that of other MIL-101 and its composites and GO and its composites. When the doping amount of GO is 8%, the uranium adsorption capacity of MIL-101(Fe,Cu) / GO-8% decreases.

[0069] Example 7

[0070] This embodiment provides an application of a bimetallic MIL-101 (Fe, Cu) / GO composite material doped with graphene oxide for removing uranyl ions from uranium-containing wastewater.

[0071] The uranium adsorption performance of MIL-101(Fe, Cu), MIL-101(Fe, Cu) / GO-2%, MIL-101(Fe, Cu) / GO-4% and MIL-101(Fe, Cu) / GO-5% obtained in Examples 1 to 4 was compared and analyzed at different pH values ​​by the following method:

[0072] The method is the same as that of Example 6, except that a negligible volume of 0.1 mol / L nitric acid solution or 0.1 mol / L sodium hydroxide solution is used to control the pH of the 40 mg / L uranium solution to 2-8.

[0073] Fig.12 The adsorption performance of uranyl ions by MIL-101(Fe, Cu), MIL-101(Fe, Cu) / GO-2%, MIL-101(Fe, Cu) / GO-4% and MIL-101(Fe, Cu) / GO-5% obtained in Examples 1 to 4 under different pH conditions is shown. In the pH range of 2 to 8, the uranium adsorption of the MIL-101(Fe, Cu) / GO-2 to 5% composite material is significantly higher than that of MIL-101(Fe, Cu).

[0074] Example 8

[0075] This embodiment provides an application of a bimetallic MIL-101 (Fe, Cu) / GO composite material doped with graphene oxide for removing uranyl ions from uranium-containing wastewater.

[0076] The uranium adsorption performance of MIL-101(Fe, Cu), MIL-101(Fe, Cu) / GO-2%, MIL-101(Fe, Cu) / GO-4% and MIL-101(Fe, Cu) / GO-5% obtained in Examples 1 to 4 was compared and analyzed at different temperatures by the following method:

[0077] The method is the same as that of Example 6, with the only difference being that the MIL-101(Fe,Cu), MIL-101(Fe,Cu) / GO-2%, MIL-101(Fe,Cu) / GO-4% and MIL-101(Fe,Cu) / GO-5% adsorbents obtained in Examples 1 to 4 are subjected to comparative analysis in a 40 mg / L uranium solution at different temperatures.

[0078] Specifically, the temperature settings are 15, 20, 25, 30, 35, 40, and 45°C, respectively.

[0079] Fig.13 The uranyl ion adsorption performance of MIL-101(Fe,Cu), MIL-101(Fe,Cu) / GO-2%, MIL-101(Fe,Cu) / GO-4% and MIL-101(Fe,Cu) / GO-5% obtained in Examples 1 to 4 at different temperatures is shown in FIG. Fig.13 As shown, although the uranium adsorption of all samples decreases with increasing temperature, the uranium adsorption of MIL-101(Fe,Cu) / GO-2~5% composite material is significantly improved compared with that of MIL-101(Fe,Cu).

[0080] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions and substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.

Claims

1. A bimetallic MIL-101 / GO composite material doped with graphene oxide, It is characterized in that It includes a carrier MIL-101 (Fe, Cu) and graphene oxide doped inside the pores of MIL-101 (Fe, Cu) and loaded on the surface of MIL-101 (Fe, Cu).

2. A method for preparing a bimetallic MIL-101 / GO composite material doped with graphene oxide, It is characterized in that The following steps are involved: Step 1: FeCl 3 6H 2 O, Cu(NO 3 ) 2 ·3H 2 O and terephthalic acid are dissolved in DMF and stirred to obtain a mixed solution; Step 2, adding graphene oxide to ethanol and stirring evenly to obtain a dispersed solution; Step 3, the mixed solution obtained in step 1 and the dispersed solution obtained in step 2 are mixed evenly and placed in a reaction kettle for constant temperature reaction at 100-150° C. After the reaction is completed, a solvent thermal product is separated; Step 4, washing the solvothermal product obtained in step 3 with DMF and anhydrous ethanol, and centrifuging to obtain a solid product; Step 5: Dry the solid product obtained in step 4 at 50-70° C. to obtain the final product.

3. The method for preparing the bimetallic MIL-101 / GO composite material doped with graphene oxide according to claim 2, It is characterized in that In step 1, FeCl in the mixed solution 3 6H 2 O concentration is 0.173~0.183mol / L, Cu(NO 3 ) 2 ·3H 2 The concentration of O is 0.041~0.051 mol / L, and the concentration of terephthalic acid is 0.161~0.171 mol / L.

4. The method for preparing the bimetallic MIL-101 / GO composite material doped with graphene oxide according to claim 2, It is characterized in that In step 2, the mass of graphene oxide added is FeCl 3 6H 2 O, Cu(NO 3 ) 2 ·3H 2 O and terephthalic acid mass 2% ~ 8%.

5. The method for preparing the bimetallic MIL-101 / GO composite material doped with graphene oxide according to claim 2, It is characterized in that In the step 3, the volume of the solution obtained by mixing the mixed solution obtained in step 1 and the dispersed solution obtained in step 2 accounts for 35-45% of the volume of the reactor.

6. The method for preparing the bimetallic MIL-101 / GO composite material doped with graphene oxide according to claim 2, It is characterized in that In the step 3, the isothermal reaction time is 10 to 15 hours; in the step 4, the solvent thermal product is washed with DMF and anhydrous ethanol 2 to 5 times respectively; in the step 5, the drying time is 12 to 24 hours.

7. A bimetallic MIL-101 / GO composite material doped with graphene oxide prepared according to the method for preparing a bimetallic MIL-101 / GO composite material doped with graphene oxide according to any one of claims 2 to 6.

8. Application of the bimetallic MIL-101 / GO composite material doped with graphene oxide prepared by the method for preparing the bimetallic MIL-101 / GO composite material doped with graphene oxide according to any one of claims 2 to 6 in removing uranyl ions from uranium-containing wastewater, It is characterized in that The dosage of the bimetallic MIL-101 / GO composite material doped with graphene oxide in uranium-containing wastewater is 0.1-0.6 g / L.

Citation Information

Patent Citations

  • Preparation method of metal organic framework composite graphene oxide matrix ozone catalyst

    CN117619446A