Preparation method and application of molybdenum oxide modified porous biochar material
Ammonium molybdate is combined with porous biochar through the impregnation-calcination method to form molybdenum oxide modified porous biochar, which solves the problem of poor dispersion performance of molybdenum oxide catalyst and achieves high performance and cost reduction of catalytic oxidative desulfurization.
Patent Information
- Application Number
- CN202410804021.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-21
AI Technical Summary
In the existing technology, molybdenum oxide catalysts have poor dispersion performance in catalyzing water and oil two-phase reactions, resulting in insufficient contact between active site aggregation and reaction matrix, and the catalyst synthesis process is complicated. Simplified methods are needed to enrich oxygen vacancies and improve Catalytic activity.
Ammonium molybdate is combined with porous biochar through the impregnation-calcination method, and the calcination temperature is controlled to form molybdenum oxide modified porous biochar, achieving uniform dispersion of molybdenum active sites and generation of oxygen vacancies, utilizing the porous structure and polarity of biochar. groups to improve catalytic performance.
The high-efficiency performance of catalytic oxidation desulfurization is achieved, especially the removal of dibenzothiophene sulfides in fuel, shortening the reaction time, reducing the amount of catalyst, eliminating the extraction stage, and reducing the cost of industrial application.
Smart Images

Figure CN118807729A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a porous biochar material, in particular to a method for preparing a molybdenum oxide modified porous biochar material and application thereof. Background Art
[0002] Previous studies have explored a range of catalysts for ODS, including metal oxides, ionic liquids (ILs), metal-organic frameworks (MOFs), polyoxometalates (POMs), heteropolyacids, noble metals, and deep eutectic solvents. Metal oxides, known for their catalytic activity and stability, are particularly prominent in this area. The defining features of metal oxides include point defects, such as oxygen vacancies (OVs), which have a significant impact on the physical and chemical properties of the materials. Many metal oxides with oxygen vacancies (e.g., MnO2, SnO2, WO3, Co3O4, MoO3) exhibit remarkable catalytic performance. Typically, oxygen vacancies in catalysts are created through heat treatment processes under vacuum or inert atmosphere (He, N2, and Ar), chemical reduction, ion doping, and interface engineering. In particular, molybdenum oxide (MoO X ) is widely used in catalysis due to its simple synthesis, high oxidation ability and unique electronic structure. However, existing techniques for generating vacancies in molybdenum oxides have disadvantages, such as complex synthesis processes, and a simplified method is needed to enrich molybdenum oxides with a large number of oxygen vacancies. In addition, the utilization of molybdenum oxide in catalyzing water and oil two-phase reactions is severely limited due to its poor dispersion properties, resulting in aggregation of active sites and insufficient contact with the reaction matrix. Therefore, there is an urgent need to design catalysts with uniformly dispersed metal oxides to achieve highly active catalysts for ODS. In order to improve MoO X Various supports such as transition metal oxides, SiO2, molecular sieves, carbon, and MOFs have been used to develop MoO X Composite catalysts. Efforts to reduce fuel desulfurization costs and minimize environmental impact have prompted the elimination of the extraction stage. Researchers have focused on preparing amphiphilic catalysts by modifying the surface groups of the support to control polarity.
[0003] As biomass waste increases, disposal costs are also increasing, highlighting the importance of converting waste into useful products in a sustainable manner. As a valuable material, biochar has been widely used in water purification, electrochemical materials, adsorption and homogeneous catalysis. Despite its porosity and abundant active sites, biochar has not been widely used as a catalyst for solvent-free catalysis of ODS due to polarity issues. Based on this, controlling the polarity of biochar and preparing highly active MoO X Catalyst is a key strategy to improve the performance of ODS.
[0004] In summary, in view of the defects of the prior art, the present invention provides a method for preparing a porous biochar material modified by molybdenum oxide and its application. Summary of the invention
[0005] The purpose of the present invention is to provide a preparation method and application of a porous biochar material modified by molybdenum oxide. The porous biochar prepared by the present invention has a size of 34-150 μm and a porous structure. The Mo species is loaded on the surface of the porous biochar by an impregnation-calcination method. During the calcination process, Mo is reduced to form a large number of oxygen vacancies. The uniform dispersion of molybdenum active sites makes the porous biochar material modified by molybdenum oxide as a catalyst show excellent performance in catalytic oxidation desulfurization. At the same time, the surface of the catalyst carrier has a large number of polar groups, which can effectively adsorb sulfur-containing compounds after large polarity oxidation; the preparation process is simple, the raw material source is wide, and the dibenzothiophene sulfide that is difficult to remove in the fuel can be efficiently reduced, the reaction time is shortened, and the amount of catalyst is also reduced. The process does not require an extraction stage, and dibenzothiophene is removed in one step, which reduces the cost of industrial application and has good application prospects in the catalytic oxidation desulfurization of fuel.
[0007] The technical solution of the present invention is a method for preparing a porous biochar material modified by molybdenum oxide. Ammonium molybdate is combined with porous biochar by impregnation, heated to 400-600°C at a heating rate of 4-6°C / min, calcined for 1-3h under the protection of nitrogen, and naturally cooled to 15-30°C to obtain a porous biochar material modified by molybdenum oxide.
[0008] During the calcination process: when the calcination temperature is higher than 200°C, ammonium molybdate decomposes to form MoO3; when the calcination temperature reaches 400°C, the porous biochar begins to reduce molybdenum oxide, converting part of Mo into 6+ Restored to Mo 5+ , active site Mo 5+ There are oxygen vacancies. With the increase of calcination temperature, Mo 5+ The content gradually increases; when the calcination temperature reaches 500℃, Mo 5+ The content reaches the highest, and the oxygen vacancies decrease the most. As the temperature continues to rise, Mo 5+ Continue to be restored to Mo 4+ , at this time Mo 4+ The content increased, Mo 5+ Gradually decreases, that is, oxygen vacancies gradually decrease; when the calcination temperature is greater than 600℃, Mo 5+ It decreases sharply, that is, the oxygen vacancies decrease sharply.
[0009] In the above-mentioned method for preparing the molybdenum oxide modified porous biochar material, the molybdenum oxide modified porous biochar material comprises: 5+It accounts for 49.1-56% of the molybdenum content.
[0010] In the aforementioned method for preparing the molybdenum oxide modified porous biochar material, ammonium molybdate is combined with the porous biochar by impregnation, specifically, 0.4-2.4 g / L of ammonium molybdate solution is added to the porous biochar material, stirred for 20-28 hours, centrifuged at 9000-11000 r / min for 4-6 minutes, and vacuum dried at 60-80°C for 10-14 hours.
[0011] In the aforementioned method for preparing the molybdenum oxide modified porous biochar material, the mass ratio of ammonium molybdate to porous biochar is 25:4-24; and the particle size of the porous biochar is 34-150 μm.
[0012] In the aforementioned method for preparing the molybdenum oxide modified porous biochar material, the porous biochar is prepared by the following method:
[0013] Wash 1g of biochar with water for 2-4 times, dry at 60-80℃ for 10-14h, add it to 40mL of 25-75g / L potassium hydroxide solution, stir, dry at 60-80℃ for 10-14h, heat to 650-750℃ at a heating rate of 4-6℃ / min, calcine for 1-3h under nitrogen protection, cool naturally to 15-30℃, wash with water for 2-4 times, dry at 60-100℃ for 1-12h, ball mill and sieve to obtain porous biochar.
[0014] In the preparation method of the aforementioned molybdenum oxide modified porous biochar material, 1 g of biochar is washed with water three times, dried at 70°C for 12 hours, added to 40 mL of 50 g / L potassium hydroxide solution, stirred, dried at 70°C for 12 hours, heated to 700°C at a heating rate of 5°C / min, calcined for 2 hours under the protection of nitrogen, naturally cooled to 20°C, washed with water three times, dried at 80°C for 6 hours, ball milled, and sieved to obtain porous biochar.
[0015] In the aforementioned method for preparing the molybdenum oxide modified porous biochar material, the biochar is prepared by the following method:
[0016] After the biomass is crushed, it is heated to 450-550°C at a heating rate of 4-6°C / min, calcined for 1-3h under the protection of nitrogen, and naturally cooled to 15-30°C to obtain biochar.
[0017] The application of the molybdenum oxide modified porous biochar material is the application of the molybdenum oxide modified porous biochar material as a catalyst in fuel desulfurization.
[0018] In the application of the aforementioned molybdenum oxide modified porous biochar material, the molybdenum oxide modified porous biochar material is used as a catalyst, the catalyst is dispersed in an n-octane solution containing dibenzothiophene, and fuel desulfurization is performed at 40-70°C.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The present invention combines ammonium molybdate with porous biochar by impregnation, heats to 400-600°C at a heating rate of 4-6°C / min, and calcines for 1-3 hours under the protection of nitrogen, and naturally cools to 15-30°C to obtain a molybdenum oxide modified porous biochar material. In the impregnation calcination method, when the calcination temperature is higher than 200°C, ammonium molybdate decomposes to form MoO3, and the Mo species is highly dispersed on the surface of the porous biochar in the form of MoO3. When the calcination temperature reaches 400°C, the porous biochar begins to reduce the molybdenum oxide, and part of the Mo 6+ Restored to Mo 5+ , active site Mo 5+ There are oxygen vacancies. With the increase of calcination temperature, Mo 5+ The content gradually increases; when the calcination temperature reaches 500℃, Mo 5+ The content reaches the highest, and the oxygen vacancies decrease the most. As the temperature continues to rise, Mo 5+ Continue to be restored to Mo 4+ , at this time Mo 4+ The content increased, Mo 5+ Gradually decreases, that is, oxygen vacancies gradually decrease; when the calcination temperature is greater than 600℃, Mo 5+ The present invention achieves Mo by controlling the calcination temperature at 400-600°C. 5+ It accounts for 49.1-56% of the molybdenum content.
[0021] 2. The present invention adds 0.4-2.4g / L ammonium molybdate solution to porous biochar material, stirs for 20-28h, centrifuges at 9000-11000r / min for 4-6min, and vacuum dries at 60-80℃ for 10-14h. The mass ratio of ammonium molybdate to porous biochar is 25:4-24. The particle size of the porous biochar is 34-150μm. Mo species are loaded by impregnation. The precursor of Mo (i.e. ammonium molybdate) relies on the surface energy of porous biochar for loading. Therefore, the concentration of ammonium molybdate is an important factor in determining the Mo content. In addition to the concentration of ammonium molybdate, the particle size determines the size of the surface energy of porous biochar, which in turn affects the overall content of Mo.
[0022] 3. The porous biochar of the present invention is prepared by the following method: 1g of biochar is washed with water 2-4 times, dried at 60-80°C for 10-14h, added to 40mL of potassium hydroxide solution with a concentration of 25-75g / L, stirred, dried at 60-80°C for 10-14h, calcined for 1-3h at a heating rate of 4-6°C / min, heated to 650-750°C, and protected by nitrogen, cooled naturally to 15-30°C, washed with water 2-4 times, dried at 60-100°C for 1-12h, ball milled, and sieved to obtain porous biochar. The porous biochar is produced by treating biochar with KOH, and its mechanism is that KOH reacts with carbon to generate gas, and the gas overflows to form pores, so the porous biochar is a carrier rich in microporous / mesoporous structure, which provides a prerequisite for the loading of Mo in the later stage. Different KOH masses determine the specific surface area of the porous biochar. The reaction of KOH with carbon consumes carbon to form pores. On the other hand, as the amount of KOH increases, the polar groups (i.e. -OH) on the surface of the porous biochar increase, which leads to an increase in the polarity of the catalyst carrier (within the scope of this patent). The catalyst carrier changes from lipophilic to amphiphilic (meaning that it can be dispersed in the oil phase, and the polar groups can make it contact with hydrogen peroxide (aqueous phase)) and then to hydrophilic. The polarity of porous biochar is not the larger the better. It should be between lipophilic and hydrophilic to form amphiphilic porous biochar, so that the catalyst prepared later can be dispersed in the oil phase and can contact with hydrogen peroxide to achieve catalytic oxidation desulfurization. The porous biochar treated by ball milling in the present invention has a particle size of 34-150μm and has more surface energy on the surface, which is used to disperse Mo species. However, too many Mo species will agglomerate, so it is crucial to control the Mo content.
[0023] 4. The molybdenum oxide modified porous biochar material prepared by the present invention is used as a catalyst in catalytic oxidation desulfurization to achieve a DBT removal rate of 99.6%. In the reaction process, the oxidant is hydrogen peroxide, and the reaction is an endothermic reaction. As the temperature rises, the reaction will accelerate, but too high a temperature will cause the decomposition of hydrogen peroxide, and the reaction will be ineffective. Therefore, the catalyst is dispersed in an n-octane solution containing dibenzothiophene, and the fuel oil is desulfurized at 40-70°C; the catalyst needs to be washed with acetonitrile for repeated use.
[0024] 5. At the same time, the polar groups (-OH) on the surface of the porous biochar prepared by the present invention can be used to adsorb the product (DBTO2) after DBT oxidation. The catalyst after adsorbing the oxidation product can be washed by acetonitrile to achieve the reuse of the catalyst. At the same time, since the oxidized sulfur-containing compounds are adsorbed, no further treatment is required, thereby achieving a one-step removal of DBT. The catalyst is an amphiphilic catalyst, which can be dispersed in the oil phase and can contact with the oxidant hydrogen peroxide to form an active substance, thereby eliminating the extraction stage and reducing the cost of industrial application. It has good application prospects in the catalytic oxidation desulfurization of fuel.
[0025] In summary, the porous biochar prepared by the present invention has a size of 34-150 μm and a porous structure. The Mo species is loaded on the surface of the porous biochar by impregnation-calcination. During the calcination process, Mo is reduced to form a large number of oxygen vacancies. The molybdenum active sites are evenly dispersed, so that the molybdenum oxide modified porous biochar material as a catalyst exhibits excellent performance in catalytic oxidation desulfurization. At the same time, the catalyst carrier surface has a large number of polar groups, which can effectively adsorb highly polar oxidized sulfur-containing compounds; the preparation process is simple, the raw material source is wide, and the dibenzothiophene sulfides that are difficult to remove in the fuel can be efficiently reduced, the reaction time is shortened, and the amount of catalyst is also reduced. The process does not require an extraction stage, and the one-step removal of dibenzothiophene is achieved, which reduces the cost of industrial application and has a good application prospect in the catalytic oxidation desulfurization of fuel. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The scanning electron microscope (SEM) and transmission electron microscope (TEM) images of the porous biochar prepared in Examples 1-3 of the present invention and the molybdenum oxide modified porous biochar material prepared in Examples 4-6; wherein a, b and c are SEM images of the porous biochar; d is the SEM image of the molybdenum oxide modified porous biochar material, e and f are TEM images of the molybdenum oxide modified porous biochar material, g and h are TEM images of the molybdenum oxide modified porous biochar material and the corresponding C, O, Mo mapping images; i is the HRTEM image of the molybdenum oxide modified porous biochar material;
[0027] Figure 2 It is the contact angle test graph of the preparation (CBC1, CBC2, CBC3) of Example 1-3 of the present invention;
[0028] Figure 3 It is a performance diagram of catalytic oxidation desulfurization prepared in Examples 1-3 of the present invention (CBC1, CBC2, CBC3);
[0029] Figure 4It is the XPS spectra of the preparations of Examples 4-6 of the present invention (Mo / CBC2-400, Mo / CBC2-500, Mo / CBC2-600);
[0030] Figure 5 It is the catalytic oxidation desulfurization performance diagram of Examples 4-6 of the present invention (Mo / CBC2-400, Mo / CBC2-500, Mo / CBC2-600);
[0031] Figure 6 It is the catalytic oxidation desulfurization performance diagram of the comparative examples 1-2 of the present invention (Mo / CBC2-300, Mo / CBC2-700);
[0032] Figure 7 It is the cycle performance diagram of (Mo / CBC2-500) prepared in Example 5 of the present invention. DETAILED DESCRIPTION
[0033] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.
[0034] Example 1. The porous biochar of the present invention is prepared by the following method: 1 g of biochar is washed twice with water, dried at 60°C for 10 h, added to 40 mL of 25 g / L potassium hydroxide solution, stirred, dried at 60°C for 10 h, heated to 650°C at a heating rate of 4°C / min, and calcined for 1 h under the protection of nitrogen, naturally cooled to 15°C, washed twice with water, dried at 60°C for 1 h, ball milled, and sieved to obtain porous biochar. The particle size of the porous biochar is 34 μm, recorded as CBC1.
[0035] Example 2. The porous biochar of the present invention is prepared by the following method: 1 g of biochar is washed with water three times, dried at 70°C for 12 h, added to 40 mL of 50 g / L potassium hydroxide solution, stirred, dried at 70°C for 12 h, heated to 700°C at a heating rate of 5°C / min, calcined for 2 h under nitrogen protection, naturally cooled to 20°C, washed with water three times, dried at 80°C for 6 h, ball milled, and sieved to obtain porous biochar with a particle size of 100 μm, recorded as CBC2.
[0036] Example 3: The porous biochar of the present invention is prepared by the following method: 1g of biochar is washed with water 4 times, dried at 80°C for 14h, added to 40mL of 75g / L potassium hydroxide solution, stirred, dried at 80°C for 14h, heated to 750°C at a heating rate of 6°C / min, calcined for 3h under the protection of nitrogen, cooled naturally to 30°C, washed with water 4 times, dried at 100°C for 12h, ball milled, and sieved to obtain porous biochar. The particle size of the porous biochar is 150μm, recorded as CBC3.
[0037] Experimental proof:
[0038] Specific desulfurization process: dissolve dibenzothiophene (DBT) in a certain amount of n-octane to obtain a 300ppm DBT n-octane solution, which is the simulated oil. Place 50mg of the catalyst in a 100mL three-necked flask, add 10mL of 300ppm simulated oil, control the reaction temperature to 60°C, add a certain amount of hydrogen peroxide (O / S is 6), the reaction time is 40min, sample every 5min, centrifuge the sample at 10000r / min for 5min, take out the supernatant, send it to the WK-2D microcoulomb sulfur analyzer to determine its sulfur content, and calculate the desulfurization rate by the following formula:
[0039] η=[(C0-C0) / C0]×100%
[0040] Where η is the desulfurization rate, C0 is the original simulated oil concentration, and C is the final simulated oil concentration. The solid separated by centrifugation was washed with acetonitrile 2-3 times and then centrifuged and dried for later circulation experiments.
[0041] The removal rates of DBT of CBC1, CBC2 and CBC3 prepared in Examples 1-3 of the present invention at 15 min are as follows:
[0042] catalyst DBT removal rate Example 1 15.8% Example 2 17.8% Example 3 12.6%
[0043] The tests in Examples 1-3 show that the polarity of the porous biochar increases with the increase of KOH (within the scope of this patent), namely the contact angles (CA) of CBC1 (92.7°), CBC2 (60.5°) and CBC2 (28.1°). However, the greater the polarity of the porous biochar, the more favorable it is to the reaction. The appropriate polarity of the porous biochar provides a prerequisite for the preparation of subsequent catalysts. The amphiphilic porous biochar can be dispersed in the oil phase (DBT n-octane solution) and can be in contact with hydrogen peroxide (oxidant). Among them, the polarity of CBC2 is between lipophilic and hydrophilic. It is an amphiphilic porous biochar, which can be dispersed in the oil phase and can be in contact with hydrogen peroxide. CBC2 has good polarity, a desulfurization performance of 17.8%, and has the best performance among the above examples, so the porous biochar preparation example 2 is the best example.
[0044] Example 4: A method for preparing a porous biochar material modified by molybdenum oxide. Ammonium molybdate is combined with the porous biochar by impregnation. The porous biochar is CBC2 prepared in Example 2. The material is heated to 400°C at a heating rate of 4°C / min and calcined for 1 hour under the protection of nitrogen. The material is naturally cooled to 15°C to obtain a porous biochar material modified by molybdenum oxide, which is denoted as Mo / CBC2-400. In the porous biochar material modified by molybdenum oxide: Mo 5+ It accounts for 49.1% of the molybdenum element.
[0045] The ammonium molybdate is combined with the porous biochar by impregnation. Specifically, 0.4 g / L ammonium molybdate solution is added to the porous biochar material, stirred for 20 hours, centrifuged at 9000 r / min for 4 minutes, and vacuum dried at 60° C. for 10 hours. The mass ratio of ammonium molybdate to porous biochar is 25:4.
[0046] Example 5: A method for preparing a porous biochar material modified by molybdenum oxide. Ammonium molybdate is combined with the porous biochar by impregnation. The porous biochar is CBC2 prepared in Example 2. The material is heated to 500°C at a heating rate of 5°C / min and calcined for 2 hours under the protection of nitrogen. The material is naturally cooled to 25°C to obtain a porous biochar material modified by molybdenum oxide, which is denoted as Mo / CBC2-500. In the porous biochar material modified by molybdenum oxide: Mo 5+ It accounts for 56% of the molybdenum content.
[0047] The ammonium molybdate is combined with the porous biochar by impregnation. Specifically, 2 g / L ammonium molybdate solution is added to the porous biochar material, stirred for 24 hours, centrifuged at 10,000 r / min for 5 minutes, and vacuum dried at 70° C. for 2 hours. The mass ratio of ammonium molybdate to porous biochar is 25:14.
[0048] Example 6: A method for preparing a porous biochar material modified by molybdenum oxide. Ammonium molybdate is combined with the porous biochar by impregnation. The porous biochar is CBC2 prepared in Example 2. The material is heated to 600°C at a heating rate of 6°C / min and calcined for 3 hours under the protection of nitrogen. The material is naturally cooled to 30°C to obtain a porous biochar material modified by molybdenum oxide, which is denoted as Mo / CBC2-600. In the porous biochar material modified by molybdenum oxide: Mo 5+ It accounts for 52.6% of the molybdenum content.
[0049] The ammonium molybdate is combined with the porous biochar by impregnation. Specifically, 2.4 g / L ammonium molybdate solution is added to the porous biochar material, stirred for 28 hours, centrifuged at 11000 r / min for 6 minutes, and vacuum dried at 80°C for 14 hours. The mass ratio of ammonium molybdate to porous biochar is 25:24.
[0050] Comparative Example 1: (300°C)
[0051] Ammonium molybdate was combined with porous biochar by impregnation. The porous biochar was CBC2 prepared in Example 2. The porous biochar was heated to 300°C at a heating rate of 5°C / min and calcined for 2 hours under the protection of nitrogen. The porous biochar was naturally cooled to 25°C to obtain a molybdenum oxide modified porous biochar material, which was recorded as Mo / CBC2-300. In the molybdenum oxide modified porous biochar material, Mo 5+ It accounts for 0% of the molybdenum element.
[0052] The ammonium molybdate is combined with the porous biochar by impregnation. Specifically, 2 g / L ammonium molybdate solution is added to the porous biochar material, stirred for 24 hours, centrifuged at 10,000 r / min for 5 minutes, and vacuum dried at 70° C. for 2 hours. The mass ratio of ammonium molybdate to porous biochar is 25:14.
[0053] Comparative Example 2: (700°C)
[0054] Ammonium molybdate was combined with porous biochar by impregnation. The porous biochar was CBC2 prepared in Example 2. The porous biochar was heated to 700°C at a heating rate of 5°C / min and calcined for 2 hours under the protection of nitrogen. The porous biochar was naturally cooled to 25°C to obtain a molybdenum oxide modified porous biochar material, which was recorded as Mo / CBC2-700. In the molybdenum oxide modified porous biochar material, Mo 5+ It accounts for 40% of the molybdenum content.
[0055] The ammonium molybdate is combined with the porous biochar by impregnation. Specifically, 2 g / L ammonium molybdate solution is added to the porous biochar material, stirred for 24 hours, centrifuged at 10,000 r / min for 5 minutes, and vacuum dried at 70° C. for 2 hours. The mass ratio of ammonium molybdate to porous biochar is 25:14.
[0056] Application examples:
[0057] Specific desulfurization process: dissolve dibenzothiophene (DBT) in a certain amount of n-octane to obtain a 300ppm DBT n-octane solution, which is the simulated oil. Place 50mg of the catalyst in a 100mL three-necked flask, add 10mL of 300ppm simulated oil, control the reaction temperature to 60°C, add a certain amount of hydrogen peroxide (O / S is 6), the reaction time is 40min, sample every 5min, centrifuge the sample at 10000r / min for 5min, take out the supernatant, send it to the WK-2D microcoulomb sulfur analyzer to determine its sulfur content, and calculate the desulfurization rate by the following formula:
[0058] η=[(C0-C0) / C0]×100%
[0059] Where η is the desulfurization rate, C0 is the original simulated oil concentration, and C is the final simulated oil concentration. The solid separated by centrifugation was washed with acetonitrile 2-3 times and then centrifuged and dried for later circulation experiments.
[0060] The DBT removal rates of Mo / CBC2-400, Mo / CBC2-500, Mo / CBC2-600, Mo / CBC2-300 and Mo / CBC2-700 prepared in Examples 4-5 and Comparative Examples 1-2 at 15 min are as follows:
[0061] catalyst DBT removal rate Example 4 98.1%% Example 5 99.6% Example 6 98.5% Comparative Example 1 92.5% Comparative Example 2 94.2%
[0062] The desulfurization efficiencies of Mo / CBC2-400, Mo / CBC2-500 and Mo / CBC2-600 in Examples 4-6 are 94.7%, 99.6% and 98.1% respectively. According to the catalytic oxidation desulfurization performance, Mo / CBC2-500 in Example 5 is the best example. The desulfurization efficiencies of Examples 4-6 are higher than those of Comparative Examples 1 and 2.
[0063] Experimental proof:
[0064] 1. Figure 1 The scanning electron microscope (SEM) and transmission electron microscope (TEM) images of the porous biochar prepared in Examples 1-3 of the present invention and the molybdenum oxide modified porous biochar material prepared in Examples 4-6; wherein a, b and c are SEM images of the porous biochar; d is the SEM image of the molybdenum oxide modified porous biochar material, e and f are TEM images of the molybdenum oxide modified porous biochar material, g and h are TEM images of the molybdenum oxide modified porous biochar material and the corresponding C, O, Mo mapping images; i is the HRTEM image of the molybdenum oxide modified porous biochar material; through Figure 1 It can be seen that the porous biochar prepared by oxygen-limited pyrolysis is in the shape of strips ( Figure 1 a), the pore structure is orderly. However, after KOH activation, many cracks appeared on the surface of CBC2 ( Figure 1 b) This is because during the high temperature activation process, KOH reacts with carbon, causing the pore walls of CBC to be corroded and damaged, forming more micro / mesopores. In order to explore the changes in element content, such as Figure 1 As shown in c, the tubular structure of CBC2 disappeared after ball milling, and the particle size decreased. The size of most particles was about 2-5 μm. 3-X The particle shape and size before and after do not change much ( Figure 1 (de)). exist Figure 1f It can also be observed that Mo atoms are uniformly distributed on the surface of CBC2. The surface content of Mo atoms is about 3.92wt% ( Figure 1 h) and are evenly dispersed. In addition, the MoO 3-X The size of the Figure 1 g). Compared with the atomic radius of Mo (0.14nm), MoO 3-X The size of the molybdenum species indicates that it is well dispersed by the porous biochar support. The corresponding high-resolution transmission electron microscopy (HRTEM) image shows an obvious interplanar spacing of 0.342 nm, which is consistent with the (-111) interplanar spacing of the MoO2 phase. These SEM and TEM images clearly show that the Mo species is highly dispersed on the CBC2 support, confirming the successful preparation of the molybdenum oxide modified porous biochar material of the present invention.
[0065] 2. Figure 2 It is the contact angle test diagram of CBC1, CBC2 and CBC3 prepared in Examples 1-3, where a is the contact angle test of CBC1, b is CBC2, and c is the contact angle test of CBC3. The polarity of porous biochar continues to increase with the increase of KOH (within the scope of this patent), and the contact angles (CA) of CBC1 (92.7°), CBC2 (60.5°) and CBC2 (28.1°). Within the scope of this patent, as the mass of KOH increases, the polarity of porous biochar increases, but it is not the case that the larger the polarity of porous biochar, the better. In catalytic oxidation desulfurization, the polarity of the catalyst must be between lipophilic and hydrophilic. CBC2 has the best polarity, and an amphiphilic porous biochar is generated, which can be dispersed in the oil phase and can also contact with hydrogen peroxide.
[0066] 3. Figure 3 The catalytic oxidation desulfurization performance diagram of (CBC1, CBC2 and CBC3) prepared in Examples 1-3 of the present invention shows that although CBC2 has good polarity, its desulfurization performance is only 17.8% due to the lack of active substances. After analyzing its polarity and desulfurization performance, it is determined that Example 2 is the best example in the preparation conditions of porous biochar.
[0067] 4. Figure 4 The XPS spectra of the catalysts prepared in Examples 4-6 (Mo / CBC2-400, Mo / CBC2-500, and Mo / CBC2-600) of the present invention are analyzed in detail. The six fitting peaks of Mo 3d are at 235.9, 234.8, 233.1, 232.7, 231.8, and 229.8 eV, respectively, which can be attributed to Mo. 6+ 3d 3 / 2 、Mo 5+ 3d 3 / 2 、Mo4+ 3d 3 / 2 、Mo 6+ 3d 5 / 2 、Mo 5+ 3d 5 / 2 and Mo 4+ 3d 5 / 2 As the calcination temperature increases from 400°C to 600°C, MoO 3-X Surface Mo 5+ The ratio of Mo increases first and then decreases. 6+ The ratio of MoO2 has a tendency to increase first and then decrease. Porous biochar can reduce Mo species and generate oxygen vacancies. The number of oxygen vacancies is affected by the calcination temperature. A series of MoO2 with rich surface OVs were successfully synthesized. 3-X The above results indicate that porous biochar can reduce Mo species to form oxygen vacancies at high temperatures, and the oxygen vacancy content can be controlled by changing the calcination temperature.
[0068] 5. Figure 5 It is the catalytic oxidation desulfurization performance diagram of Examples 4-6 of the present invention (Mo / CBC2-400, Mo / CBC2-500, Mo / CBC2-600); Figure 5 It can be seen that the desulfurization efficiencies of Mo / CBC2-400, Mo / CBC2-500 and Mo / CBC2-600 are 94.7%, 99.6% and 98.1% respectively. The correlation analysis between the surface Mo species ratio and the desulfurization rate shows that Mo 5+ It is strongly positively correlated with the desulfurization rate, while Mo 4+ and Mo 6+ Negatively correlated. 5+ The presence of species can accelerate the desulfurization rate.
[0069] 6. Figure 6 It is the catalytic oxidation desulfurization performance diagram of the comparative example 1-2 of the present invention (Mo / CBC2-300, Mo / CBC2-700), Figure 6 The catalytic oxidation desulfurization performance of Comparative Examples 1-2 can be seen in the figure, where the desulfurization performance of Comparative Example 1 is 92.5%, and the desulfurization performance of Comparative Example 2 is 94.2%. This is because Mo 5+ It is the main active substance in the catalytic reaction. When the temperature is below 400, carbon cannot reduce Mo species to form low-valent Mo. However, as the temperature increases, Mo is over-reduced by carbon. 4+ Increase will also lead to a decrease in catalytic performance.
[0070] 7. Figure 7This is a cycle performance diagram of (Mo / CBC2-500) prepared in Example 5 of the present invention, and the stability of the Mo / CBC2-500 catalyst is evaluated through a cycle experiment. It is worth noting that after 5 cycles of recycling, the desulfurization capacity of the spent catalyst (without acetonitrile washing) is only 36.62%, while the desulfurization rate of the regenerated catalyst (washed with acetonitrile) does not decrease significantly after 5 repeated uses, and still meets the allowable sulfur content in the fuel.
[0071] In summary, the preparation conditions of the present invention are mild, the process is simple, the raw material price is low, and it is easy to operate. The porous biochar reduces molybdenum species to form a large number of vacancies, which can effectively remove aromatic sulfides that are difficult to remove from fuel. Ball milling shortens the reaction time, reduces the amount of catalyst, and has good cycle stability. The catalyst of the present invention is amphiphilic, eliminates the extraction stage, simplifies the desulfurization process, and reduces the cost of industrial application. At the same time, it is applicable to different biomass and has a good application prospect in the catalytic oxidation adsorption desulfurization of fuel.
Claims
1. A method for preparing a porous biochar material modified by molybdenum oxide, characterized in that: Ammonium molybdate is combined with porous biochar by impregnation, heated to 400-600°C at a heating rate of 4-6°C / min, calcined for 1-3h under the protection of nitrogen, and naturally cooled to 15-30°C to obtain a molybdenum oxide modified porous biochar material.
2. The method for preparing the molybdenum oxide modified porous biochar material according to claim 1, characterized in that: In the molybdenum oxide modified porous biochar material: Mo 5+ It accounts for 49.1-56% of the molybdenum content.
3. The method for preparing the molybdenum oxide modified porous biochar material according to claim 1, characterized in that: The ammonium molybdate is combined with the porous biochar by impregnation, specifically, 0.4-2.4 g / L ammonium molybdate solution is added to the porous biochar material, stirred for 20-28 hours, centrifuged at 9000-11000 r / min for 4-6 minutes, and vacuum dried at 60-80° C. for 10-14 hours.
4. The method for preparing the molybdenum oxide modified porous biochar material according to claim 1, characterized in that: The mass ratio of the ammonium molybdate to the porous biochar is 25:4-24; and the particle size of the porous biochar is 34-150 μm.
5. The method for preparing the molybdenum oxide modified porous biochar material according to claim 1, characterized in that: The porous biochar is prepared by the following method: Wash 1g of biochar with water for 2-4 times, dry at 60-80℃ for 10-14h, add it to 40mL of 25-75g / L potassium hydroxide solution, stir, dry at 60-80℃ for 10-14h, heat to 650-750℃ at a heating rate of 4-6℃ / min, calcine for 1-3h under nitrogen protection, cool naturally to 15-30℃, wash with water for 2-4 times, dry at 60-100℃ for 1-12h, ball mill and sieve to obtain porous biochar.
6. The method for preparing the molybdenum oxide modified porous biochar material according to claim 5, characterized in that: The method comprises washing 1 g of biochar with water for 3 times, drying at 70°C for 12 h, adding it to 40 mL of 50 g / L potassium hydroxide solution, stirring it, drying it at 70°C for 12 h, heating it to 700°C at a heating rate of 5°C / min, calcining it for 2 h under the protection of nitrogen, naturally cooling it to 20°C, washing it with water for 3 times, drying it at 80°C for 6 h, ball milling it, and sieving it to obtain porous biochar.
7. The method for preparing the molybdenum oxide modified porous biochar material according to claim 5, characterized in that: The biochar is prepared by the following method: After the biomass is crushed, it is heated to 450-550°C at a heating rate of 4-6°C / min, calcined for 1-3h under the protection of nitrogen, and naturally cooled to 15-30°C to obtain biochar.
8. The use of the molybdenum oxide modified porous biochar material according to any one of claims 1 to 7, characterized in that: The molybdenum oxide modified porous biochar material is used as a catalyst in fuel desulfurization.
9. The use of the molybdenum oxide modified porous biochar material according to claim 8, characterized in that: The molybdenum oxide modified porous biochar material is used as a catalyst, the catalyst is dispersed in an n-octane solution containing dibenzothiophene, hydrogen peroxide is used as an oxidant, and fuel oil desulfurization is performed at 40-70° C. The catalyst needs to be washed with acetonitrile for repeated use.
Citation Information
Patent Citations
Preparation method for supported Mo-based oxidation and desulfurization catalyst
CN102294236A
High-selectivity fuel adsorption and desulfurization agent of bamboo source porous biomass carbon
CN106824068A
Preparation method of modified biochar and modified biochar
CN113145076A
Hydrodesulfurization catalyst as well as preparation method and application thereof
CN113145103A
2D lamellar structure silica-based desulfurization catalyst and preparation method thereof
CN114849777A
Cited By
Solid catalyst and preparation method of L-ribose
CN119098207A