Precious metal single-component dehydrogenation catalyst as well as preparation method and application thereof

By modifying the carrier to load the precious metal catalyst, the problems of low selectivity and short life of the existing LOHCs addition and dehydrogenation catalysts are solved, and efficient, long-term hydrogen purity improvement and cost reduction are achieved, which is suitable for the addition and dehydrogenation process of LOHCs.

CN118807736APending Publication Date: 2024-10-22WUHAN HYNERTECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310390755.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing LOHCs addition and dehydrogenation catalysts have problems such as low selectivity, many side reactions, and short lifespan, resulting in poor hydrogen purity and increased costs. The high activity and high price of precious metal catalysts make their applications prone to agglomeration, activity attenuation, and difficulty in recycling. problem.

Method used

Using a single-component precious metal dehydrogenation catalyst, the precious metal is loaded through a modified carrier, such as Ru, Rh, Pd, Ag, Pt or Au, combined with modified Al2O3, SiO2, TiO2, CeO2, MgO, ZrO2 or silicon-aluminum composite carrier. It is prepared through steps such as impregnation, drying, roasting and hydrogen atmosphere reduction to improve the activity and stability of the catalyst.

Benefits of technology

The long-term cyclic application of the LOHCs addition and dehydrogenation process is realized, the hydrogen purity and the sustainable service life of the catalyst are improved, side reactions and costs are reduced, and the preparation process is simple and scalable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004175640340000081
    Figure BDA0004175640340000081
  • Figure BDA0004175640340000091
    Figure BDA0004175640340000091
  • Figure HDA0004175640350000011
    Figure HDA0004175640350000011
Patent Text Reader

Abstract

The invention discloses a noble metal single-component dehydrogenation catalyst as well as a preparation method and application thereof. The catalyst is a modified carrier loaded with noble metal, the noble metal is Ru, Rh, Pd, Ag, Pt or Au, and the modified carrier is modified Al2O3, modified SiO2, modified TiO2, modified CeO2, modified MgO, modified ZrO2 or a modified silicon-aluminum composite carrier. According to the invention, LOHCs and a dehydrogenation catalyst are improved by selecting a proper system, an auxiliary agent and a preparation method, so that the activity and selectivity are effectively improved, side reactions are reduced, and long-period cyclic and dehydrogenation application of LOHCs is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalysts, and particularly relates to a noble metal single-component dehydrogenation catalyst and a preparation method and application thereof. Background Art

[0002] The basis of the "hydrogen economy" is to use hydrogen as a new clean energy for storage, transportation, and power generation. Therefore, hydrogen needs to be produced in tons. Traditional hydrogen storage and transportation technologies such as high-pressure gaseous hydrogen storage, low-temperature liquefied hydrogen storage, and solid hydrogen storage restrict the application of hydrogen energy due to high costs and safety requirements. Organic liquid hydrogen storage materials (LOHCs) are a type of hydrogen storage material with a fully reversible hydrogenation-dehydrogenation cycle. In recent years, they have become the focus of hydrogen research due to their reversibility and zero CO2 emissions. The principle is to achieve hydrogen storage (chemical bonding) through the reversible reaction and hydrogenation reaction of unsaturated liquid organic matter such as olefins, alkynes or aromatic hydrocarbons and hydrogen, and to achieve hydrogen release through dehydrogenation reactions, making hydrogen storage and release safe and efficient. Since the hydrogenated Hn-LOHCs compounds have similar properties to crude oil derivatives (such as diesel and gasoline), they can be transported over long distances using existing liquid fuel transportation logistics (such as pipelines, ships, and trucks). Therefore, it is very feasible to transition to the "hydrogen economy" with existing infrastructure.

[0003] Organic liquid hydrogen storage materials mainly include traditional organic liquid hydrogen storage materials and new organic liquid hydrogen storage materials. Traditional organic liquid hydrogen storage molecules are mainly aromatic benzene-cyclohexane, toluene-methylcyclohexane, naphthalene-decalin, dibenzyltoluene-perhydrodibenzyltoluene systems. Such traditional organic liquid hydrogen storage molecules can change the properties of organic compounds by changing the number of substituents, bridging methods, etc. At present, there are still problems such as high temperature required for the dehydrogenation process and easy occurrence of side reactions such as cracking and disproportionation, resulting in reduced purity of the generated hydrogen. New organic liquid hydrogen storage materials are mainly condensed aromatic molecules containing heteroatoms (O, N, S), among which N-heterocyclic systems such as quinoline and its derivatives, indole and its derivatives, carbazole and its derivatives are the most studied new organic liquid hydrogen storage materials. The hydrogen storage capacity is usually expressed in mass fraction (wt%), and the reaction enthalpy ΔH in kJ / mol H2 represents the energy value released in the hydrogenation reaction, and the energy value required in the dehydrogenation reaction. For example, the dehydrogenation temperature of methylcyclohexane used by Chiyoda in Japan is as high as 350℃~400℃. The selection of LOHCs with more than 4wt% hydrogen storage and low reaction enthalpy (-15kcal / mol H2≤ΔH≤-10kcal / mol H2) has low external energy demand, and the hydrogen storage capacity can meet most of the actual needs, thereby improving the overall efficiency of the dehydrogenation process and facilitating the industrial application of the hydrogen energy industry chain.

[0004] The key to realizing the hydrogenation and dehydrogenation of LOHCs is to add dehydrogenation catalysts. Catalysts can not only reduce the reaction temperature, but also improve the reaction rate of chemical hydrogen storage technology. The hydrogenation and dehydrogenation of LOHCs are reversible reactions, following Le Chatelier's principle. Hydrogenation releases heat and dehydrogenation absorbs heat. By changing the temperature, pressure and concentration of the reactants, the equilibrium direction of the reaction can be effectively controlled to move toward hydrogenation or dehydrogenation. Under pressurized conditions, the catalyst adsorbs LOHCs, causing the unsaturated bonds to vibrate and break, and H2 is added; under normal pressure conditions, the catalyst adsorbs Hn-LOHCs, CH vibrates and breaks, and H2 is removed.

[0005] The essence of the hydrogenation and dehydrogenation process is the bond vibration breaking to achieve H2 storage and release. In theory, it can catalyze hydrogenation and dehydrogenation at the same time, but because the hydrogenation and dehydrogenation reaction pathways are opposite, based on cost, yield and other considerations, the choice of catalyst is generally different. Hydrogenation catalysts mainly include nickel catalysts, palladium and platinum catalysts, ruthenium catalysts and rhodium catalysts. Conventional hydrogenation catalysts are nickel metal catalysts with aluminum as the carrier, while for deep aromatics catalysis, precious metal catalysts are the first choice. Dehydrogenation catalysts are mainly precious metal catalysts, non-precious metal catalysts and mixed catalysts. Precious metal catalysts have high activity and can improve the dehydrogenation efficiency of organic liquid hydrogen storage materials. In theory, catalysts that can be used for hydrogenation can also be used for dehydrogenation, but in fact, the reaction pathways of hydrogenation and dehydrogenation processes are opposite, so it is very demanding to meet the requirements of catalysts for both hydrogenation and dehydrogenation processes. Most of the applicable bifunctional catalysts are based on precious metals as the main components, mostly for the research of Pt, Pd, and Ir, and are rarely used in practice. Hydrogenation and dehydrogenation bifunctional catalysts based on non-precious metal elements have not been used.

[0006] The currently commonly used LOHCs dehydrogenation catalysts have problems such as low selectivity, many side reactions, and short life, which lead to large LOHCs losses, increased costs, and poor hydrogen purity. To address these problems, we have improved the LOHCs dehydrogenation catalyst by selecting suitable systems, additives, and preparation methods to effectively improve the activity and selectivity, reduce side reactions, and realize the long-term cyclic dehydrogenation application of LOHCs dehydrogenation.

[0007] Precious metals are highly active and expensive, and their application content is generally low. Most of the current precious metal LOHCs dehydrogenation catalysts will experience problems such as agglomeration, activity decay, and deactivation after long-term use. They also have complex preparation methods, low selectivity, poor stability, difficulty in recycling and reuse, are environmentally unfriendly, and have high costs. Summary of the invention

[0008] The purpose of the present invention is to provide a single-component noble metal dehydrogenation catalyst and a preparation method and application thereof in view of the defects of the prior art.

[0009] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a single-component noble metal dehydrogenation catalyst, wherein the catalyst is a modified carrier loaded with noble metal; the noble metal is Ru, Rh, Pd, Ag, Pt or Au, and the modified carrier is modified Al2O3, modified SiO2, modified TiO2, modified CeO2, modified MgO, modified ZrO2 or a modified silicon-aluminum composite carrier.

[0010] Furthermore, the mass ratio of the noble metal to the modified carrier is 0.1% to 20%.

[0011] A method for preparing the above-mentioned noble metal single-component dehydrogenation catalyst comprises the following steps: configuring a soluble salt of the noble metal into a metal impregnation solution, loading the impregnated modified carrier, aging, drying, calcining in an inert gas atmosphere, nitrogen replacement, hydrogen atmosphere reduction, and passivation in an atmosphere containing a small amount of oxygen to obtain a catalyst with a modified carrier loaded with the noble metal.

[0012] Furthermore, the loading conditions are as follows: the immersion time is 10 min to 12 h, the aging time is 4 to 72 h, the drying temperature is 40 to 150 ° C, the drying time is 30 min to 36 h, the inert gas is nitrogen or argon, the calcination temperature in the inert gas atmosphere is 200 to 800 ° C, the calcination time is 1 to 24 h, the calcination heating rate is 1 ° C / min to 6 ° C / min, the hydrogen content in the hydrogen atmosphere reduction is 10% to 100%, and the oxygen content in the passivation atmosphere is 0.1% to 15%.

[0013] Furthermore, the modified carrier is prepared by the following steps: dissolving the carrier modifier to obtain a modified liquid, impregnating the carrier with the modified liquid, and performing impregnation, aging, drying, and calcining in an inert gas atmosphere to obtain a modified carrier; the carrier is a macroporous alumina, a silica molecular sieve, TiO2, CeO2, MgO, ZrO2, or a silicon-aluminum composite carrier, and the carrier is spherical in shape, with a diameter of 0.5 to 5 mm, a pore size of 8 to 20 nm, and a specific surface area of ​​150 to 550 m 2 / g, pore volume is 0.35~1.5cm 3 / g; strength is 5-100N / grain, abrasion is 0.01%-0.5%, and bulk density is 0.5-1.5g / cm 3 . .

[0014] Further, the carrier modifier includes:

[0015] (1) Soluble salts of one or more metals selected from Mg, Ca, Sr, Ba and W, in an amount of 0.1% to 5% of the mass of the carrier;

[0016] (2) one or more of B, N, P, Br, and I, in an amount of 0.1% to 10% of the carrier mass;

[0017] (3) one or more of Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, and Lu, with the amount being 0.1% to 5% of the carrier mass;

[0018] (4) Modification aid, the amount used is 0.01% to 50% of the carrier mass.

[0019] Furthermore, the modification aid is one or more of a water-soluble organic matter, a surfactant, and a sol; wherein the water-soluble organic matter is polyvinyl pyrrolidone, urea, a soluble azide salt, urea, thiourea, dicyandiamide, methanol, ethanol, propanol, butanol or ethylene glycol; the surfactant is a cationic surfactant or a nonionic surfactant, wherein the cationic surfactant is dodecyldimethylbenzylammonium chloride, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide or polyquaternium-16, and the nonionic surfactant is polyethylene glycol octylphenyl ether, dodecanol polyoxyethylene ether, tridecanol polyoxyethylene ether, nonylphenol polyoxyethylene ether, alkylphenol polyoxyethylene ether, polyether F127 or polyether P123; the sol is silica sol or aluminum sol.

[0020] Furthermore, the solvent used to dissolve the carrier modifier is deionized water, a small molecule alcohol, an acid or a base, or a mixture of two or more thereof.

[0021] Furthermore, the carrier is macroporous alumina, silica molecular sieve, TiO2, CeO2, MgO, ZrO2 or a silicon-aluminum composite carrier.

[0022] Furthermore, the modification conditions of the carrier are: impregnation time 10min~12h, aging time 4~72h, drying temperature 40~150°C, drying time 30min~36h, inert gas is nitrogen or argon, the calcination temperature in inert gas atmosphere is 200~800°C, the calcination time is 1~24h, and the heating rate is 1°C / min~6°C / min.

[0023] An application of the above-mentioned single-component noble metal plus dehydrogenation catalyst as a catalyst in a reversible hydrogenation hydrogen storage system, wherein the reversible hydrogenation hydrogen storage system includes one or a mixture of two or more π-conjugated reversible hydrogenation hydrogen storage materials; the π-conjugated reversible hydrogenation hydrogen storage material, at 25°C and 1atm, releases 10 to 15kcal of heat per 1mol of H2 stored, that is, -15kcal / mol H2≤ΔH≤-10kcal / mol H2; and the hydrogen storage density after complete hydrogenation is greater than 4% of the mass of the hydrogen storage material; the π-conjugated reversible hydrogenation hydrogen storage material is solid or liquid, and has a melting point of less than 80°C.

[0024] The noble metal single-component dehydrogenation catalyst prepared by the present invention has the following advantages:

[0025] 1. The self-made carrier has a higher specific surface area, providing more adsorption sites for precious metal atoms and clusters;

[0026] 2. The homemade carrier is modified by adding metal components that are beneficial to metal dispersion, non-metallic components that help to confine and anchor precious metal atoms and clusters, and rare earth metal components that prevent pore collapse, sintering, and resist poisoning during the preparation and calcination process, so that the precious metal catalyst can retain high activity and be stable for a long time.

[0027] 3. Due to high dispersibility and confinement effect, the catalyst's anti-poisoning performance is improved, and it can be activated and regenerated under certain conditions, with its performance restored to more than 98% of its initial state, enabling ultra-long-term sustainable use and recycling.

[0028] 4. The preparation process is simple and scalable, with less wastewater and waste residue, economical and efficient, high catalytic LOHCs dehydrogenation efficiency, few side reactions, high hydrogen purity, and long-term stable use. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 These are electron microscope photos of the unmodified SiO2 molecular sieve and the modified SiO2 molecular sieve carrier loaded with precious metals and dehydrogenated in the comparative example and Example 2. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiment of the present application will be clearly and completely described below in combination with the embodiment of the present application. Obviously, the described embodiment is only a part of the embodiment of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work should fall within the scope of protection of the present application.

[0031] It should be noted that the terms "including" and "having" and any variations thereof in the specification and claims of the present application are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units that are not explicitly listed or inherent to these processes, methods, products or apparatuses.

[0032] 1. Catalyst components: precious metal single component A, modified carrier B;

[0033] Precious metal component A: one of Ru, Rh, Pd, Ag, Pt, Au. The above precious metal components have rich electronic structures, extremely high catalytic effects, and are widely used in industry, but have poor reusability. The content is 0.1% to 20%, and the content is calculated by the mass ratio of the element mass to the mass ratio of the carrier B;

[0034] Carrier B: one of modified Al2O3, modified SiO2, modified TiO2, modified CeO2, modified MgO, modified ZrO2, and modified silicon-aluminum composite carriers; the above metal oxides have good mechanical strength and abundant pores that can be closely combined with active metal components;

[0035] Carrier materials: homemade macroporous alumina, homemade silica molecular sieve, homemade TiO2, homemade CeO2, homemade MgO, homemade ZrO2, homemade silicon-aluminum composite carrier

[0036] Specific parameters of the self-made carrier: spherical shape, diameter of 0.5-5mm, pore size of 8-20nm, specific surface area of ​​150-550m 2 / g, pore volume is 0.35-1.5cm 3 / g; strength is 5-100N / grain, abrasion is 0.01%-0.5%, and bulk density is 0.5-1.5g / cm 3 .

[0037] Support modifier C: contains four components, among which the metal component can also participate in the catalytic process as an active component or auxiliary agent. Because the unmodified support loaded with precious metal components is very likely to cause irreversible phenomena such as metal component aggregation and maturation, pore collapse, carbon deposition, poisoning and even breakage during repeated long-term heating, targeted modification treatment is carried out.

[0038] ①Soluble salts of one or more metal elements such as Mg, Ca, Sr, Ba, W, etc., with a content of 0.1% to 5%; can enrich the surface oxide structure, adjust the acid center, and prevent carbon deposition;

[0039] ②One or more of the non-metallic elements such as B, N, P, Br, I, etc. can be added in combination with the metals in ①③, with a content of 0.1% to 10%; these non-metallic elements can combine with or form coordination with precious metals to fix metal atoms and clusters, help high dispersion and improve stability;

[0040] ③ Rare earth elements: one or more of Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Lu, with a content of 0.1% to 5%; rare earth metals can improve the thermal stability and mechanical strength of the catalyst, prevent pore collapse, and also help to disperse the precious metals; and the synergistic effect of rare earth metals and precious metal components can effectively improve the anti-poisoning ability;

[0041] ④ Modification aid: one or more of water-soluble organic matter, surfactant, and sol, with a content of 0.01% to 50%; it makes each component evenly dispersed during the dissolution process;

[0042] Water-soluble organic matter: polyvinyl pyrrolidone, urea, soluble azide salts, urea, thiourea, dicyandiamide, alcohols (methanol, ethanol, propanol, butanol, ethylene glycol), etc.

[0043] Surfactants: cationic surfactants such as dodecyl dimethyl benzyl ammonium chloride, hexadecyl trimethyl ammonium chloride, octadecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium bromide (CTAB), polyquaternium-16, polyethylene glycol octyl phenyl ether, dodecanol polyoxyethylene ether (C 12 E3, C 12 E5, C 12 E7, C 12 E9), tridecanol polyoxyethylene ether (C13E3), nonylphenol polyoxyethylene ether (NP-7, NP-10), alkylphenol polyoxyethylene ether (OP), polyether F127, polyether P123 and other nonionic surfactants;

[0044] Sol: silica sol, aluminum sol;

[0045] 2. Preparation method: impregnation method. Because the amount of precious metal used is small, the impregnation method can prevent the loss of precious metals and can fully disperse them, and the preparation process is simple.

[0046] 1. Dissolve the four components in the carrier modifier. The amount of each component is calculated based on the ratio of element mass to carrier mass. ① component 0.1%~5%, ② component 0.1%~10%, ③ component 0.1%~5%, ④ component 0.01%~50%. The solvent can be one or more of deionized water, small molecule alcohol (ethanol, ethylene glycol), acid (hydrochloric acid, nitric acid), and alkali (ammonia water) to obtain a modified solution.

[0047] 2. The modified carrier B is obtained by impregnating the selected homemade macroporous alumina, homemade silica molecular sieve, homemade TiO2, homemade CeO2, homemade MgO, homemade ZrO2 or homemade silicon-aluminum composite carrier with the modified liquid, and then calcining the carrier in an inert gas atmosphere such as nitrogen and argon after impregnation, aging, drying and nitrogen, argon and the like.

[0048] Modification conditions: impregnation time 10min~12h, aging time 4h~72h, drying temperature 40℃~150℃, drying time 30min~36h, calcination at 200℃~800℃ in an inert gas atmosphere such as nitrogen and argon, calcination time 1h~24h, heating rate 1℃ / min~6℃ / min;

[0049] 3. If there is a difficult-to-co-soluble component among the four components, a modified liquid can be prepared separately, and steps 1 and 2 can be repeated 1 to 4 times until all modified components are impregnated into the carrier.

[0050] 4. The soluble salt of the precious metal component A is prepared into a metal impregnation solution according to the content of the component A of 0.1% to 20%, and the modified carrier B is impregnated with the solution. After aging, drying, and calcination in an inert gas atmosphere, nitrogen replacement, hydrogen atmosphere reduction, and passivation in an atmosphere containing a small amount of oxygen, a catalyst product of the modified carrier B loaded with precious metal A is obtained.

[0051] Load preparation conditions: impregnation time 10min~12h, aging time 4h~72h, drying temperature 40℃~150℃, drying time 30min~36h, calcination at 200℃~800℃ in an inert gas atmosphere such as nitrogen and argon, calcination time 1h~24h, heating rate 1℃ / min~6℃ / min; hydrogen accounts for 10%~100% in the hydrogen atmosphere, and oxygen accounts for 0.1%~15% in the oxygen atmosphere;

[0052] Catalyst product requirements: The content of the main oxide of the carrier in the carrier B is 70-98%; other components are calculated by the ratio of element mass to carrier mass, the content of precious metal A is 0.1-20%, the content of metal elements such as Mg, Ca, Sr, Ba, W, Zr is 0.1%-5%; the content of non-metallic elements such as B, C, N, P, Cl, Br, I is 0.1%-2%; the content of rare earth elements such as Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Lu is 0.01-5%

[0053] 3. Application method:

[0054] The prepared modified carrier-loaded noble metal dehydrogenation catalyst can be used for hydrogenation of a reversible hydrogenation hydrogen storage system and dehydrogenation of its hydrogenation product.

[0055] Application example: taking fixed bed and reactor applications as examples, the hydrogenation raw material and dehydrogenation raw material are respectively exemplified by N-propylcarbazole and fully hydrogenated N-propylcarbazole, but the actual application is not limited to this.

[0056] Fixed bed hydrogenation reaction conditions: catalyst filling height 10 ~ 30cm, liquid space velocity: 0.3 / h ~ 2.0 / h, reaction temperature: 140 ℃ ~ 250 ℃, reaction pressure: 3MPa ~ 9MPa, hydrogenation conversion rate can reach more than 99%, complete hydrogenation product 60% ~ 98%, stable cycle time can reach 5000h.

[0057] Reactor hydrogenation conditions: the ratio of catalyst to reversible hydrogenation hydrogen storage system is 1:10-1:20, reaction temperature is 140°C-240°C, reaction pressure is 3MPa-9MPa, reaction time is 2h-10h, hydrogenation conversion rate can reach more than 99%, and complete hydrogenation product is 90%-99%.

[0058] Fixed bed dehydrogenation reaction conditions: dehydrogenation raw materials: catalyst filling height 10 ~ 30cm, liquid space velocity: 0.3 / h ~ 2.0 / h, reaction temperature 160 ℃ ~ 260 ℃, reaction pressure less than 3MPa, dehydrogenation conversion rate can reach more than 99%, complete dehydrogenation product 60% ~ 98%, stable cycle time can reach 5000h, if longer use, only simple activation is required.

[0059] Reactor dehydrogenation conditions: the ratio of catalyst to reversible hydrogenation hydrogen storage system is 1:5-1:20, reaction temperature is 160°C-240°C, reaction pressure is normal pressure, reaction time is 1h-10h, hydrogenation conversion rate can reach more than 99%, and complete dehydrogenation product is 70%-99%.

[0060] 4. Application object requirements

[0061] 1. The reversible hydrogenation hydrogen storage system is one or more π-conjugated reversible hydrogenation hydrogen storage materials; or a combination of one or more π-conjugated reversible hydrogenation hydrogen storage materials and other substances, and the other substances are regarded as solvents or auxiliary materials that do not participate in hydrogenation and dehydrogenation;

[0062] 2. The π-conjugated reversible hydrogenation hydrogen storage material is a π-conjugated compound. At 25°C and 1atm, the heat released by the π-conjugated compound for storing 1 mol of H2 is 10-15kcal, that is, -15kcal / mol H2≤ΔH≤-10kcal / mol H2; and the hydrogen storage density after complete hydrogenation should be greater than 4wt%; the dehydrogenation of LOHCs within this reaction enthalpy range has low external energy requirements, avoiding excessive energy requirements for the dehydrogenation process. The hydrogen storage density range is conducive to actual industrial applications, and if the hydrogen storage density is too low, the actual application efficiency will deteriorate.

[0063] Example 1

[0064] Modify 100g of self-made macroporous alumina carrier, and record the contents of other components in terms of mass ratio with the carrier. Modifier component ① weighs salt containing 0.1g Mg (such as magnesium nitrate, magnesium chloride, magnesium sulfate), and salt containing 2g Ba (such as barium chloride, barium nitrate); Modifier component ② weighs carbon material containing 10g C (such as fullerene, sugar), and substance containing 1g Br (such as ammonium bromide); Modifier component ③ weighs soluble salt containing 0.1g La (such as lanthanum nitrate), and soluble salt containing 2g Ce (such as cerium nitrate); Modifier component ④ weighs 0.5g hexadecyltrimethylammonium bromide (CTAB), 2g aluminum sol, and 5g ethylene glycol; Components ①②③④ can be mixed with water and stirred to obtain a modified solution without being dissolved separately;

[0065] 100 g of the homemade macroporous alumina carrier was impregnated with the modified solution for 6 h, aged for 20 h, dried at 60-120 °C for 24 h, and calcined at 300-500 °C in a nitrogen atmosphere for 8 h at a heating rate of 2-5 °C / min to obtain a modified alumina carrier;

[0066] Weigh a soluble Ru salt (such as ruthenium chloride) containing 1g of Ru, add deionized water to dissolve it to obtain an impregnation solution, impregnate 100g of the modified alumina carrier for 3h, age it for 20h, dry it at 100℃ for 24h, calcine it at 400℃ in a nitrogen atmosphere for 8h, and heat it at a rate of 5℃ / min. After calcination, replace it with nitrogen, reduce it at 300℃ in a 10% hydrogen atmosphere for 12h, and passivate it in a 0.5% oxygen atmosphere for 2h to obtain a modified Al2O3-loaded Ru catalyst (1%Ru / modified Al2O3).

[0067] Example 2

[0068] Modify 100g SiO2 molecular sieve, the content of other components is recorded by mass ratio with the carrier, modifier component ① weighs zirconium salt (such as zirconium nitrate) containing 2g Zr; modifier component ② weighs compounds containing 3g B (such as boric acid); modifier component ③ weighs compounds containing 0.1g Y (such as yttrium oxide), modifier component ④ weighs 5g soluble azide salt, 2g aluminum sol. Components ①②④ can be mixed with water to obtain modified solution 1, and component ③ is dissolved and diluted with hydrochloric acid or nitric acid to obtain modified solution 2.

[0069] 100g SiO2 molecular sieve was impregnated with modified solution 1 for 4h, aged for 18h, dried at 70℃ for 48h, calcined at 600℃ in nitrogen atmosphere for 5h with a heating rate of 2℃ / min, and then impregnated with modified solution 2;

[0070] Weigh a soluble Pd salt (such as palladium nitrate) containing 0.5g Pd, add nitric acid and deionized water to dissolve it to obtain an impregnation solution, impregnate 100g of the modified SiO2 molecular sieve carrier for 1h, age it for 20h, dry it at 120℃ for 8h, calcine it at 400℃ in a nitrogen atmosphere for 8h, and heat it at a rate of 5℃ / min. After calcination, replace it with nitrogen, reduce it at 300℃ in a 10% hydrogen atmosphere for 12h, and passivate it in a 0.5% oxygen atmosphere for 3h to obtain a modified SiO2-loaded Pd catalyst (0.5% Pd / modified SiO2).

[0071] Example 3

[0072] Modify 100g of self-made ZrO2 carrier, and record the contents of other components in terms of mass ratio with the carrier. Modifier component ① weighs a salt containing 5g W (such as ammonium metatungstate) and a salt containing 0.2g Sr (such as strontium chloride); modifier component ② weighs a substance containing 1g I (such as iodate); modifier component ③ weighs a soluble salt containing 0.1g Nd (such as niobium oxalate); modifier component ④ weighs 10g urea and 5g polyether F127; components ①②③④ can be mixed with water and stirred to obtain a modified solution;

[0073] 100 g of the homemade ZrO2 carrier was impregnated with the modified solution for 3 h, aged for 8 h, dried at 120 °C for 10 h, and calcined at 500 °C in a nitrogen atmosphere for 8 h at a heating rate of 3 °C / min to obtain a modified alumina carrier;

[0074] Weigh a soluble Pt salt (such as platinum chloride) containing 1g of Pt, add hydrochloric acid and deionized water to dissolve it to obtain a Pd impregnation solution, impregnate 100g of modified ZrO2 carrier for 5h, age for 28h, dry at 130℃ for 12h, calcine at 450℃ in a nitrogen atmosphere for 5h, with a heating rate of 5℃ / min, replace with nitrogen after calcination, reduce at 450℃ in a 10% hydrogen atmosphere for 12h, and passivate in a 0.5% oxygen atmosphere for 4h to obtain a modified ZrO2-loaded Pt catalyst (1% Pt / modified ZrO2).

[0075] Comparative Example 1

[0076] Weigh a soluble Pd salt (such as palladium nitrate) containing 0.5g Pd, add nitric acid and deionized water to dissolve to obtain an impregnation solution, impregnate 100g unmodified SiO2 molecular sieve for 1h, age for 20h, dry at 120℃ for 8h, calcine at 400℃ in a nitrogen atmosphere for 8h, with a heating rate of 5℃ / min, replace with nitrogen after calcination, reduce at 300℃ in a 10% hydrogen atmosphere for 12h, and passivate in a 0.5% oxygen atmosphere for 3h to obtain an unmodified SiO2-loaded Pd catalyst (0.5% Pd / SiO2).

[0077] Comparative Example 1 Unmodified SiO2 molecular sieve carrier loaded with precious metals after dehydrogenation ( Figure 1Left, the particles aggregate and grow to a size of 20-40 nm), Example 2 Modified SiO2 molecular sieve carrier loaded with precious metals and dehydrogenated (right, the particles are evenly distributed and the size is still concentrated in 3-5 nm)

[0078] Catalyst dehydrogenation cycle test

[0079] The N-ethylcarbazole system was selected, and two fixed bed reactors were used for hydrogenation and dehydrogenation respectively. The raw material N-ethylcarbazole was first hydrogenated, and the first dehydrogenation used the N-ethylcarbazole hydrogenation product, and the second hydrogenation used the dehydrogenation product, and so on, to achieve the hydrogenation and dehydrogenation cycle, liquid space velocity: 0.3 / h, hydrogenation: 200℃, 7Mpa, dehydrogenation: 220℃ normal pressure. The values ​​in the table are the lowest values ​​in the cycle process.

[0080] By comparison, it can be found that the dehydrogenation conversion rate, selectivity and life of the modified support are greatly improved (Table 1).

[0081] Table 1

[0082]

[0083]

[0084] It should be noted that the various embodiments of the present application are only for the purpose of explaining the present invention and cannot limit the present invention. It should also be known to those skilled in the art that the present embodiment only uses specific examples to elaborate on the principles and implementation methods of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the principles of the present invention should all be within the scope of protection of the present invention.

Claims

1. A noble metal single-component dehydrogenation catalyst, characterized in that: The catalyst is a modified carrier loaded with a noble metal; the noble metal is Ru, Rh, Pd, Ag, Pt or Au, and the modified carrier is a modified Al2O3, modified SiO2, modified TiO2, modified CeO2, modified MgO, modified ZrO2 or a modified silicon-aluminum composite carrier.

2. The noble metal single-component dehydrogenation catalyst according to claim 1, characterized in that: The mass ratio of the noble metal to the modified carrier is 0.1% to 20%.

3. A method for preparing the noble metal single-component dehydrogenation catalyst according to claim 1 or 2, characterized in that The following steps are involved: The soluble salt of the precious metal is configured into a metal impregnation solution, loaded on a modified carrier after impregnation, aged, dried, calcined in an inert gas atmosphere, replaced with nitrogen, reduced in a hydrogen atmosphere, and passivated in an atmosphere containing a small amount of oxygen to obtain a catalyst with the precious metal loaded on the modified carrier.

4. The preparation method according to claim 3, characterized in that: The loading conditions are as follows: the immersion time is 10 min to 12 h, the aging time is 4 to 72 h, the drying temperature is 40 to 150° C., the drying time is 30 min to 36 h, the inert gas is nitrogen or argon, the temperature of the inert gas atmosphere calcination is 200 to 800° C., the calcination time is 1 to 24 h, the calcination heating rate is 1° C. / min to 6° C. / min, the hydrogen content in the hydrogen atmosphere reduction is 10% to 100%, and the oxygen content in the passivation atmosphere is 0.1% to 15%.

5. The preparation method according to claim 3, characterized in that: The modified carrier is prepared by the following steps: dissolving the carrier modifier to obtain a modified liquid, impregnating the carrier with the modified liquid, and performing impregnation, aging, drying, and calcining in an inert gas atmosphere to obtain the modified carrier; the carrier is a macroporous alumina, a silica molecular sieve, TiO2, CeO2, MgO, ZrO2 or a silicon-aluminum composite carrier, and the carrier is spherical in shape, with a diameter of 0.5 to 5 mm, a pore size of 8 to 20 nm, and a specific surface area of ​​150 to 550 m 2 / g, pore volume is 0.35~1.5cm 3 / g; strength is 5-100N / grain, abrasion is 0.01%-0.5%, and bulk density is 0.5-1.5g / cm 3 .

6. The preparation method according to claim 5, characterized in that: The carrier modifier comprises: (1) Soluble salts of one or more metals selected from Mg, Ca, Sr, Ba, and W, in an amount of 0.1% to 5% of the mass of the carrier; (2) One or more metals selected from B, N, P, Br, and I, in an amount of 0.1% to 10% of the mass of the carrier; (3) one or more of Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, and Lu, with the amount being 0.1% to 5% of the carrier mass; (4) Modification aid, the amount used is 0.01% to 50% of the carrier mass.

7. The preparation method according to claim 6, characterized in that: The modification auxiliary agent is one or more of water-soluble organic matter, surfactant and sol; wherein the water-soluble organic matter is polyvinyl pyrrolidone, urea, soluble azide salt, urea, thiourea, dicyandiamide, methanol, ethanol, propanol, butanol or ethylene glycol; the surfactant is a cationic surfactant or a nonionic surfactant, wherein the cationic surfactant is dodecyl dimethyl benzyl ammonium chloride, hexadecyl trimethyl ammonium chloride, octadecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium bromide or polyquaternium-16, and the nonionic surfactant is polyethylene glycol octyl phenyl ether, dodecanol polyoxyethylene ether, tridecanol polyoxyethylene ether, nonylphenol polyoxyethylene ether, alkylphenol polyoxyethylene ether, polyether F127 or polyether P123; the sol is silica sol or aluminum sol.

8. The preparation method according to claim 5, characterized in that: The solvent used to dissolve the carrier modifier is one or a mixture of two or more of ion water, small molecule alcohol, acid or alkali.

9. The preparation method according to claim 5, characterized in that: The modification conditions of the carrier are: impregnation time 10min to 12h, aging time 4 to 72h, drying temperature 40 to 150°C, drying time 30min to 36h, inert gas is nitrogen or argon, the temperature of calcination in inert gas atmosphere is 200 to 800°C, the calcination time is 1 to 24h, and the heating rate is 1°C / min to 6°C / min.

10. Use of the noble metal single component dehydrogenation catalyst according to claim 1 or 2 as a catalyst in a reversible hydrogenation hydrogen storage system, characterized in that: The reversible hydrogenation hydrogen storage system includes one or a mixture of two or more π-conjugated reversible hydrogenation hydrogen storage materials; the π-conjugated reversible hydrogenation hydrogen storage material, at 25°C and 1atm, releases 10 to 15 kcal of heat per 1 mol H2 stored, that is, -15 kcal / mol H2≤ΔH≤-10 kcal / mol H2; and the hydrogen storage density after complete hydrogenation is greater than 4% of the mass of the hydrogen storage material; the π-conjugated reversible hydrogenation hydrogen storage material is solid or liquid, and has a melting point less than 80°C.

Citation Information

Patent Citations

  • O-phenyl phenol preparation catalyst by cyclohexanone dimer dehydrogenation and preparation method thereof

    CN101455962A

  • Dehydrogenation catalyst, preparation method and application thereof

    CN112705198A

  • Catalyst for hydrogenation and dehydrogenation of organic liquid hydrogen storage material as well as preparation method and application of catalyst

    CN114917929A

  • Method for Storing and Releasing Hydrogen Using Catalysts Based upon Carbon-coated Support

    KR101950701B1

  • Hydrogen storage by reversible hydrogenation of pi-conjugated substrates

    US20040223907A1